Method for efficiently removing inclusions in stainless steel using VOD

By pre-evacuation, post-reduction pressurization, and dynamic vacuum control during the VOD smelting process, the problem of low inclusion removal efficiency in stainless steel has been solved, achieving efficient and rapid inclusion removal and meeting the requirements for high-purity stainless steel.

CN118086629BActive Publication Date: 2026-11-10SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410161395.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2026-11-10
Estimated Expiration
2044-02-05

AI Technical Summary

Technical Problem

Existing technologies are difficult to efficiently remove inclusions smaller than 30μm in stainless steel smelting, and do not fully consider the impact of steel temperature drop, production rhythm and cost, making them particularly unsuitable for efficient removal of inclusions in stainless steel.

Method used

By employing the pre-evacuation, post-reduction pressurization, dynamic control of vacuum degree, and high-vacuum degassing steps in the VOD smelting process, combined with the high-temperature characteristics of stainless steel and the features of the production process, and utilizing the principle of bubble adhesion to inclusions, efficient removal of inclusions of different types and particle sizes can be achieved.

Benefits of technology

It achieves efficient removal of inclusions smaller than 30μm, shortens smelting time, reduces the temperature drop of molten steel, and meets the requirements for high-purity stainless steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004698505650000061
    Figure BDA0004698505650000061
  • Figure BDA0004698505650000071
    Figure BDA0004698505650000071
Patent Text Reader

Abstract

The application discloses a method for efficiently removing inclusions in stainless steel by VOD, which comprises the steps of pre-evacuation, post-reduction pressurization, dynamic control of vacuum degree, high vacuum degassing and the like. In the pre-evacuation, the vacuum is extracted to 50-80 mbar and maintained for 2-5 min, and then extracted to <0.5 mbar; in the post-reduction pressurization, 1.5-2.5 MPa nitrogen is top-blown to make the nitrogen pressure reach 1-2 bar, and the nitrogen is bottom-blown for 5-15 min; in the dynamic control of vacuum degree, the bottom-blown nitrogen is first closed, the vacuum is extracted to 30-50 mbar and maintained for 5-20 min, then the bottom-blown nitrogen is opened, the vacuum degree is adjusted to 10-20 mbar and maintained for 5-20 min; in the high vacuum degassing, argon is bottom-blown in a ladle, and the vacuum degree and the holding time are controlled according to the saturated solubility of N and the target N content. The application considers the influence of the solubility of N in steel, the N content, the vacuum degree and the like on the bubble size, the influence of the bubble on the removal effect of inclusions of different types and particle sizes, and the influence of the process on the temperature drop of the molten steel, the production rhythm and the cost, so that the inclusions of different types and particle sizes below 30 mu in the stainless steel are efficiently removed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of iron and steel smelting technology, specifically relating to a method for efficiently removing inclusions in stainless steel using VOD. Background Technology

[0002] As the application of steel products extends to high-end fields, the requirements for steel purity are becoming increasingly stringent. The purity of stainless steel, especially the quantity and size of inclusions, directly affects surface quality and corrosion resistance. Studies have shown that inclusions as small as 10–30 μm can cause surface defects in cold-rolled stainless steel sheets.

[0003] In stainless steel smelting, the main function of vacuum degassing (VOD) is to utilize high vacuum for deep decarburization and degassing. Although high-flow-rate stirring during the reduction stage can achieve slag washing, the removal efficiency of inclusions of specific sizes under vacuum has not received much attention. Currently, inclusion removal methods mainly involve allowing the ladle to settle or bottom-blowing gas to promote flotation into the slag layer during the refining process. Based on the mechanism of bubble adhesion to inclusions, larger bubbles have a poorer removal effect. Traditional gas stirring, using Ar or N2, produces relatively large bubbles with poor inclusion removal efficiency, and is also affected by the ladle structure and the distribution of the molten steel flow field. However, under RH and VOD vacuum conditions, the bubbles precipitated inside the molten steel are typically finer, resulting in higher inclusion removal efficiency, even for inclusions smaller than 30μm. Therefore, compared to conventional argon blowing and stirring, using VOD for inclusion removal is more advantageous.

[0004] Currently, there are related patented technologies both domestically and internationally that utilize this principle to remove inclusions, such as Chinese invention patents with publication numbers CN104404205, CN105779699, CN106086315, CN111944953, and CN110592322. The main idea behind these existing technologies is to add nitrogen or hydrogen to the molten steel, and then, under vacuum conditions, allow nitrogen and hydrogen to precipitate from the molten steel using inclusions as nuclei, forming bubbles. These bubbles carry the inclusions to the surface and continuously capture fine inclusions during their ascent, significantly promoting the removal of microscopic non-metallic inclusions in the steel. However, the above patented technologies have the following shortcomings:

[0005] 1. The impact of the process on the temperature drop of molten steel, production rhythm and cost was not considered. In actual production, the nitrogen addition and vacuum nitrogen removal processes consume a lot of time, making it difficult to meet the requirements of fast-paced production, and the temperature drop of molten steel is relatively large.

[0006] 2. The removal effect on inclusions of different types and sizes was not considered. Due to the different nitrogen partial pressure and vacuum degree, the generated bubble particle size is different, and the removal effect on inclusions of different types and sizes varies.

[0007] 3. The above technologies are mainly applied to carbon steel and low-alloy steel. As the chromium content in the steel increases, the solubility of nitrogen increases. According to thermodynamic and kinetic studies, bubble size is related to factors such as the nitrogen content after nitrogen addition, nitrogen saturation solubility, and vacuum level. Since the nitrogen solubility in stainless steel reaches 900–3000 ppm, if the nitrogen addition is small, it is necessary to evacuate to the ultimate vacuum level, and nitrogen bubbles will be small or even non-existent. If the vacuum level is reduced, a higher nitrogen addition is required, and both adding nitrogen to saturation solubility and evacuating to the ultimate vacuum level take a long time. Therefore, compared to other steels, the nitrogen content and bubble size in stainless steel are not easy to control.

[0008] 4. The stainless steel process differs significantly from VOD vacuum smelting and RH or VD processes. Deep decarburization involves a large oxygen blowing volume, and slag has a significant impact on inclusion removal. Therefore, the above technologies are not suitable for the efficient removal of inclusions in stainless steel.

[0009] Regarding methods for nitrogen addition to molten steel, Chinese invention patent CN103555882 proposes a method for nitrogen addition to low-carbon stainless steel ladles, which involves inserting a VOD top lance below the molten steel for nitrogen addition. However, this method is limited to situations where the amount of molten steel is limited, the amount of slag is small, and the ladle has sufficient space; otherwise, it will cause splashing of molten steel and slag. Generally, the slag thickness after reduction is more than 100mm. Chinese invention patent CN101275174 proposes a method for controlling the nitrogen content in stainless steel smelting using a vacuum oxygen decarburization device. During the vacuum treatment process, decarburization, desulfurization, and nitrogen introduction are performed, and finally, during the atmospheric adjustment stage, the nitrogen composition is fine-tuned by bottom-blowing nitrogen. However, this method has a slow nitrogen addition rate, and the nitrogen content control is unstable due to external conditions, making it difficult to meet the requirements of high-efficiency smelting. Summary of the Invention

[0010] To address the technical problems existing in the prior art, the present invention provides a method for efficiently removing inclusions in stainless steel using VOD, comprising the following steps:

[0011] S1. Pre-vacuuming: Before tapping steel using KOBMS or AOD, control the w(N) content in the steel to be 0.05-0.09%, w(Si) ≥ 0.03%, and w(S) ≤ 0.01%. Before VOD enters the station, remove slag to 50-100mm and ensure the temperature of the molten steel is above 1660℃. Turn off the bottom blowing gas, add lime and fluorite at 0.5-0.7kg per ton of steel, cover with a vacuum cover and evacuate to 50-80mbar, maintain for 2-5 minutes, and then evacuate to a vacuum degree < 0.5mbar.

[0012] S2. Pressurization after reduction: After the decarburization and boiling periods, add reducing agent and slag deoxidation and slag adjustment under vacuum conditions. Maintain bottom blowing argon stirring for 5-15 minutes to ensure that the temperature of the molten steel after VOD reduction is above 1600℃. Control the slag basicity ≥2.0, w(Cr2O3) ≤0.2% and w(TO) ≤0.01% in the slag. Then stop the vacuum pump, keep the vacuum cover tightly closed, and lower the top gun nozzle to 0.5-1.0m above the surface of the molten steel. Blow in nitrogen gas with a pressure of 1.5-2.5Mpa so that the nitrogen pressure in the space above the molten steel reaches 1-2 bar. At the same time, nitrogen gas is blown into the bottom of the ladle. The bottom blowing flow rate is controlled at 10-16NL / min per ton of steel, and the duration is 5-15 minutes, so that the final N content in the molten steel reaches 0.3-0.5 times the saturation solubility.

[0013] S3. Dynamic control of vacuum degree: First, perform the first stage of evacuation, turn off the bottom blowing nitrogen in the ladle, evacuate to 30-50 mbar, and maintain for 5-20 minutes; then perform the second stage of evacuation, turn on the bottom blowing nitrogen in the ladle, control the bottom blowing flow rate to 1-5 NL / min per ton of steel, adjust the vacuum degree to 10-20 mbar, and maintain for 5-20 minutes.

[0014] S4. High-vacuum degassing: If the N content is higher than the target range for the steel grade, the bottom blowing of the ladle is switched to argon gas, and the bottom blowing flow rate is controlled at 7-16 NL / min per ton of steel. The vacuum degree and vacuum time are controlled according to the N saturation solubility of the molten steel and the target N content. If the N content is lower than the target range, this step is not performed.

[0015] Furthermore, in the above-mentioned method for efficiently removing inclusions in stainless steel using VOD, in the post-reduction pressurization step, if the temperature of the molten steel after VOD reduction is lower than 1600℃, the molten steel is transferred to LF for heating. After being heated to above 1600℃ by LF, the molten steel is transferred back to VOD to continue the subsequent pressurization operation.

[0016] Furthermore, in the above-mentioned method for efficiently removing inclusions in stainless steel using VOD, after the high vacuum degassing step, step S5 is also included: LF adjusts the temperature and composition of the molten steel to achieve the target before continuous casting.

[0017] The method of the present invention for efficiently removing inclusions in stainless steel using VOD has at least the following advantages and beneficial effects:

[0018] The effects of nitrogen solubility, nitrogen content, and vacuum degree in steel on bubble size, as well as the effect of bubbles on the removal efficiency of inclusions of different types and particle sizes, were considered. The efficient removal of inclusions of different types and particle sizes was achieved by dynamically adjusting the nitrogen partial pressure and vacuum degree.

[0019] Taking into full account the impact of the process on the temperature drop of molten steel, production rhythm and cost, by pressurizing and low vacuum evacuation, the smelting time is shortened while ensuring the size and number of bubbles, thereby achieving a smaller temperature drop and efficient removal of inclusions.

[0020] By controlling the temperature of the molten steel, nitrogen dissolution is promoted; nitrogen gas is introduced above the molten steel surface through the top lance under VOD sealing to maintain a high nitrogen partial pressure, and bottom blowing nitrogen gas rapidly increases nitrogen content. Moreover, the top lance does not contact the slag surface or the molten steel, so it will not cause splashing. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0022] This invention aims to solve the technical problem of low efficiency in removing inclusions smaller than 30μm from stainless steel using traditional argon blowing and stirring. It mainly achieves efficient removal of inclusions in stainless steel by pressurizing and vacuuming the stainless steel VOD smelting process and utilizing the principle of bubble adhesion to inclusions. It fully considers the high-temperature characteristics of stainless steel, the characteristics of the production process, and the bubble size. It achieves efficient smelting and inclusion removal through steps such as pre-evacuation, pressurization after reduction, dynamic control of vacuum degree, and high-vacuum degassing.

[0023] Specifically, the method of the present invention for efficiently removing inclusions in stainless steel using VOD includes the following steps:

[0024] S1. Pre-vacuuming: Before tapping steel using KOBMS or AOD, control the w(N) content in the steel to be 0.05-0.09%, w(Si) ≥ 0.03%, and w(S) ≤ 0.01%. Before VOD enters the station, remove slag to 50-100mm and ensure the temperature of the molten steel is above 1660℃. Turn off the bottom blowing gas, add lime and fluorite at 0.5-0.7kg per ton of steel, cover with a vacuum cover and evacuate to 50-80mbar, maintain for 2-5 minutes, and then evacuate to the ultimate vacuum degree, which is <0.5mbar.

[0025] S2. Post-reduction pressurization: After the decarburization and boiling periods, add reducing agent and slag deoxidation and slag adjustment under vacuum conditions. Maintain bottom blowing argon stirring for 5-15 minutes to ensure that the temperature of the molten steel after VOD reduction is above 1600℃. Control the slag basicity R(CaO / SiO2) ≥ 2.0, w(Cr2O3) ≤ 0.2%, and w(TO) ≤ 0.01% in the slag. Then stop the vacuum pump, keep the vacuum cover tightly closed, and lower the top gun nozzle to 0.5-1.0m above the surface of the molten steel. Blow in nitrogen gas at a pressure of 1.5-2.5 MPa so that the nitrogen pressure in the space above the molten steel reaches 1-2 bar. At the same time, blow nitrogen gas into the bottom of the ladle. The bottom blowing flow rate is controlled at 10-16 NL / min per ton of steel, and the duration is 5-15 minutes, so that the final N content in the molten steel reaches 0.3-0.5 times the saturation solubility.

[0026] S3. Dynamic control of vacuum degree: First, perform the first stage of evacuation, turn off the bottom blowing nitrogen in the ladle, evacuate to 30-50 mbar, and maintain for 5-20 minutes; then perform the second stage of evacuation, turn on the bottom blowing nitrogen in the ladle, control the bottom blowing flow rate to 1-5 NL / min per ton of steel, adjust the vacuum degree to 10-20 mbar, and maintain for 5-20 minutes.

[0027] S4. High-vacuum degassing: If the N content is higher than the target range for the steel grade, the bottom blowing of the ladle is switched to argon gas, and the bottom blowing flow rate is controlled at 7-16 NL / min per ton of steel. The vacuum degree and vacuum time are controlled according to the N saturation solubility of the molten steel and the target N content. If the N content is lower than the target range, this step is not performed.

[0028] Furthermore, in the method of efficiently removing inclusions in stainless steel using VOD according to the present invention, after the high vacuum degassing step, step S5 is also included: LF adjusts the temperature and composition of the molten steel to achieve the target and then performs continuous casting.

[0029] Furthermore, in the method of efficiently removing inclusions in stainless steel using VOD according to the present invention, in the post-reduction pressurization step, if the temperature of the molten steel after VOD reduction is lower than 1600°C, the molten steel is transferred to LF for heating. After being heated to above 1600°C by LF, the molten steel is transferred back to VOD to continue the subsequent pressurization operation.

[0030] The following, in conjunction with comparative examples and embodiments of the present invention, further illustrates the method of the present invention for efficiently removing inclusions in stainless steel using VOD.

[0031] Examples 1-4 illustrate specific practices and applications of the technical solutions of this invention in industrial production. In Examples 1-2, the steel used is 304L stainless steel; in Example 3, it is 0Cr13 stainless steel; and in Example 4, it is 409 stainless steel. Furthermore, Comparative Example 1 uses 304L stainless steel, and Comparative Examples 2 and 3 use 0Cr13 stainless steel. The process flow for Examples 1-4 and Comparative Examples 1-3 is the same: 80t KOBMS / AOD-VOD-LF-CCM.

[0032] Examples 1-4

[0033] S1. Pre-vacuuming: Before tapping the steel using KOBMS or AOD, control the w(N) content in the steel to be 0.05-0.09%, w(Si) ≥ 0.03%, and w(S) ≤ 0.01%. Before VOD enters the station, remove slag to 50-100mm and ensure the temperature of the molten steel is above 1660℃. Turn off the bottom blowing gas, add 50kg each of lime and fluorite, cover with a vacuum cover and evacuate to 50-80mbar, maintain for 2-5min, and then evacuate to the ultimate vacuum degree, which is <0.5mbar.

[0034] S2. Pressurization after reduction: After the decarburization and boiling periods, add reducing agent and slag deoxidation and slag adjustment under vacuum conditions. Maintain bottom blowing argon stirring for 5-15 minutes to ensure that the temperature of the molten steel after VOD reduction is above 1600℃. If the temperature is below 1600℃, switch to LF heating. Control the slag basicity R≥2.0, w(Cr2O3)≤0.2% and w(TO)≤0.01% in the slag. Then stop the vacuum pump, keep the vacuum cover tightly closed, and lower the top gun nozzle to 0.5-1.0m above the surface of the molten steel. Blow in nitrogen gas with a pressure of 1.5-2.5Mpa so that the nitrogen pressure in the space above the molten steel reaches 1-2 bar. At the same time, blow nitrogen gas into the ladle through two bottom blowing holes. The bottom blowing flow rate of each bottom blowing hole is controlled at 10-16Nl / min per ton of steel for 5-15 minutes, so that the final N content in the molten steel reaches 0.3-0.5 times the saturation solubility.

[0035] S3. Dynamic control of vacuum degree: First, perform a first-stage evacuation, turn off the bottom blowing nitrogen in the ladle, evacuate to 30-50 mbar, and maintain for 5-20 minutes; then perform a second-stage evacuation, blow nitrogen into the ladle through two bottom blowing holes, control the bottom blowing flow rate of each bottom blowing hole to 1-5 Nl / min per ton of steel, adjust the vacuum degree to 10-20 mbar, and maintain for 5-20 minutes.

[0036] S4. High-vacuum degassing: In Examples 3 and 4, since the N content is higher than the target range for the steel grade, argon gas is blown into the ladle through two bottom blow holes. The bottom blow flow rate of each bottom blow hole is controlled at 7-16 NL / min per ton of steel. The vacuum degree and vacuum holding time are controlled according to the N saturation solubility of the molten steel and the target N content. In Examples 1 and 2, since the N content is lower than the target range, this step is not performed.

[0037] S5. Subsequent processing: LF adjusts the temperature and composition of the molten steel to achieve the target before continuous casting.

[0038] Comparative Example 1

[0039] Step 1, Pre-vacuuming: Before the VOD enters the station, remove the slag to below 50mm and evacuate to the ultimate vacuum level, which is <0.5mbar;

[0040] Step II, Nitrogen Addition: After the decarburization and boiling periods are completed, a reducing agent and slag are added under vacuum conditions for deoxidation and slag conditioning. The bottom-blown argon gas is maintained for stirring for 5 to 15 minutes. Then the vacuum pump is stopped, and nitrogen is added by bottom-blowing nitrogen gas through two bottom-blowing holes in the ladle. The bottom-blowing flow rate of each bottom-blowing hole is 10 to 16 NL / min per ton of steel.

[0041] Step III, Nitrogen Evolution: Increase nitrogen for 10-15 minutes until the final nitrogen content is 300-400 ppm, then turn off the bottom-blowing nitrogen in the ladle, evacuate to 0.1 mbar, and maintain for 15 minutes;

[0042] Step IV, Denitrification: Argon gas is blown into the ladle through two bottom blow holes. The bottom blow flow rate of each bottom blow hole is 7-16 NL / min per ton of steel. The vacuum degree and vacuum holding time are controlled according to the saturated nitrogen solubility of the liquid steel and the target nitrogen content.

[0043] Step V, Post-processing: LF adjusts the temperature and composition of the molten steel to achieve the target, and then performs continuous casting.

[0044] Comparative Example 2

[0045] Step 1, Pre-vacuuming: Before VOD enters the station, remove slag to below 50mm and evacuate to the ultimate vacuum level, which is <0.5mbar;

[0046] Step II, Nitrogen Addition: After the decarburization and boiling periods are completed, a reducing agent and slag are added under vacuum conditions for deoxidation and slag conditioning. The bottom-blown argon gas is maintained for stirring for 5 to 15 minutes. Then the vacuum pump is stopped, and nitrogen is added by bottom-blowing nitrogen gas through two bottom-blowing holes in the ladle. The bottom-blowing flow rate of each bottom-blowing hole is 10 to 16 NL / min per ton of steel.

[0047] Step III, Nitrogen Evolution: After increasing nitrogen for 30 minutes until the final nitrogen content is 1000 ppm, the gas is heated by LF and then transferred to VOD. The bottom blowing nitrogen in the ladle is turned off, and the gas is evacuated to 50 mbar and held for 15 minutes.

[0048] Step IV, Denitrification: Argon gas is blown into the ladle through two bottom blow holes. The bottom blow flow rate of each bottom blow hole is 7-16 NL / min per ton of steel. The vacuum degree and vacuum holding time are controlled according to the saturated nitrogen solubility of the liquid steel and the target nitrogen content.

[0049] Step V, Post-processing: LF adjusts the temperature and composition of the molten steel to achieve the target, and then performs continuous casting.

[0050] Comparative Example 3

[0051] After VOD reduction is completed, no nitrogen addition, nitrogen precipitation, or nitrogen removal treatments are performed. The process is directly transferred to LF to adjust the temperature and composition of the molten steel. Once the target is achieved, continuous casting is carried out.

[0052] The specific process parameters of Examples 1-4 and Comparative Examples 1-3 are shown in Table 1 below:

[0053] Table 1. Specific process parameters for the examples and comparative examples.

[0054]

[0055] The total VOD smelting time (including decarburization, boiling period, and reduction period) and the inclusion removal rate for different size ranges were recorded for Examples 1-4 and Comparative Examples 1-3. The inclusion removal rate was calculated as (total inclusions after VOD reduction - total inclusions leaving the VOD station) / total inclusions after VOD reduction * 100%. The inclusion removal effect in the stainless steel of Examples 1-4 and Comparative Examples 1-3 is shown in Table 2 below:

[0056] Table 2 Comparison of inclusion removal effects in the examples and comparative examples

[0057]

[0058] As shown in the table above, Examples 1-4 mainly achieve efficient removal of inclusions through pre-evacuation, nitrogen addition after reduction, two-stage low-vacuum dynamic nitrogen evolution, and high-vacuum denitrification. Comparative Example 1 removes inclusions by adding nitrogen at 300-400 ppm after reduction and nitrogen evolution under high vacuum; Comparative Example 2 removes inclusions by adding nitrogen to near-saturation solubility after reduction and nitrogen evolution under low vacuum; Comparative Example 3 leaves the station directly without any treatment after reduction, showing no inclusion removal effect. The comparison shows that the inclusion removal rate of Examples 1-4 of the present invention is significantly higher than that of Comparative Examples 1-3, and the VOD treatment time for the same steel grade is shorter.

[0059] In summary, the method for efficiently removing inclusions from stainless steel using VOD of the present invention, through steps such as pre-evacuation, post-reduction pressurization, dynamic vacuum control, and high-vacuum degassing in the stainless steel VOD smelting process, combined with the high-temperature characteristics of stainless steel, the production process, and the characteristics of VOD equipment, achieves efficient removal of inclusions from stainless steel. Compared with the prior art, it has the following advantages and beneficial effects:

[0060] 1. This invention considers the effects of nitrogen solubility, nitrogen content, and vacuum level in steel on bubble size, as well as the influence of bubbles on the removal efficiency of inclusions of different types and sizes. By controlling smelting process parameters, it achieves efficient removal of different types of inclusions smaller than 30 μm. Specifically, the inclusions in steel produced by KOBMS or AOD are mainly chromium-manganese spinel inclusions smaller than 10 μm. Therefore, the pre-evacuation stage generates small bubbles smaller than 3 mm to promote the flotation of inclusions in KOBMS or AOD and minimizes their size. The residual [O] and [S] in the steel create initial conditions for VOD smelting. After VOD reduction, the inclusions are mainly Al2O3, calcium aluminum silicate, magnesium aluminum spinel, etc., smaller than 30 μm. By controlling the vacuum degree and balancing the nitrogen partial pressure, bubbles smaller than 10 mm are generated, promoting the adsorption and removal of inclusions. After evacuation for a period of time, as the nitrogen content decreases, the bubble size decreases. Due to the static pressure, the molten steel at the bottom of the ladle may not be able to generate bubbles. At this time, it is necessary to adjust the vacuum degree and bottom blowing flow rate to promote the circulation and floating of inclusions. Therefore, this invention dynamically adjusts the nitrogen partial pressure and vacuum degree according to the smelting situation, thereby achieving the removal of inclusions of different types and particle sizes.

[0061] 2. This invention fully considers the impact of the process on the temperature drop of molten steel, production rhythm and cost. By pressurizing and evacuating with low vacuum, the smelting time is shortened while ensuring the size and number of bubbles, thereby achieving a smaller temperature drop and efficient removal of inclusions.

[0062] 3. If the inclusions that float to the surface cannot be absorbed by the slag in time, they will contaminate the molten steel again during subsequent smelting processes. This invention promotes the absorption and removal of inclusions by controlling the oxygen and sulfur content in the slag and steel.

[0063] 4. By controlling the temperature of the molten steel, nitrogen dissolution is promoted; by using a top lance in VOD sealed state to introduce nitrogen above the molten steel surface to maintain a high nitrogen partial pressure, and bottom blowing nitrogen rapidly increases nitrogen, thereby obtaining a high nitrogen increase rate of 50-120 ppm / min. Moreover, the top lance does not contact the slag surface and molten steel, so it will not cause splashing. Since the top lance is not affected by the static pressure of the molten steel and has a larger flow rate than bottom blowing, a large amount of nitrogen can be introduced in a short time to maintain high pressure.

[0064] 5. The prior art, represented by the patent documents cited in the background section of this application, mainly focuses on carbon steel and low alloy steel. This invention combines the characteristics and process features of stainless steel, taking into account the significant differences between VOD vacuum smelting and RH or VD, the large oxygen blowing volume in the deep decarburization process, and the significant impact of slag on inclusion removal. It can achieve a high removal rate for different types of inclusions below 30μm in a short time, meeting the requirements for high-purity stainless steel.

[0065] It should be noted that, in this document, the terms “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for efficiently removing inclusions in stainless steel using VOD, characterized by, Includes the following steps: S1. Pre-vacuuming: Before tapping steel using KOBMS or AOD, control the w(N) content in the steel to be 0.05-0.09%, w(Si) ≥ 0.03%, and w(S) ≤ 0.01%. Before VOD enters the station, remove slag to 50-100mm and ensure the temperature of the molten steel is above 1660℃. Turn off the bottom blowing gas, add lime and fluorite at 0.5-0.7kg per ton of steel, cover with a vacuum cover and evacuate to 50-80mbar, maintain for 2-5 minutes, and then evacuate to a vacuum degree < 0.5mbar. S2. Pressurization after reduction: After the decarburization and boiling periods, add reducing agent and slag deoxidation and slag adjustment under vacuum conditions. Maintain bottom blowing argon stirring for 5-15 minutes to ensure that the temperature of the molten steel after VOD reduction is above 1600℃. Control the slag basicity ≥2.0, w(Cr2O3) ≤0.2% and w(TO) ≤0.01% in the slag. Then stop the vacuum pump, keep the vacuum cover tightly closed, and lower the top gun nozzle to 0.5-1.0m above the surface of the molten steel. Blow in nitrogen gas with a pressure of 1.5-2.5Mpa so that the nitrogen pressure in the space above the molten steel reaches 1-2 bar. At the same time, nitrogen gas is blown into the bottom of the ladle. The bottom blowing flow rate is controlled at 10-16NL / min per ton of steel, and the duration is 5-15 minutes, so that the final N content in the molten steel reaches 0.3-0.5 times the saturation solubility. S3. Dynamic control of vacuum degree: First, perform the first stage of evacuation, turn off the bottom blowing nitrogen in the ladle, evacuate to 30-50 mbar, and maintain for 5-20 minutes; then perform the second stage of evacuation, turn on the bottom blowing nitrogen in the ladle, control the bottom blowing flow rate to 1-5 NL / min per ton of steel, adjust the vacuum degree to 10-20 mbar, and maintain for 5-20 minutes. S4. High-vacuum degassing: If the N content is higher than the target range for the steel grade, the bottom blowing of the ladle is switched to argon gas, and the bottom blowing flow rate is controlled at 7-16 NL / min per ton of steel. The vacuum degree and vacuum time are controlled according to the N saturation solubility of the molten steel and the target N content. If the N content is lower than the target range, this step is not performed.

2. The method for efficiently removing inclusions in stainless steel using VOD according to claim 1, characterized by, In the post-reduction pressurization step, if the temperature of the molten steel after VOD reduction is below 1600℃, the molten steel is transferred to LF for heating. After being heated to above 1600℃ by LF, the molten steel is transferred back to VOD to continue the subsequent pressurization operation.

3. The method for efficiently removing inclusions in stainless steel using VOD according to claim 1 or 2, characterized in that, After the high vacuum degassing step, step S5 is also included: LF adjusts the temperature and composition of the molten steel, and after reaching the target, continuous casting is carried out.

Citation Information

Patent Citations

  • Method for deoxidizing and alloying molten steel in converter steel ladle

    CN103555885A

  • Production method of stainless steel and high-thermal-conductivity corrosion-resistant special stainless steel