Method for forming thin-walled cylindrical blank forgings
By combining vacuum induction and electroslag heating with free forging and rolling processes, the problems of low production efficiency and low raw material utilization of thin-walled cylindrical blank forgings have been solved, enabling mass production and high-efficiency manufacturing.
Patent Information
- Application Number
- CN202410342237.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-25
AI Technical Summary
The existing thin-walled cylindrical blank forgings have low production efficiency, low raw material utilization, and difficult-to-control dimensions. In particular, the process of dividing thin-walled cylindrical blank forgings with a height ≤600mm into small blanks is cumbersome, with large forging allowances and extremely low production efficiency.
The process involves heating steel ingots using vacuum induction and electroslag heating, combined with free forging and rolling. The ingots are then upset and drawn into round forgings, followed by rolling and annealing, and finally sawn into thin-walled cylindrical blanks according to dimensional requirements.
This has enabled the mass production of thin-walled cylindrical blank forgings, improving production efficiency, reducing forging allowance, and enhancing raw material utilization and product quality.
Smart Images

Figure CN118106705B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of thin-walled cylindrical forging technology, and specifically relates to a method for forming thin-walled cylindrical blank forgings. Background Technology
[0002] 31Si2MnCrMoVE (material code: D406A) is a low-alloy ultra-high-strength steel, generally used to manufacture aircraft landing gear, connecting shafts, and solid rocket motor casings. Solid rocket motors are the main power equipment of modern missile weapons, and the motor casing serves as both a propellant tank and a fuel chamber. Thin-walled cylindrical forging blanks are the blanks used to manufacture solid rocket motor casings.
[0003] The general manufacturing method for thin-walled cylindrical blank forgings is to forge steel ingots into round billets, then divide the billets into smaller blanks, each of which produces one thin-walled cylindrical blank forging. Depending on the specifications, each steel ingot can produce 2 to 25 thin-walled cylindrical blank forgings. For thin-walled cylindrical blank forgings with a height ≤600mm, the method of dividing into smaller blanks is very cumbersome. It requires a saw to divide the round billet into smaller blanks, which are then heated at high temperatures and then processed one by one on a free forging press or hammer forging machine through upsetting, punching, reaming, and leveling. Because the operation of small parts is very cumbersome, it takes two shifts to complete the forging process of about 10 thin-walled cylindrical blank forgings, resulting in extremely low production efficiency. Furthermore, the dimensions of free-forged ring and cylindrical parts are difficult to control, and the forging allowance is relatively large. Generally, the diameter allowance of a free-forged thin-walled cylindrical blank is about 40mm on both sides, the inner hole is about 60mm on both sides, and the height is about 50mm. Therefore, the utilization rate of raw materials is low. Summary of the Invention
[0004] The purpose of this invention is to address the shortcomings of existing technologies by providing a method for mass-producing thin-walled cylindrical blank forgings with a wall thickness between 15mm and 38mm and an outer diameter between φ500mm and φ820mm. This method can significantly improve production efficiency, reduce blank forging allowance, and increase raw material utilization.
[0005] To achieve the above objectives, the present invention provides a method for forming thin-walled cylindrical blank forgings, as detailed below:
[0006] 1) After heating the vacuum induction + electroslag steel ingot, it is upsetting and drawing into a round billet forging on a free forging press;
[0007] 2) After annealing the round billet forging, rough machine the surface of the round billet forging to remove white residue;
[0008] 3) Heating the machined round billet forging;
[0009] 4) If the outer diameter of the thin-walled cylindrical blank forging is φ700mm~φ820mm, it shall be rolled in two heats; if the outer diameter of the thin-walled cylindrical blank forging is φ500mm~φ699mm, it shall be rolled in one heat; and rolled into a thin-walled cylindrical blank tube with a wall thickness of 15~38mm.
[0010] 5) The thin-walled cylindrical blank tube is subjected to normalizing and spheroidizing annealing as a whole, and then sawn into the required thin-walled cylindrical blank forgings according to the size requirements.
[0011] Furthermore, the surface of the steel ingot heated by vacuum induction + electroslag in step 1) is machined before heating.
[0012] Furthermore, the specific process of vacuum induction + electroslag heating of steel ingots in step 1) is as follows: the steel ingot is kept at 500℃~550℃ for 2~3 hours, then the temperature is raised to 850±10℃ at a rate of 60~80℃ / h, kept at 850±10℃ for 4~5 hours, and then raised to 1190±10℃ and kept for 6~8 hours before being taken out of the furnace.
[0013] Furthermore, the specific process of heating the machined round billet forging in step 3) is as follows: first, heat to 650±10℃ and hold for 2 to 3 hours, then control the temperature to 850±10℃ at 60 to 80℃ / h, hold at 850±10℃ for 3 to 4 hours, and then heat to 1180±10℃ for sufficient holding before removing from the furnace.
[0014] Further, in step 4), if the outer diameter of the thin-walled cylindrical blank forging is φ700mm~φ820mm, then a two-fire rolling process is adopted. The specific process is as follows: the first fire is held at 1180±10℃ for 7~8 hours, and the diameter expansion amount of the first fire rolling is 10%~15%; the second fire is held at 1180±10℃ for 4~5 hours, and the diameter expansion amount of the second fire rolling is 4%~5%. The total diameter expansion amount of the two fires is controlled at 14%~20%.
[0015] Furthermore, in step 4), if the outer diameter of the thin-walled cylindrical blank forging is φ500mm~φ699mm, it is rolled in one heat and held at 1180±10℃ for 7~8 hours, with an expansion amount of 10%~15%.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention combines free forging and rolling. For thin-walled cylindrical blank forgings of different specifications, it is only necessary to freely forge blanks of different diameters and use different heats and tooling during rolling to mass-produce thin-walled cylindrical blank forgings with wall thickness between 15mm and 38mm and outer diameter between φ500mm and φ820mm. This can not only greatly improve production efficiency, reduce blank forging allowance, but also improve raw material utilization. Detailed Implementation
[0017] The present invention will be further described in detail below with reference to specific embodiments.
[0018] The method for forming thin-walled cylindrical blank forgings is as follows:
[0019] The first step is to machine the surface of the vacuum induction + electroslag steel ingot with a diameter of φ650mm, with a single-sided machining amount of 10mm, to eliminate casting defects such as porosity and scale on the surface of the steel ingot, while improving the surface smoothness of the steel ingot and avoiding surface fine cracks caused by surface porosity and scale during the forging process; the diameter of the steel ingot after surface machining is φ630mm.
[0020] The second step involves holding the φ630mm diameter steel ingot at 500℃~550℃ for 2~3 hours, then raising the temperature to 850±10℃ at a rate of 60~80℃ / h, holding it at 850±10℃ for 4~5 hours, and then raising the temperature to 1190±10℃ and holding it for 6~8 hours before removing it from the furnace. The steel ingot is then upsetting and drawing into a round billet forging on a free forging press.
[0021] The third step is to anneal the round billet forging and then rough machine the surface of the round billet forging to remove the white residue. The diameter of the machined round billet forging is smaller than the diameter of the thin-walled cylindrical billet forging. The rough machining removes the pits, black skin and fine cracks on the surface of the round billet forging after forging, ensuring that the surface is smooth and flat during rolling.
[0022] The fourth step is to heat the machined round billet forging. First, heat it to 650±10℃ and hold it for 2 to 3 hours. Then, control the temperature to rise to 850±10℃ at a rate of 60 to 80℃ / h and hold it at 850±10℃ for 3 to 4 hours. Finally, heat it to 1180±10℃ and hold it for a sufficient period of time before rolling it out of the furnace.
[0023] Fifth step: If the outer diameter of the thin-walled cylindrical blank forging is φ700mm~φ820mm, then two-fire rolling is adopted. The specific process is as follows: the first fire is held at 1180±10℃ for 7~8 hours, and the diameter expansion amount of the first fire is 10%~15%; the second fire is held at 1180±10℃ for 4~5 hours, and the diameter expansion amount of the second fire is 4%~5%. The total diameter expansion amount of the two fires is controlled at 14%~20%. If the outer diameter of the thin-walled cylindrical blank forging is φ500mm~φ699mm, then one-fire rolling is adopted. The first fire is held at 1180±10℃ for 7~8 hours, and the diameter expansion amount is 10%~15%. The thin-walled cylindrical blank tube with a wall thickness of 15~38mm is rolled into a tube.
[0024] The sixth step involves normalizing and spheroidizing annealing the entire thin-walled cylindrical blank tube, and then sawing it into the required thin-walled cylindrical blank forgings according to the dimensional requirements.
[0025] The specific process of normalizing + spheroidizing annealing is as follows:
[0026] After rolling, the thin-walled cylindrical blank tubes are air-cooled to room temperature as a whole, and then loaded into the furnace as a whole, supported by multiple arc-shaped shims to prevent deformation during heat treatment due to the thin wall thickness of the cylindrical blank tubes. The temperature is raised to 650±10℃ and held for 0.5 to 1 hour, then raised to 920±10℃ at a rate of ≤80℃ / h, held at 920±10℃ for 2 to 3 hours, and then air-cooled. After air-cooling to room temperature, the temperature is raised to 720±10℃ at a rate of ≤80℃ / h and held for 0.5 to 1 hour, then raised to 810±10℃ at a rate of ≤80℃ / h and held for 3 to 4 hours, then furnace-cooled to 740±10℃ and held for 24 to 28 hours, then furnace-cooled to 670±10℃ and held for 2 to 3 hours, and finally removed from the furnace and air-cooled to room temperature.
[0027] The ends of the thin-walled cylindrical blank tube are sawn flat, and hardening tests are performed on the end face at 90° intervals. The hardness is uniform, and the HB of each point is ≤205. The grain size of the bulk material is ≥4.
[0028] 100mm test rings were cut from both ends to test material properties. The heat treatment regime for material properties was as follows: normalizing: 920℃ for 1 hour, air cooling; quenching: 930℃ for 1 hour, oil cooling; tempering: 300℃ for 3 hours, air cooling. Tensile and impact tests were performed on transverse and longitudinal test bars, and the fracture toughness Kic was measured. All mechanical properties met the following standards: σb≥1620MPa, σ0.2≥1320MPa, δ5≥8%, Ψ≥30%, AkU2≥35J, and KIC≥80MPa√m. However, overall, the transverse mechanical properties were significantly better than the longitudinal mechanical properties, and the grain size was ≥6 in both cases.
[0029] This invention combines free forging and rolling. For thin-walled cylindrical blank forgings of different specifications, only free forging is required to form blanks of different diameters. During rolling, different heat treatments and tooling are used to form multiple thin-walled cylindrical blank forgings in one operation. This invention can ensure the mass production and high-efficiency production of thin-walled cylindrical blank forgings. At the same time, it greatly reduces the forging allowance of thin-walled cylindrical blank forgings, improves the utilization rate of raw materials and product quality.
Claims
1. A method for forming a thin-walled cylindrical blank forging, characterized in that: The molding method is as follows: 1) After heating the vacuum induction + electroslag steel ingot, it is upsetting and drawing into a round billet forging on a free forging press; 2) After annealing the round billet forging, rough machine the surface of the round billet forging to remove white residue; 3) Heating the machined round forging blank; 4) If the outer diameter of the thin-walled cylindrical blank forging is φ700mm~φ820mm, a two-fire rolling process is adopted. The specific process is as follows: the first fire is held at 1180±10℃ for 7~8 hours, and the diameter expansion amount of the first fire is 10%~15%; the second fire is held at 1180±10℃ for 4~5 hours, and the diameter expansion amount of the second fire is 4%~5%. The total diameter expansion amount of the two fires is controlled at 14%~20%. If the outer diameter of the thin-walled cylindrical blank forging is φ500mm~φ699mm, a single fire rolling process is adopted. The thin-walled cylindrical blank tube with a wall thickness of 15~38mm is rolled, and the first fire is held at 1180±10℃ for 7~8 hours, with a diameter expansion amount of 10%~15%. 5) The thin-walled cylindrical blank tube is subjected to normalizing and spheroidizing annealing as a whole, and then sawn into the required thin-walled cylindrical blank forgings according to the size requirements.
2. The method for forming a thin-walled cylindrical blank forging according to claim 1, characterized in that: The surface of the steel ingot in step 1) is machined before vacuum induction + electroslag heating.
3. The method for forming a thin-walled cylindrical blank forging according to claim 1, characterized in that: The specific process of vacuum induction + electroslag heating of steel ingots in 1) is as follows: the steel ingot is kept at 500℃~550℃ for 2~3 hours, then the temperature is raised to 850±10℃ at a rate of 60~80℃ / h, kept at 850±10℃ for 4~5 hours, and then raised to 1190±10℃ and kept for 6~8 hours before being taken out of the furnace.
4. The method for forming a thin-walled cylindrical blank forging according to claim 1, characterized in that: The specific process of heating the machined round billet forging in 3) is as follows: first, heat to 650±10℃ and hold for 2~3 hours, then control the temperature to 850±10℃ at 60~80℃ / h, hold at 850±10℃ for 3~4 hours, then heat to 1180±10℃ and hold for a sufficient time before taking it out of the furnace.
Citation Information
Patent Citations
Method for producing seamless steel pipe for producing gas cylinder with heavy caliber for hauled vehicle
CN101439350A
Large cylindrical forge piece forging and rolling composite production technology
CN108994249A