An atomically thin Cu2Te two-dimensional material, a synthesis method and application thereof

By employing nested deposition tubes and a temperature-controlled CVD method, the preparation challenges of two-dimensional Cu2Te materials have been solved, enabling the fabrication of atomically thin, large-size Cu2Te and the formation of heterojunctions. This enhances photoelectric performance and makes the material suitable for the manufacture of optoelectronic devices.

CN118086865BActive Publication Date: 2026-11-10HUNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410227609.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2026-11-10
Estimated Expiration
2044-02-29

AI Technical Summary

Technical Problem

Existing fabrication processes for Cu2Te two-dimensional materials are scarce, with stringent conditions, making it difficult to control the material thickness and planar dimensions, thus hindering the development of photoelectric properties and the formation of heterojunctions.

Method used

CVD deposition was performed using nested deposition tubes, combined with temperature control and the use of copper sources. By evaporating copper and tellurium sources inside the inner tube and depositing them on the substrate, atomically thin, large-size Cu2Te two-dimensional materials were prepared.

Benefits of technology

Cu2Te nanosheets with controllable thickness and good crystallinity were successfully prepared at low temperature. They can form heterojunctions and exhibit excellent optoelectronic properties, making them suitable for the manufacture of optoelectronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118086865B_ABST
    Figure CN118086865B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of two-dimensional semiconductor material preparation, specifically relating to a method for preparing atomically thin Cu2Te two-dimensional materials. The method employs a nested deposition tube for CVD deposition, wherein the deposition tube consists of an outer tube and an inner tube; the inner tube is open at the gas inlet end and sealed at the other end. During CVD deposition, a copper source and substrate are pre-positioned on the open side of the inner tube, and a tellurium source is positioned on the sealed side. Temperature control is implemented within the inner tube, maintaining the temperature T1 at the copper source and substrate on the open side at 460–510°C, and the temperature T2 at the tellurium source on the sealed side at 530–570°C. This allows the copper and tellurium sources to volatilize within the inner tube and be CVD deposited on the substrate, thus obtaining the atomically thin Cu2Te two-dimensional material. This invention also includes the materials prepared by the described method and their applications in optoelectronic devices. The process described in this invention can successfully prepare atomically thin Cu2Te two-dimensional materials and related heterojunctions, and the prepared materials exhibit excellent optoelectronic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nanomaterials, specifically relating to the preparation of atomically thin two-dimensional semiconductor materials by van der Waals epitaxy and their application in electrical and optoelectronic devices. Technical Background

[0002] The discovery of graphene in 2004 attracted widespread attention from the academic community. 1 The family of two-dimensional materials is growing rapidly. For example, two-dimensional transition metal dichalcogenides (TMDs), which are a research hotspot, possess unconventional physical and chemical properties, including atomic-level thickness, diverse crystal structures, and layer-dependent band gaps. These studies have yielded significant progress in fields such as electronics, optoelectronics, magnetism, and energy. 2-10 Therefore, the library of relevant two-dimensional semiconductor materials continues to expand, especially n-type semiconductors, whose properties are caused by strong electron doping from interface charge impurities and intrinsic structural defects. 11,12 Among them, MoS2 is a representative n-type semiconductor with high electron mobility and environmental stability. 13 Bi2O2Se 14 In contrast, intrinsic p-type two-dimensional semiconductors with holes as the primary charge carriers remain scarce. WSe2, as a typical predominantly p-type semiconductor, exhibits excellent electronic properties only at certain thicknesses. 15 Black phosphorus is considered a promising p-type semiconductor due to its excellent properties, but it suffers from poor environmental stability and requires stringent synthesis conditions. 16 Therefore, exploring intrinsic p-type two-dimensional materials with high stability and excellent properties is of great significance.

[0003] Cu₂Te, as one of the most abundant and environmentally friendly copper chalcogenides on Earth, has been widely used in thermoelectric and photovoltaic fields due to its ultra-low thermal conductivity and high thermoelectric properties. 17,18 Bulk Cu₂Te is a polycrystalline material that undergoes various phase transitions under different conditions. Furthermore, the synthesis of Cu₂Te using traditional methods leads to severe copper deficiency in the product, resulting in complex non-stoichiometric Cu compositions. 2-x Te 19,20 The relatively loose bonding of copper chalcogenides results in a low migration barrier for Cu ions, which facilitates low defect formation energy and abundant Cu vacancies. 21,22 To date, only a few research groups have achieved the synthesis of two-dimensional Cu2Te crystals. For example, monolayer Cu2Te two-dimensional materials were prepared by co-depositing copper and tellurium atoms on a bilayer graphene / SiC(0001) substrate using ultra-high vacuum molecular beam epitaxy (MBE). 23 Scalable 2D Cu2Te arrays are vertically grown on copper foil via chemical etching and chemical vapor deposition (CVD).24 Ultrathin Cu₂Te two-dimensional materials were synthesized on mica at a high temperature of approximately 800 °C using atmospheric pressure chemical vapor deposition (APCVD). 25,26 The methods described above for synthesizing two-dimensional Cu₂Te require ultra-high vacuum or high temperature and special substrates, making it difficult to explore two-dimensional Cu₂Te crystals and construct functional devices on SiO₂ / Si substrates. This is crucial for the fundamental research and potential technological applications of two-dimensional Cu₂Te materials.

[0004] References

[0005] 1.KSNovoselov,AKGeim,SVMorozov,D.Jiang,Y.Zhang,SVDubonos,IVGrigorieva,AAFirsov,Science 2004,306(5659),666-669.

[0006] 2. J. Zhou, J. Lin, X. Huang, Y. Zhou, Y. Chen, J. Xia, H. Wang, Y. Xie, H. Yu, J. Lei, D. Wu, F. Liu, Q. Fu, Q. Zeng, CH. Hsu, C. Yang, L. Lu, T. Yu, Z. Shen, H. Lin, BI. Yakobson, Q. Liu, K. Suenaga, G. Liu, Z. Liu, Nature 2018, 556(7701), 355-359.

[0007] 3.T.Zhang,J.Wang,P.Wu,A.-Y.Lu,J.Kong,Nat.Rev.Mater.2023,8(12),799-821.

[0008] 4.Y.Liu,X.Duan,HJShin,S.Park,Y.Huang,X.Duan,Nature 2021,591(7848),43-53.

[0009] 5.PVPham,SC Bodepudi,K.Shehzad,Y.Liu,Y.Xu,B.Yu,X.Duan,Chem.Rev.2022,122(6),6514-6613.

[0010] 6.QHWang,K.Kalantar-Zadeh,A.Kis,JNColeman,MSStrano,Nat.Nanotechnol.2012,7(11),699-712.

[0011] 7.B.Li,Z.Wan,C.Wang,P.Chen,B.Huang,X.Cheng,Q.Qian,J.Li,Z.Zhang,G.Sun,B.Zhao,H.Ma,R.Wu ,Z.Wei,Y.Liu,L.Liao,Y.Ye,Y.Huang,X.Xu,X.Duan,W.Ji,X.Duan,Nat.Mater.2021,20(6),818-825.

[0012] 8.C.Gong,L.Li,Z.Li,H.Ji,A.Stern,Y.Xia,T.Cao,W.Bao,C.Wang,Y.Wang,ZQQiu,RJCava,SGLouie,J.Xia,X.Zhang,Nature 2017,546(7657),26.26.

[0013] 9.K.Chang,WLChen,ACSNano 2011,5(6),4720-4728.

[0014] 10.Q.Yun,L.Li,Z.Hu,Q.Lu,B.Chen,H.Zhang,Adv.Mater.2019,32(1),1903826.

[0015] 11.Q.He,Y.Liu,C.Tan,W.Zhai,GHNam,H.Zhang,ACS Nano 2019,13(11),12294-12300.

[0016] 12.MIBeddiar,X.Zhang,B.Liu,Z.Zhang,Y.Zhang,Small Struct.2022,3(12),2200125.

[0017] 13.B.Radisavljevic,A.Radenovic,J.Brivio,V.Giacometti,A.Kis,Nat.Nanotechnol.2011,6(3),147-150.

[0018] 14.J.Wu,H.Yuan,M.Meng,C.Chen,Y.Sun,Z.Chen,W.Dang,C.Tan,Y.Liu,J.Yin,Y.Zhou,S.Huang. ,HQXu,Y.Cui,HYHwang,Z.Liu,Y.Chen,B.Yan,H.Peng,Nat.Nanotechnol.2017,12(6),530-534.

[0019] 15.H.Zhou,C.Wang,JCShaw,R.Cheng,Y.Chen,X.Huang,Y.Liu,NOWeiss,Z.Lin,Y.Huang,X.Duan,Nano Lett.2014,15(1),709-713.

[0020] 16.H.Liu,ATNeal,Z.Zhu,Z.Luo,X.Xu,D.Tomanek,PDYe,ACSNano2014,8(4),4033-4041.

[0021] 17.S.Ballikaya,H.Chi,JRSalvador,C.Uher,J.Mater.Chem.A 2013,1(40),12478-12484.

[0022] 18.C.Coughlan,M. O.Dobrozhan,A.Singh,A.Cabot,KMRyan,Chem.Rev.2017,117(9),5865-6109.

[0023] 19.S.Mukherjee,R.Chetty,PVPMadduri,AKNayak,K.Wojciechowski,T.Ghosh,K.Chattopadhyay,S.Suwas,RCMallik,Dalton Trans.2019,48(3),1040-1050.

[0024] 20.J.Pandey,S.Mukherjee,D.Rawat,S.Athar,KSRana,RCMallik,A.Soni,ACSAppl.Energy Mater.2020,3(3),2175-2181.

[0025] 21.Y.He,T.Zhang,X.Shi,SHWei,L.Chen,NPG Asia Mater.2015,7(8),e210-e210.

[0026] 22.D.Zhang,ZDLuo,Y.Yao,P.Schoenherr,C.Sha,Y.Pan,P.Sharma,M.Alexe,J.Seidel,Nano Lett.2021,21(2),995-1002.

[0027] 23.K.Qian,L.Gao,H.Li,S.Zhang,JHYan,C.Liu,JOWang,T.Qian,H.Ding,YYZhang,X.Lin,SXDu,HJGao,Chin.Phys.B 2020,29(1),018104.

[0028] 24. H.Wang, G.Zhan, C.Tang, D.Yang, W.Liu, D.Wang, Y.Wu, H.Wang, K.Liu, J.Li, M.Huang, K.Chen, ACSNano 2023, 17(5), 4790-4799.

[0029] 25. L.Yin, R.Cheng, S.Pan, W.Xiong, S.Chang, B.Zhai, Y.Wen, Y.Cai, Y.Guo, MGSendeku, J.Jiang, W.Liao, Z.Wang, J.He, Adv.Mater. 2023, 35(51), 2306850.

[0030] 26.L.Yin,R.Cheng,Y.Wen,B.Zhai,J.Jiang,H.Wang,C.Liu,J.He,Adv.Mater.2022,34(9),2108313. Summary of the Invention

[0031] In view of the lack of existing Cu2Te two-dimensional material preparation processes, the few existing processes have problems such as harsh conditions, difficulty in controlling material thickness and planar size, and difficulty in realizing photoelectric properties, the primary objective of this invention is to provide a method for preparing atomically thin Cu2Te two-dimensional materials at low temperatures, aiming to successfully prepare Cu2Te two-dimensional materials with atomically thinness, large size, and excellent photoelectric properties under mild preparation conditions.

[0032] The second objective of this invention is to provide a Cu2Te two-dimensional material prepared by the aforementioned method and its application in the preparation of optoelectronic devices.

[0033] A third objective of the present invention is to provide an optoelectronic device comprising the Cu2Te two-dimensional material and made of the Cu2Te two-dimensional material.

[0034] Due to its inherent properties, Cu2Te two-dimensional materials are difficult to synthesize via CVD, making it challenging to synthesize atomically thin, large-sized Cu2Te two-dimensional materials, and even more difficult to form two-dimensional heterostructures containing Cu2Te. To address this problem, this invention, after in-depth research, provides the following improved solutions:

[0035] A method for preparing atomically thin Cu2Te two-dimensional materials involves CVD deposition using nested deposition tubes. The deposition tubes include an outer tube with an inlet and an outlet, and an inner tube disposed within the outer tube chamber. The inner tube is open at the inlet end and sealed at the other end.

[0036] During the CVD deposition process, the copper source and substrate are pre-positioned on the open side of the inner tube, and the tellurium source is positioned on the sealed side of the inner tube. Carrier gas is introduced into the deposition tube through the gas inlet for purging. Subsequently, the temperature of the inner tube is controlled, so that the temperature T1 at the copper source and substrate on the open side of the inner tube is controlled at 460-510℃, and the temperature T2 at the tellurium source on the sealed side is controlled at 530-570℃. This allows the copper source and tellurium source to volatilize in the inner tube and be CVD deposited on the substrate, thus obtaining the atomically thin Cu2Te two-dimensional material.

[0037] The copper source is copper oxide and / or cuprous iodide.

[0038] To address the challenges of forming atomically thin Cu2Te two-dimensional materials, particularly the difficulty in successfully preparing them at low temperatures and forming heterojunctions, this invention innovatively employs nested deposition tubes for CVD deposition of Cu2Te two-dimensional materials. By combining the temperature control of the CVD deposition process with the joint control of the copper source, a synergistic effect is achieved, which solves the problem of the difficulty in preparing Cu2Te two-dimensional materials. This allows for the formation of Cu2Te two-dimensional materials with superior performance, especially atomically thin and large-sized materials, at lower temperatures. Furthermore, the materials prepared by this method exhibit excellent optoelectronic properties.

[0039] The inner tube of the present invention is a blind tube with one end sealed, and its open end is located on the air inlet side of the outer tube.

[0040] In this invention, both the inner and outer tubes of the deposition tube are quartz tubes;

[0041] In this invention, both the inner tube and the outer tube are cylindrical straight tubes.

[0042] In this invention, the length directions of the inner tube and the outer tube are parallel or nearly parallel;

[0043] In this invention, the diameter ratio of the inner tube to the outer tube is 0.1 to 0.5:1.

[0044] The technical solution of this invention does not have special requirements for the substrate; it can be any substrate available in the industry, such as a conventional silicon substrate or a two-dimensional material substrate. For example, the substrate is a silicon wafer or a substrate with a two-dimensional Mx2 layer grown on its surface. The silicon wafer is a 285nm SiO2 / Si substrate. In the two-dimensional Mx2 layer, M is a transition metal element containing at least one of Mo or W, and X is a chalcogenide element containing at least one of S or Se.

[0045] In this invention, the substrate is disposed in the inner tube and is located above the copper source.

[0046] In this invention, the tellurium source is tellurium powder;

[0047] Preferably, the copper source is cuprous iodide. This invention demonstrates that using cuprous iodide synergizes better with the nested deposition and temperature control methods described in this invention, facilitating the synthesis of Cu2Te two-dimensional materials, controlling their thickness and size, and unexpectedly improving their photoelectric properties. Furthermore, it facilitates unexpected adaptation to two-dimensional material substrates, enabling the successful fabrication of heterojunctions containing Cu2Te two-dimensional materials for the first time in the industry.

[0048] Preferably, the mass ratio of copper source to tellurium source is 1 to 5:1, and more preferably 2 to 3:1.

[0049] In this invention, the carrier gas is a hydrogen-containing atmosphere, preferably a mixture of hydrogen and a protective gas;

[0050] Preferably, the protective gas is at least one of nitrogen and an inert gas;

[0051] Preferably, the flow rate of the protective gas in the carrier gas is 10-200 sccm, more preferably 40-100 sccm, and even more preferably 50-80 sccm, and the flow rate of the hydrogen gas is 0.1-10 sccm, more preferably 1-5 sccm, even more preferably 1-2 sccm, and even more preferably 1.4-1.6 sccm.

[0052] In this invention, at the initial stage of the reaction, the copper source, substrate, and tellurium source are first placed in corresponding parts of the inner tube. Then, carrier gas is introduced through the inlet of the outer tube and output through the outlet, forming a carrier gas flow. After gas washing, the carrier gas is maintained to control the temperature of the inner tube, so that the temperature of the copper source and substrate is controlled at T1 (referring to the copper source volatilization temperature and deposition temperature), and the temperature of the tellurium source is controlled at T2 (referring to the tellurium source volatilization temperature), which promotes the volatilization of raw materials in the inner tube and gas phase deposition to obtain the material.

[0053] In this invention, the temperature T1 is preferably 460-490℃, more preferably 475-485℃; the temperature T2 is preferably 540-560℃, more preferably 535-545℃.

[0054] In this invention, the CVD deposition time is 10–25 min, and can be further 14–16 min.

[0055] The present invention also provides an atomically thin Cu2Te two-dimensional material prepared by the preparation method described above; comprising a substrate and a hexagonal phase Cu2Te two-dimensional material composited thereon;

[0056] Preferably, the thickness of the Cu2Te two-dimensional material is 2-50 nm, and the size is 3-80 μm;

[0057] Preferably, the substrate is a substrate with two-dimensional MX2 grown on its surface, and the atomically thin Cu2Te two-dimensional material is an MX2-Cu2Te heterojunction.

[0058] The present invention also provides an application of the atomically thin Cu2Te two-dimensional material for the fabrication of optoelectronic devices.

[0059] In this invention, any desired optoelectronic device can be fabricated from the atomically thin Cu2Te two-dimensional material described herein using known processes.

[0060] In this invention, the optoelectronic device is a field-effect transistor or a semiconductor diode.

[0061] The optoelectronic device described in this invention, apart from containing the Cu2Te two-dimensional material described in this invention, can have other conventional components and parts that can be prepared using conventional methods.

[0062] For example, the field-effect transistor includes a channel Cu2Te, a dielectric layer SiO2, source and drain electrodes Au, and a gate Si;

[0063] Preferably, the fabrication of the field-effect transistor comprises the following steps:

[0064] A layer of polymethyl methacrylate (PMMA) was spin-coated onto a SiO2 / Si surface on which Cu2Te two-dimensional material was deposited. The sample was then marked by electron beam exposure. Subsequently, metal was deposited on the surface. Finally, the gold film and PMMA were removed to obtain a field-effect transistor.

[0065] Preferably, metal is deposited on the surface of Cu2Te two-dimensional material using a vacuum coating machine;

[0066] Preferably, the metal is Au, and its thickness is 40-60 nm.

[0067] Preferably, the obtained MX2-Cu2Te heterojunction is used to fabricate a semiconductor diode, and the steps are as follows:

[0068] A layer of polymethyl methacrylate (PMMA) was spin-coated onto a SiO2 / Si surface with an MX2-Cu2Te heterojunction deposited on it. The sample was then marked by electron beam exposure. Subsequently, metal was deposited on its surface. Finally, the gold film and PMMA were removed with acetone to obtain a field-effect transistor.

[0069] Preferably, metal is deposited on the surface of the heterojunction using a vacuum coating machine;

[0070] Preferably, the metal is Au, and its thickness is 40-60 nm;

[0071] Preferably, it is used in the fabrication of optoelectronic devices;

[0072] The aforementioned optoelectronic device is a photodetector, comprising a channel Cu2Te, a dielectric layer SiO2, source / drain Au, and a gate Si;

[0073] The steps for fabricating a photodetector using the atomically thin Cu2Te two-dimensional material are as follows:

[0074] A layer of polymethyl methacrylate (PMMA) was spin-coated onto a SiO2 / Si surface on which Cu2Te two-dimensional material was deposited. The sample was then marked by electron beam exposure. Subsequently, metal was deposited on the surface. Finally, the gold film and PMMA were removed to obtain a photodetector.

[0075] Preferably, metal is deposited on the surface of Cu2Te two-dimensional material using a vacuum coating machine;

[0076] Preferably, the metal is Au, and its thickness is 40-60 nm.

[0077] The present invention also provides an optoelectronic device comprising the atomically thin Cu2Te two-dimensional material described above, or an optoelectronic device made of the atomically thin Cu2Te two-dimensional material described above.

[0078] Beneficial effects

[0079] This invention innovatively employs nested deposition tubes for the CVD deposition of Cu2Te two-dimensional materials, and combines this with the joint control of the temperature and copper source during the CVD deposition process. This unexpected synergy solves the problem of the difficulty in preparing Cu2Te two-dimensional materials, and enables the formation of Cu2Te two-dimensional materials with superior properties, especially atomically thin and large-sized materials, at lower temperatures. Furthermore, the materials prepared by this method exhibit excellent optoelectronic properties. In addition, this method is also applicable to two-dimensional material substrates, thus enabling the preparation of MX2-Cu2Te heterojunction materials in the industry.

[0080] This invention enables the preparation of single-crystal Cu2Te nanosheets with controllable thickness and good crystallinity through atmospheric pressure chemical vapor deposition at a preferred growth temperature.

[0081] The Cu₂Te nanosheets prepared in this invention can reach a thickness of up to 2.6 nm on a 285 nm SiO₂ / Si substrate, with a size ranging from 3 to 80 μm. They exhibit regular hexagonal or semi-trapezoidal morphologies and high crystal quality. This method can be used to fabricate Cu₂Te field-effect transistors and high-response photodetectors. The ultrathin Cu₂Te nanosheets prepared in this invention provide a foundation for studying their photoelectric properties at the two-dimensional scale and hold promise for applications in spintronics, nanoelectronics, and other fields.

[0082] This invention utilizes a simple atmospheric pressure chemical vapor deposition method to fabricate Cu2Te nanosheets with a thickness of 1.6 nm on a dangling bond-free MX2 substrate, such as MoS2, constructing an MX2-Cu2Te, or Cu2Te / MoS2 heterojunction. The Cu2Te / MoS2 heterojunction prepared in this invention provides a foundation for the study of their electrical properties at the two-dimensional scale and offers a reference for the fabrication of other two-dimensional p-type semiconductor materials.

[0083] The preparation process of this invention does not involve complicated operation steps or expensive raw materials. The equipment is simple, the operation is easy and convenient, and the reproducibility is good. Attached Figure Description

[0084] Figure 1 A schematic diagram of an atmospheric pressure chemical vapor deposition apparatus for preparing Cu2Te nanosheets;

[0085] Figure 2 Optical image of Cu2Te nanosheets fabricated on a SiO2 / Si substrate in Example 1-1;

[0086] Figure 3 Optical images of Cu2Te nanosheets fabricated on a MoS2 substrate in Examples 1-2;

[0087] Figure 4Optical images of Cu2Te nanosheets fabricated on WS2 substrates in Examples 1-3;

[0088] Figure 5 Optical images of Cu2Te nanosheets fabricated on SiO2 / Si substrates in Examples 1-4;

[0089] Figure 6 Optical images of Cu2Te nanosheets fabricated on SiO2 / Si substrates in Examples 1-5;

[0090] Figure 7 Optical images of Cu2Te nanosheets fabricated on SiO2 / Si substrates in Examples 1-6;

[0091] Figure 8 Optical images of Cu2Te nanosheets fabricated on SiO2 / Si substrates in Examples 1-7;

[0092] Figure 9 Optical images of Cu2Te nanosheets fabricated on SiO2 / Si substrates in Examples 1-8;

[0093] Figure 10 Optical images of Cu2Te nanosheets fabricated on SiO2 / Si substrates in Examples 1-9;

[0094] Figure 11 Optical images of Cu2Te nanosheets fabricated on SiO2 / Si substrates in Examples 1-10;

[0095] Figure 12 Optical images of Cu2Te nanosheets fabricated on SiO2 / Si substrates in Examples 1-11;

[0096] Figure 13 Optical images of Cu2Te nanosheets fabricated on SiO2 / Si substrates in Examples 1-12;

[0097] Figure 14 Optical image of Cu2Te nanosheets fabricated on a SiO2 / Si substrate in Comparative Example 1;

[0098] Figure 15 Optical image of Cu2Te nanosheets fabricated on MoS2 substrate in Comparative Example 2;

[0099] Figure 16 Optical image of Cu2Te nanosheets fabricated on SiO2 / Si substrate in Comparative Example 3;

[0100] Figure 17 Optical image of Cu2Te nanosheets fabricated on SiO2 / Si substrate in Comparative Example 4;

[0101] Figure 18 Optical image of Cu2Te nanosheets fabricated on SiO2 / Si substrate in Comparative Example 5;

[0102] Figure 19 An optical image of the thin-layer Cu2Te field-effect transistor of Example 1-1 in Example 2-1;

[0103] Figure 20 The output curve of the Cu2Te field-effect transistor in Example 1-1 of Example 2-1;

[0104] Figure 21 The transfer curve of the Cu2Te field-effect transistor in Example 1-1 of Example 2-1;

[0105] Figure 22 The output curves of the Cu2Te field-effect transistor from Example 1-1 in Example 2-1 at different temperatures;

[0106] Figure 23 An optical image of the slightly thicker Cu2Te field-effect transistor from Example 1-1 in Example 2-1;

[0107] Figure 24 The output curve of the Cu2Te field-effect transistor in Example 1-1 of Example 2-1;

[0108] Figure 25 The transfer curve of the Cu2Te field-effect transistor in Example 1-1 of Example 2-1;

[0109] Figure 26 Optical images of Cu2Te field-effect transistors from Examples 1-8 in Example 2-2;

[0110] Figure 27 The output curves of Cu2Te field-effect transistors from Examples 1-8 in Example 2-2;

[0111] Figure 28 The transfer curves of Cu2Te field-effect transistors from Examples 1-8 in Example 2-2;

[0112] Figure 29 This is a schematic diagram of the Cu2Te photodetector in Example 1-1 of Examples 2-3;

[0113] Figure 30 Optical images of the Cu2Te photodetector from Example 1-1 in Examples 2-3;

[0114] Figure 31 The output curves of the Cu2Te photodetector in Example 1-1 of Examples 2-3 under different optical powers;

[0115] Figure 32 This is a schematic diagram of the semiconductor diodes in Examples 1-2 of Examples 2-4;

[0116] Figure 33 The output curves of the Cu2Te / MoS2 semiconductor diodes in Examples 1-2 of Examples 2-4 are shown.

[0117] Figure 34 The output curves of the Cu2Te / WS2 semiconductor diodes in Examples 1-3 of Examples 2-4 are shown. Specific implementation methods:

[0118] The present invention will be further illustrated by the following implementation examples, but the content of the present invention is not limited to the following content.

[0119] This invention utilizes Figure 1 The nested deposition tubes shown are used for CVD deposition. Figure 1 The process involves an outer tube and an inner tube housed within the outer tube's cavity, the inner tube being a blind tube sealed at one end. During deposition, a copper source is pre-positioned at the opening of the inner tube, with the substrate positioned above the copper source at the inner tube's opening, and tellurium powder positioned at the sealed end of the inner tube. Subsequently, carrier gas is introduced into the outer tube for purging, and the inner tube is then temperature-controlled to allow the copper source-substrate temperature (T1, temperature zone 1, also known as the copper source volatilization temperature or deposition temperature) and the tellurium powder temperature (T2, temperature zone 2, also known as the tellurium powder volatilization temperature) to volatilize and be CVD deposited on the substrate, thus obtaining the aforementioned two-dimensional material.

[0120] In this invention, both the outer tube and the inner tube are straight quartz circular tubes, and their length directions are parallel. For ease of installation, the inner tube can be placed directly parallel to the bottom inner wall of the outer tube. In this invention, the diameter ratio of the outer tube and the inner tube is not particularly required and can be adjusted according to the manufacturing efficiency. For example, it can be 2 to 4:1. In the following examples, unless otherwise stated, 2:1 is used as a typical example.

[0121] The process described in this invention has no special requirements for the substrate and is unexpectedly suitable for Cu2Te deposition on the surface of MX2 two-dimensional materials, thereby enabling the formation of MX2-Cu2Te heterojunctions. The MX2 two-dimensional material described is prepared using conventional CVD and PVD methods.

[0122] For example, the preparation conditions for MoS2 two-dimensional materials are as follows: 2 mg of molybdenum trioxide and 30 mg of sulfur powder are placed in two different ceramic boats. A SiO2 / Si sheet is placed flat on the ceramic boat containing molybdenum trioxide with its bright side facing down. The ceramic boat containing sulfur powder is placed in the upstream temperature zone, and the ceramic boat containing molybdenum trioxide is placed in the downstream temperature zone. The carrier gas flow is kept constant at 60 sccm of argon. Within 20 minutes, the upstream and downstream temperature zones are raised to 800 and 150°C respectively, and held at these temperatures for five minutes. After the growth period, the tube furnace is allowed to cool naturally to room temperature.

[0123] Preparation method of WS2: A single-zone tube furnace was used. A ceramic boat loaded with WS2 powder was placed in the center of the furnace's temperature zone. A SiO2 / Si flat sheet with its bright side facing up was placed on the ceramic boat, downstream of the furnace. The temperature at the center of the furnace temperature zone was heated to 1195℃ with argon gas flowing in the reverse direction at 80 sccm. After reaching 1195℃, the flow direction of the 80 sccm carrier gas was reversed and maintained at a constant temperature for 2 minutes. After the growth process was completed, the argon gas flow direction was reversed again, and the furnace was allowed to cool naturally to ambient temperature.

[0124] 1. Preparation of Cu2Te nanosheets:

[0125] Example 1-1

[0126] The experimental setup diagram for Cu2Te nanosheets is shown below. Figure 1 As shown in the figure. Point 1 represents 285nm SiO2 / Si, point 2 represents cuprous iodide as the copper source, and point 3 represents elemental tellurium powder as the tellurium source. 30mg of cuprous iodide powder was placed at the open end of the inner tube in temperature zone 1 (temperature T1), and 15mg of elemental tellurium powder was placed in the closed section of the inner tube in temperature zone 2 (temperature T2). A 285nm SiO2 / Si substrate was placed in the inner tube above the CuI powder. Before heating, the air in the quartz tube was purged with a large flow of argon (gas purging). Then, T1 and T2 were raised to 480℃ and 540℃ respectively, with an argon flow rate of 60 sccm and a hydrogen flow rate of 1.5 sccm, and held at these temperatures for 15 minutes. Single-crystal Cu2Te nanosheets were formed on the SiO2 / Si substrate. An optical photograph of the prepared Cu2Te nanosheets is shown below. Figure 2 As shown.

[0127] The Cu2Te nanosheets obtained under these conditions have good crystallinity, are thin, and are distributed in the range of 8-12 nm, with a size of 7-37 μm. Figure 2 The scale bar is 20 μm.

[0128] Examples 1-2

[0129] Compared with Example 1-1, the difference is that MoS2 without dangling bonds is used as the substrate. Figure 3 This is an optical schematic diagram of Cu2Te nanosheets prepared on a MoS2 substrate. The Cu2Te nanosheets obtained under these conditions have good crystallinity, thin thickness, and are basically distributed at 1.6 nm. Figure 3 The scale bar is 5 μm.

[0130] Examples 1-3

[0131] Compared with Example 1-1, the difference is that WS2 without dangling keys is used as the substrate. Figure 4 This is an optical schematic diagram of Cu2Te nanosheets prepared on a WS2 substrate. The Cu2Te nanosheets obtained under these conditions have good crystallinity, thin thickness, and are basically distributed at 1.7 nm. Figure 4 The scale bar is 10 μm.

[0132] Examples 1-4

[0133] Compared with Example 1-1, the difference is that T1 is 460°C, T2 is 540°C, argon flow rate is 60 sccm, hydrogen flow rate is 1.5 sccm, and deposition time is 15 min. Figure 5 This is an optical schematic diagram of Cu2Te nanosheets prepared on a SiO2 / Si substrate. The Cu2Te nanosheets obtained under these conditions have good crystallinity, atomic-level thickness, small size, distributed in the range of 2-7 nm, and a size of 3-10 μm. Figure 5 The scale bar is 20 μm.

[0134] Examples 1-5

[0135] Compared with Example 1-1, the difference is that T1 is 490°C, T2 is 540°C, argon flow rate is 60 sccm, hydrogen flow rate is 1.5 sccm, and deposition time is 15 min. Figure 6 This is an optical schematic diagram of Cu2Te nanosheets prepared on a SiO2 / Si substrate. The Cu2Te nanosheets obtained under these conditions have good crystallinity, are slightly thick, and are distributed in the range of 15-26 nm with a size of 14-26 μm. Figure 6 The scale bar is 20 μm.

[0136] Examples 1-6

[0137] Compared with Example 1-1, the difference is that T1 is 480°C, T2 is 560°C, argon flow rate is 60 sccm, hydrogen flow rate is 1.5 sccm, and deposition time is 15 min. Figure 7This is an optical schematic diagram of Cu2Te nanosheets prepared on a SiO2 / Si substrate. The Cu2Te nanosheets obtained under these conditions have good crystallinity, are thick, and are distributed in the range of 30-35 nm with a size of 10-13 μm. Figure 7 The scale bar is 20 μm.

[0138] Examples 1-7

[0139] Compared with Example 1-1, the difference is that T1 is 480°C, T2 is 570°C, argon flow rate is 60 sccm, hydrogen flow rate is 1.5 sccm, and deposition time is 15 min. Figure 8 This is an optical schematic diagram of Cu2Te nanosheets prepared on a SiO2 / Si substrate. The Cu2Te nanosheets obtained under these conditions have good crystallinity, are thick, and are distributed in the range of 32-45 nm with a size of 14-18 μm. Figure 8 The scale bar is 20 μm.

[0140] Examples 1-8

[0141] Compared with Example 1-1, the only difference is that copper oxide of equal copper element weight is used instead of cuprous iodide as the raw material; all other operations and parameters are the same as in Example 1-1. The obtained material is shown in [reference needed]. Figure 9 The scale bar is 20 μm. The Cu2Te nanosheets obtained under these conditions are relatively thick, have an uneven surface, and irregular edge shapes.

[0142] Examples 1-9

[0143] Compared with Examples 1-2, the only difference is that copper oxide of equal copper element weight is used instead of cuprous iodide as the raw material; all other operations and parameters are the same as in Examples 1-2. The obtained material is shown in [reference needed]. Figure 10 The scale bar is 20 μm. The material prepared under these conditions was etched.

[0144] Examples 1-10

[0145] Compared to Examples 1-1, the only difference is that the argon flow rate used as the carrier gas is 60 sccm and the hydrogen flow rate is 3.5 sccm; all other operations and parameters are the same as in Examples 1-1. The obtained material is shown in [reference needed]. Figure 11 The scale bar is 20 μm. The material prepared under these conditions is thin, small in size, and has black particles distributed around it.

[0146] Examples 1-11

[0147] Compared to Examples 1-1, the only difference is that the argon flow rate used as the carrier gas is 90 sccm and the hydrogen flow rate is 1.5 sccm; all other operations and parameters are the same as in Examples 1-1. The obtained material is shown in [reference needed]. Figure 12The scale bar is 20 μm. The material prepared under these conditions has a large size, but large black particles are present around it.

[0148] Examples 1-12

[0149] Compared to Example 1-1, the only difference is that the deposition time is 25 min; all other operations and parameters are the same as in Example 1-1. The obtained material is shown in [reference needed]. Figure 13 The scale bar is 20 μm. The materials prepared under these conditions are all thicker than 100 nm, and many black particles are present around the samples.

[0150] Comparative Example 1

[0151] Compared to Example 1-1, the only difference is that the deposition apparatus only includes the outer tube and does not include the inner tube. Cuprous iodide powder and tellurium powder are placed in two separate ceramic boats. The ceramic boat containing tellurium powder is placed in upstream temperature zone one, and the ceramic boat containing cuprous iodide powder is placed in downstream temperature zone two. A SiO2 / Si substrate is placed flat on the ceramic boat containing cuprous iodide powder, with the bright side facing down. All other operations and parameters are the same as in Example 1-1. The obtained material is shown in [reference needed]. Figure 14 The scale bar is 20 μm. The material obtained under these conditions consists of small black particles.

[0152] Comparative Example 2

[0153] Compared to Example 1-1, the only difference is that the temperature T1 is increased to 580°C; all other operations and parameters are the same as in Example 1-1. The obtained material is shown in [reference needed]. Figure 15 The scale bar is 10 μm. The material prepared under these conditions is small in size, thick in thickness, and has an irregular morphology.

[0154] Comparative Example 3

[0155] Compared with Example 1-1, the only difference is that the temperature of T2 is increased to 650°C. All other operations and parameters are the same as in Example 1-1. The material obtained is shown in [reference needed]. Figure 16 The scale bar is 20 μm. The Cu₂Te nanosheets obtained under these conditions are blue-purple, sparsely distributed, small in size, and thick, with thicknesses all greater than 100 nm.

[0156] Comparative Example 4

[0157] Compared to Example 1-1, the only difference is that cuprous iodide is replaced with cuprous chloride, while the amount of copper remains the same. Other operations and parameters are the same as in Example 1-1. The resulting material is shown in [reference needed]. Figure 17 The scale bar is 20 μm. The materials prepared under these conditions are small in size, few in quantity, and mostly consist of small black particles.

[0158] Comparative Example 5

[0159] Compared to Examples 1-1, the only difference is that the carrier gas does not contain hydrogen; only argon at 60 sccm is used as the protective gas. All other operations and parameters are the same as in Examples 1-1. The obtained material is shown in [reference needed]. Figure 18 The scale bar is 10 μm. The material prepared under these conditions appears as purple dots.

[0160] 2. Fabrication of field-effect transistors and their application in two-dimensional materials

[0161] Example 2-1

[0162] The method for fabricating Cu2Te field-effect transistors involves spin-coating a layer of polymethyl methacrylate (PMMA) onto Cu2Te nanosheets prepared by CVD (materials obtained in Examples 1-1 or 1-4), then marking the sample with electron beam exposure, followed by depositing 50 nm Au on the surface, and finally removing the gold film and PMMA with acetone to obtain Cu2Te field-effect transistors of different thicknesses.

[0163] Optical images of thin-layer (referring to the two-dimensional material with a thickness of 3-5 nm obtained in Examples 1-4) Cu2Te field-effect transistors are shown below. Figure 19 As shown.

[0164] Figure 19 In the figure, the SiO2 / Si substrate is gray, Cu2Te is pinkish-purple, and the long golden rectangle on the Cu2Te surface is deposited metallic Au. The scale bar in the figure is 5 μm.

[0165] The electrical transport and transfer characteristic curves obtained from the tests are as follows: Figure 20 and Figure 21 As shown, this indicates that gate modulation weakens when the Cu2Te thickness is thinner. The electrical transport characteristic curves obtained at different temperatures are shown below. Figure 22 As shown, this demonstrates that the Cu2Te nanosheets prepared in this invention are semiconductors.

[0166] Optical images of relatively thick Cu₂Te field-effect transistors (referring to the two-dimensional material with a thickness of 8-12 nm prepared in Example 1-1) are shown below. Figure 23 As shown.

[0167] Figure 23 In the figure, the SiO2 / Si substrate is grayish-purple, Cu2Te is yellowish-white, and the long golden rectangle on the Cu2Te surface is deposited metallic Au. The scale bar in the figure is 5 μm.

[0168] The electrical transport and transfer characteristic curves obtained from the tests are as follows: Figure 24 and Figure 25 As shown, this demonstrates that the Cu₂Te nanosheets prepared in this invention are p-type semiconductors.

[0169] Example 2-2

[0170] Compared with Example 2-1, field-effect transistors were prepared using Cu2Te nanosheets obtained in Examples 1-8, with all other specific operations and parameters being the same as in Example 2-1.

[0171] Optical images of Cu2Te field-effect transistors are shown below. Figure 26 As shown.

[0172] Figure 26 In the figure, the SiO2 / Si substrate is gray, Cu2Te is a non-uniform hexagonal surface, and the gold rectangle on the Cu2Te surface is deposited metal Au. The scale bar in the figure is 5 μm.

[0173] The electrical transport and transfer characteristic curves obtained from the tests are as follows: Figure 27 and Figure 28 As shown, when the Cu2Te thickness is thick and the surface is uneven, the gate modulation is weakened and the current is unstable. This proves that the cuprous iodide raw material selected in this invention, compared with copper oxide of the same copper element weight, produces Cu2Te nanosheets with higher crystallinity and electrical properties.

[0174] Example 2-3

[0175] The fabrication method of the Cu2Te photodetector involves spin-coating a layer of polymethyl methacrylate (PMMA) onto Cu2Te nanosheets prepared by CVD (materials obtained in Example 1-1), followed by electron beam exposure labeling of the sample, and then depositing 50 nm Au on the surface. Finally, the gold film and PMMA are removed with acetone to obtain the Cu2Te photodetector. The Cu2Te photodetector is then irradiated with a 520 nm wavelength laser as the incident light. A schematic diagram is shown below. Figure 29 As shown; optical images of the Cu2Te photodetector are as follows. Figure 30 As shown.

[0176] Figure 30 In the figure, the SiO2 / Si substrate is grayish-purple, Cu2Te is blue-purple, and the long golden rectangle on the Cu2Te surface is deposited metal Au. The scale bar in the figure is 5 μm.

[0177] Irradiation with a 520nm wavelength laser at different optical powers Figure 30 The electrical transfer characteristic curves obtained from the Cu2Te photodetector test are shown below. Figure 31 As shown, the Cu₂Te photodetector prepared in this invention exhibits a significant increase in current as the optical power increases.

[0178] Examples 2-4

[0179] The fabrication method of Cu2Te / MoS2 or Cu2Te / WS2 semiconductor diodes involves spin-coating a layer of polymethyl methacrylate (PMMA) onto Cu2Te nanosheets (materials obtained in Examples 1-2 or 1-3) prepared on a MoS2 or WS2 substrate. The sample is then labeled using electron beam lithography. Subsequently, 50 nm Au is deposited on the upper Cu2Te layer and the lower MoS2 layer as the drain and source, respectively. Finally, the gold film and PMMA are removed with acetone to obtain the Cu2Te / MoS2 (Cu2Te / WS2) semiconductor diode. A schematic diagram is shown below. Figure 32 As shown.

[0180] The transfer characteristic curve of the Cu2Te / MoS2 semiconductor diode is shown below. Figure 33 As shown in the figure. The transfer characteristic curve of the Cu2Te / WS2 semiconductor diode is as follows. Figure 34 As shown, the semiconductor diode prepared by this invention has a rectification ratio. In summary, the successful preparation of two-dimensional p-type semiconductor Cu2Te nanosheets requires a deposition apparatus with nested quartz tubes. Based on this, controlling the volatilization temperature of the raw materials, selecting a substrate without dangling bonds (e.g., MoS2), and choosing cuprous iodide as the raw material can further reduce the thickness of the two-dimensional Cu2Te material, improving crystal quality and electrical performance.

Claims

1. A method for preparing atomically thin Cu₂Te two-dimensional materials, characterized in that, CVD deposition is performed using nested deposition tubes, wherein the deposition tube includes an outer tube with an air inlet and an air outlet, and an inner tube disposed within the outer tube chamber; the inner tube is open at the air inlet end and sealed at the other end. During the CVD deposition process, the copper source and substrate are pre-positioned on the open side of the inner tube, and the tellurium source is positioned on the sealed side of the inner tube. Carrier gas is introduced into the deposition tube through the gas inlet for purging. Subsequently, the temperature of the inner tube is controlled, so that the temperature T1 at the copper source and substrate on the open side of the inner tube is controlled at 460~510℃, and the temperature T2 at the tellurium source on the sealed side is controlled at 530~570℃. This allows the copper source and tellurium source to volatilize in the inner tube and be CVD deposited on the substrate, thus obtaining the atomically thin Cu2Te two-dimensional material. The copper source is copper oxide and / or cuprous iodide.

2. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 1, characterized in that, Both the inner and outer tubes of the deposition tube are quartz tubes.

3. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 2, characterized in that, Both the inner and outer tubes are cylindrical straight tubes.

4. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 3, characterized in that, The inner and outer tubes are parallel in length.

5. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 4, characterized in that, The diameter ratio of the inner tube to the outer tube is 0.1 to 0.5:

1.

6. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 1, characterized in that, The copper source is cuprous iodide.

7. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 1, characterized in that, The source of tellurium is tellurium powder.

8. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 1, characterized in that, The mass ratio of copper source to tellurium source is 1~5:

1.

9. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 1, characterized in that, The substrate is a silicon wafer or a substrate with a two-dimensional MX2 layer grown on its surface; The silicon wafer is a 285 nm SiO2 / Si substrate; In the two-dimensional MX2, M is a transition metal element containing at least one of Mo or W, and X is a chalcogenide element containing at least one of S or Se.

10. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 1, characterized in that, The carrier gas is a hydrogen-containing atmosphere.

11. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 10, characterized in that, The carrier gas is a mixture of hydrogen and a protective gas; The protective gas is at least one of nitrogen or an inert gas.

12. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 11, characterized in that, In the carrier gas, the flow rate of the protective gas is 10~200 sccm, and the flow rate of the hydrogen gas is 0.1~10 sccm.

13. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 12, characterized in that, In the carrier gas, the flow rate of the protective gas is 40~100 sccm, and the flow rate of the hydrogen gas is 1~5 sccm.

14. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 1, characterized in that, The temperature T1 is 460~490℃; The T2 is 540~560℃.

15. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 14, characterized in that, The temperature T1 is 475~485℃; The T2 is 540~545℃.

16. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 1, characterized in that, The CVD deposition time for the vapor phase is 10-25 min.

17. The method for preparing atomically thin Cu₂Te two-dimensional material as described in claim 16, characterized in that, The CVD deposition time for the vapor phase was 14–16 min.

18. An atomically thin Cu₂Te two-dimensional material prepared by the method according to any one of claims 1 to 17; characterized in that, This includes a substrate and a two-dimensional Cu2Te material with a hexagonal phase composited on its surface.

19. The atomically thin Cu₂Te two-dimensional material as described in claim 18; characterized in that, The thickness of the Cu2Te two-dimensional material is 2~50 nm, and the size is 3~80 μm; The substrate is a substrate with two-dimensional MX2 grown on its surface, and the atomically thin Cu2Te two-dimensional material is an MX2-Cu2Te heterojunction.

20. An application of the atomically thin Cu₂Te two-dimensional material as described in claim 18 or 19, characterized in that, It is used to prepare optoelectronic devices.

21. The application of the atomically thin Cu₂Te two-dimensional material as described in claim 20, characterized in that, The aforementioned optoelectronic device is a field-effect transistor or a semiconductor diode.

22. The application of the atomically thin Cu₂Te two-dimensional material as described in claim 21, characterized in that, The field-effect transistor includes a channel Cu2Te, a dielectric layer SiO2, source and drain Au, and a gate Si; The fabrication steps of the aforementioned field-effect transistor are as follows: A layer of PMMA was spin-coated onto the SiO2 / Si surface on which Cu2Te two-dimensional material was deposited. The sample was then marked by electron beam exposure. Au was then deposited on the Cu2Te two-dimensional material surface using a vacuum coating machine. Finally, the Au film and PMMA were removed to obtain a field-effect transistor. The thickness of the deposited Au was 40-60 nm.

23. The application of the atomically thin Cu₂Te two-dimensional material as described in claim 21, characterized in that, The semiconductor diode is fabricated from the obtained MX2-Cu2Te heterojunction using the following steps: A layer of PMMA was spin-coated onto a SiO2 / Si surface with an MX2-Cu2Te heterojunction, and the sample was then marked by electron beam exposure. Au was deposited on the heterojunction surface using a vacuum coating machine. Finally, the Au film and PMMA were removed to obtain a semiconductor diode. The thickness of the deposited Au was 40~60 nm.

24. The application of the atomically thin Cu₂Te two-dimensional material as described in claim 20, characterized in that, The optoelectronic device is a photodetector, which includes a channel Cu2Te, a dielectric layer SiO2, source and drain electrodes Au, and a gate Si. The steps for fabricating a photodetector using the atomically thin Cu2Te two-dimensional material are as follows: A layer of PMMA was spin-coated onto the SiO2 / Si surface on which Cu2Te two-dimensional material was deposited. The sample was then marked by electron beam exposure. Au was deposited on the surface of Cu2Te two-dimensional material using a vacuum coating machine. Finally, the Au film and PMMA were removed with acetone to obtain a photodetector. The thickness of the deposited Au was 40-60 nm.