A method for recovering aluminum fluoride from solid waste from aluminum electrolysis
By generating calcium fluoride through low-temperature roasting and combining it with water leaching and aluminate leaching, the problem of resource waste such as Na, Al and F in aluminum electrolysis solid waste is solved, achieving efficient and safe aluminum fluoride recovery, which is applicable to a wide range of aluminum plant solid waste treatment.
Patent Information
- Application Number
- CN202410117391.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-29
AI Technical Summary
In existing technologies, a large amount of resources such as Na, Al and F, other than lithium, in aluminum electrolysis solid waste cannot be effectively recovered, resulting in resource waste. Furthermore, existing methods are difficult to industrialize and involve the use of high-temperature and highly corrosive substances.
The process involves calcining calcium salts and pulverized solid waste at a low temperature of 300℃-600℃ to produce the intermediate product calcium fluoride chloride. This is then combined with water leaching and aluminate leaching, followed by pH adjustment and further calcination to obtain aluminum fluoride products. This method avoids the use of strong acids and alkalis, reducing the risk of equipment corrosion and the generation of waste residue and wastewater.
It achieves efficient recovery of aluminum fluoride from aluminum electrolysis solid waste, reduces energy consumption and cost, improves operational safety, is suitable for the treatment of high-concentration fluorine, has good recovery effect, wide applicability, and is applicable to most aluminum plant solid waste.
Smart Images

Figure CN118125479B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum electrolysis resource utilization technology, and in particular to a method for recovering aluminum fluoride from solid waste from aluminum electrolysis. Background Technology
[0002] With the ever-increasing demand for aluminum materials, the mainstream industrial method for aluminum production remains molten salt electrolysis, with fluoride molten salt systems being the most widely used. Therefore, as the aluminum industry continues to advance, the demand for electrolytes supporting production is also constantly increasing. Furthermore, due to the frequent sampling, overhauls, or shutdowns of the electrolyte during electrolytic aluminum production, a large amount of waste electrolyte is generated. Currently, waste electrolyte is generally piled up on a certain area of open ground. This accumulation not only wastes a significant amount of land but also causes significant environmental damage over time. Simultaneously, a large amount of aluminum fluoride is added during aluminum production to adjust the molecular ratio of the electrolyte. The accumulation of waste electrolyte also results in a significant waste of its rich aluminum fluoride resources. Therefore, there is an urgent need to find a green and environmentally friendly method for recycling aluminum electrolytes.
[0003] Currently, Chinese invention patent CN110240182A discloses a method for the resource recovery of waste lithium-containing aluminum electrolytes. This method mainly involves calcining and modifying the electrolyte, then using water-soluble inorganic salts as leaching agents to recover the electrolyte, followed by impurity removal from the filtrate for lithium extraction. However, in this method, after water leaching, aluminum and calcium ions exist in the form of aluminum fluoride and calcium fluoride, making further separation of aluminum and calcium difficult; they coexist in the leaching residue, resulting in resource waste. Additionally, Chinese invention patent CN115216630A proposes a method for leaching waste electrolytes that combines phase transformation and leaching. The method describes that the first reactant includes at least one of NaOH, KOH, Ba(OH)2, Ca(OH)2, MgCl2, CaCl2, BaCl2, Mg(NO3)2, Ca(NO3)2, Ba(NO3)2, and their hydrates; the second reactant includes at least one of NaOH, KOH, Ba(OH)2, Ca(OH)2, CaO, MgCl2, CaCl2, BaCl2, Mg(NO3)2, Ca(NO3)2, Ba(NO3)2, and their hydrates. In the pyrometallurgical roasting and transformation process, the two added additives are directly roasted at high temperatures (above 800℃) to prepare calcium fluoride. The required reaction temperature is extremely high, resulting in high energy consumption of raw materials. Furthermore, in the subsequent leaching process, aluminum enters the leaching residue in the form of calcium aluminate and mixes with calcium fluoride, resulting in a complex composition of the leaching residue that cannot be recycled. Finally, Chinese invention patent CN115198111A discloses a method for extracting lithium from lithium-containing waste aluminum electrolyte. This method involves mixing the electrolyte with additives and then calcining it at an ultra-high temperature of 850-1200℃, followed by a water leaching process to extract lithium. This process only recovers Li from the electrolyte; the higher concentrations of Al and F are not effectively utilized. In other words, the three patents primarily address the lithium extraction process from waste electrolytes. Furthermore, the methods proposed in these three patents are only applicable to lithium-containing aluminum electrolytes, limiting their applicability. They cannot be used for other solid waste generated by aluminum plants. Additionally, this method mainly extracts lithium from the electrolyte, failing to effectively recover higher concentrations of Na, Al, and F, resulting in significant resource waste.
[0004] Furthermore, in Chinese invention CN115216630A, the reactant used is molten sodium hydroxide (Example 1 in the original text). Sodium hydroxide is caustic soda, which is extremely corrosive and dangerous in its molten state, requiring very high standards for equipment and operating environment. In the subsequent defluorination process, activated alumina is chosen as the adsorbent (original text: during defluorination, the amount of activated alumina used is 10mg / g of alumina based on the fluoride adsorption capacity). It is difficult to achieve the expected defluorination effect, resulting in incomplete defluorination and a significant impact on the purity of subsequent products.
[0005] For CN115198111A, directly selecting metal salts for roasting will generate a large amount of non-recyclable polluting gases such as SO2, HCl, and N2O5.
[0006] Chinese patent CN114438329A discloses a comprehensive recovery method for waste lithium-containing aluminum electrolytes. First, the electrolyte is leached at high temperature in a mixed solution of high-concentration aluminum chloride and hydrochloric acid. Then, it is filtered with a strong alkali to obtain filter residue and filtrate, causing aluminum to precipitate with the residue. The residue is then dried and calcined to obtain aluminum fluoride. Next, sulfate is added to the filtrate after filtration with the strong alkali to remove calcium, and finally, lithium is extracted. In other words, this method can recover high-value lithium from waste electrolytes. Although the method includes an aluminum extraction step, its production process involves a large amount of strong acid salts (high-concentration hydrochloric acid). Furthermore, the aluminum extraction process consumes a large amount of alkali solution, and the hydrochloric acid used will cause significant corrosion to the equipment. However, this process uses both strong acids and alkalis, making industrial implementation difficult. Additionally, the sulfate introduced during calcium removal further complicates the solution composition. Moreover, since calcium sulfate is only slightly soluble in water, the dissolution of calcium sulfate is not complete precipitation; some calcium ions will dissolve in water, meaning that calcium removal using sulfate is not thorough. Summary of the Invention
[0007] (a) Technical problems to be solved
[0008] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a method for recovering aluminum fluoride from solid waste from aluminum electrolysis. This method solves the technical problem that the general waste electrolyte only removes lithium, while large amounts of Na, Al and F are not effectively recovered, resulting in a great waste of resources, and that the existing waste electrolyte aluminum extraction method is difficult to industrialize.
[0009] (II) Technical Solution
[0010] To achieve the above objectives, the main technical solutions adopted by the present invention include:
[0011] A method for recovering aluminum fluoride from solid waste from aluminum electrolysis, the method comprising the following steps:
[0012] S1. Pulverize solid waste to make powder;
[0013] S2. The powder from S1 is mixed with the first reactant to obtain a powder mixture, wherein the first reactant is a calcium salt;
[0014] S3. The powder mixture in S2 is roasted at a certain temperature to obtain the first roasted residue, and the certain temperature range is between 300℃ and 600℃.
[0015] S4. The first roasted residue in S3 is soaked in water, and after soaking, it is filtered to obtain water-soaked residue and water-soaked liquid.
[0016] S5. Mix the water-impregnated residue from S4 with the first auxiliary sintering agent to obtain the second calcined residue;
[0017] S6. Add the second roasted residue from S5 to an aluminate leaching or acid leaching solution, filter, and obtain a leaching solution and a leaching residue.
[0018] S7. Adjust the pH of the leachate from S6 and filter it to obtain filter residue and filtrate. Calcine the obtained filter residue to obtain aluminum fluoride.
[0019] This invention proposes a method for recovering aluminum fluoride from solid waste from aluminum electrolysis. The method involves mixing calcium salts with pulverized solid waste to obtain a powder mixture, which is then subjected to low-temperature calcination at 300℃-600℃. During calcination, the remaining fluoride ions are not directly destroyed in one step; instead, an intermediate product, calcium fluoride chloride, is generated under low-temperature conditions. This requires a lower temperature. Furthermore, it should be noted that in existing technologies, the reaction between solid waste and reactants is carried out at high temperatures above 800℃. Compared to existing technologies, this invention operates at low temperatures and first generates the intermediate product, forming molten calcium fluoride chloride, allowing the powder to react from the inside out, resulting in a more thorough and easier reaction. In comparison, this method avoids the drawbacks of traditional processes involving strong acids and alkalis at high temperatures, such as high-temperature melting or leaching. The entire process involves no strong acids or alkalis, the calcined raw materials are all neutral salts, there are almost no requirements for equipment, no hazardous gases are generated, operation is safe, environmentally friendly, and the operating environment is very safe. This avoids the large amounts of waste residue and wastewater generated in traditional processes.
[0020] Optionally, the leaching residue obtained in S6 is further fed into the second roasted residue for leaching.
[0021] Optionally, in S7, the obtained filtrate is recycled to S6.
[0022] Optionally, it also includes selectively extracting lithium based on the lithium ion content in the aqueous extract obtained in S4;
[0023] If the aqueous extract contains lithium ions, calcium is removed first, and then lithium is extracted by evaporation to obtain lithium salt.
[0024] Optionally, the solid waste mentioned in S1 includes any one of the following: waste aluminum electrolyte, furnace bottom sediment, and anode covering material, wherein each element is predominantly Na3AlF6, Na5Al3F6, etc. 14Li₂NaAlF₆, Li₃Na₃AlF₆ 12 It exists in one or more of the forms of Na2MgAlF7 and LiCaAlF7, with a Li content of 0-3%.
[0025] Optionally, the first reactant includes one or more of the following: CaCl2*nH2O (n=0-12), calcium nitrate, calcium formate, and calcium propionate;
[0026] The first auxiliary sintering agent includes one or more of sodium carbonate, sodium bicarbonate, sodium fluoride, potassium fluoride, ammonium fluoride, and ammonium bifluoride.
[0027] Optionally, in S2, the mass mixing ratio of the powder to the first reactant should be 1:(1-10), the calcination temperature should be 300-600℃, and the calcination time should be 1-5h.
[0028] Optionally, in S4, the liquid-to-solid ratio of water immersion should be 1-50, the water immersion temperature should be 20-90°C, and the immersion time should be 1-5 hours.
[0029] Optionally, in S5, the mass ratio of the impregnation residue to the first auxiliary sintering agent should be 1:(2-10), the calcination temperature should be 160-800℃, and the calcination time should be 1-6h.
[0030] Optionally, in S6, the concentration of aluminum in the aluminate should be 0.2-2 mol / L, the acid in the acid leaching is any organic or inorganic acid, and the aluminate or acid is a leaching agent. The pH of the leaching agent should be between 0 and 4, the liquid-to-solid ratio should be between 3 and 20, the leaching temperature should be between 20 and 90°C, and the leaching time should be between 2 and 6 hours.
[0031] (III) Beneficial Effects
[0032] The beneficial effects of this invention are as follows: This invention provides a method for recovering aluminum fluoride from solid waste from aluminum electrolysis. The method involves mixing calcium salts with pulverized solid waste to obtain a powder mixture, which is then subjected to low-temperature calcination at 300℃-600℃. Simultaneously, the calcination process does not directly destroy all remaining fluoride ions in one step; instead, an intermediate product, calcium fluoride chloride, is generated under low-temperature conditions. This requires a lower temperature. Furthermore, it should be noted that in existing technologies, the reaction between solid waste and the reactant is carried out at high temperatures above 800℃. In other words, existing technologies directly generate calcium fluoride, which forms a solid precipitate that directly coats the outside of the calcined powder. This results in insufficient reaction of the powder coated with calcium fluoride. In contrast, this invention operates under low-temperature conditions and first generates an intermediate product, calcium fluoride chloride, in a molten state, allowing the powder to react from both the inside and outside, resulting in a more thorough and easier reaction. In comparison, the existing traditional process of high-temperature melting or leaching of strong acids and alkalis is less effective. The entire process does not involve strong acids or alkalis, the roasting raw materials are all neutral salts, there are almost no requirements for equipment, no dangerous gases are generated, the operation is safe, green and environmentally friendly, and the operating environment is also very safe. It avoids the defects of generating a large amount of waste residue and wastewater in traditional processes.
[0033] Following roasting and water leaching, the calcium chloride produced during roasting dissolves in water, and the free calcium ions readily and spontaneously combine with fluoride ions to form calcium fluoride, thus disrupting the structure of fluorides such as cryolite. After roasting and transformation with the addition of a first auxiliary sintering agent, the water-leached residue undergoes aluminum salt leaching. After pH adjustment, filter residue is obtained. Roasting this filter residue yields aluminum fluoride. The remaining leachate after pH adjustment can be purified and recycled for the next leaching process. This ensures the full recovery of aluminum fluoride. Furthermore, the roasting and transformation process uses only one calcium salt additive, saving costs and simplifying the raw material process. Attached Figure Description
[0034] Figure 1 This is a flowchart of a method for recovering aluminum fluoride from solid waste from aluminum electrolysis, as disclosed in this invention.
[0035] Figure 2 This is the XRD pattern of the aluminum fluoride product in Example 1 of this invention. Detailed Implementation
[0036] To better explain and facilitate understanding of the present invention, the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0037] This invention provides a method for recovering aluminum fluoride from solid waste generated by aluminum electrolysis. The method includes the following steps:
[0038] S1. Pulverize solid waste to make powder;
[0039] S2. The powder from S1 is mixed with the first reactant to obtain a powder mixture, wherein the first reactant is a calcium salt;
[0040] S3. The powder mixture in S2 is roasted at a certain temperature to obtain the first roasted residue, and the certain temperature range is between 300℃ and 600℃.
[0041] S4. The first roasted residue in S3 is soaked in water, and after soaking, it is filtered to obtain water-soaked residue and water-soaked liquid.
[0042] S5. Mix the water-impregnated residue from S4 with the first auxiliary sintering agent to obtain the second calcined residue;
[0043] S6. Add the second roasted residue from S5 to an aluminate leaching or acid leaching solution, filter, and obtain a leaching solution and a leaching residue.
[0044] S7. Adjust the pH of the leachate from S6 and filter it to obtain filter residue and filtrate. Calcine the obtained filter residue to obtain aluminum fluoride.
[0045] This invention discloses a method for recovering aluminum fluoride from solid waste from aluminum electrolysis. The method involves mixing calcium salts with pulverized solid waste to obtain a powder mixture, which is then subjected to low-temperature calcination at 300°C-600°C. During calcination, the remaining fluoride ions are not directly destroyed in one step; instead, an intermediate product, calcium fluoride chloride, is generated under low-temperature conditions. This requires a lower temperature. Furthermore, it should be noted that in existing technologies, the reaction between solid waste and reactants is carried out at high temperatures above 800°C. This means that calcium fluoride is directly generated in the existing technology, forming a solid precipitate that directly coats the outside of the calcined powder. Consequently, the powder coated with calcium fluoride cannot undergo sufficient reaction. In contrast, this invention, conducted under low-temperature conditions and first generating the intermediate product, calcium fluoride chloride, in a molten state, allows the powder to react from both the inside and outside, resulting in a more thorough and easier reaction. In comparison, the existing traditional process of high-temperature melting or leaching of strong acids and alkalis is less effective. The entire process does not involve strong acids or alkalis, the roasting raw materials are all neutral salts, there are almost no requirements for equipment, no dangerous gases are generated, the operation is safe, green and environmentally friendly, and the operating environment is also very safe. It avoids the defects of generating a large amount of waste residue and wastewater in traditional processes.
[0046] Following roasting and water leaching, the calcium chloride produced during roasting dissolves in water, and the free calcium ions readily and spontaneously combine with fluoride ions to form calcium fluoride, thus disrupting the structure of fluorides such as cryolite. After roasting and transformation with the addition of a first auxiliary sintering agent, the water-leached residue undergoes aluminum salt leaching. After pH adjustment, filter residue is obtained. Roasting this filter residue yields aluminum fluoride. The remaining leachate after pH adjustment can be purified and recycled for the next leaching process. This ensures the full recovery of aluminum fluoride. Furthermore, the roasting and transformation process uses only one calcium salt additive, saving costs and simplifying the raw material process.
[0047] Furthermore, existing physical adsorption methods are only suitable for very low concentrations of fluoride in the air, providing only slight adsorption. For actual production and the treatment of fluoride-containing waste, the fluoride concentration is always very high, making large-scale processing impossible with existing physical adsorption methods. In contrast, this embodiment is suitable for treating high concentrations of fluoride, exhibiting strong fluoride adsorption capacity, excellent adsorption effect, and good fluoride recovery.
[0048] Furthermore, the leaching residue obtained in S6 is further fed into the second roasted residue for leaching. Recycling this residue for the next leaching process allows for more efficient utilization of the fluorine.
[0049] Further, in S7, the obtained filtrate is recycled to S6.
[0050] Furthermore, it also includes selective lithium extraction based on the lithium-ion content in the aqueous leachate obtained in S4. If the aqueous leachate contains lithium ions, calcium removal is performed first, followed by evaporation to extract lithium salts. Specifically, if the raw material contains lithium, the aqueous leachate is decalcified before lithium extraction to prepare lithium carbonate and co-produce calcium carbonate. Lithium extraction can be performed simultaneously, co-producing calcium carbonate and lithium carbonate. This avoids the defects of traditional processes involving high-temperature melting or leaching with strong acids and alkalis, which generate large amounts of waste residue and wastewater.
[0051] Furthermore, the solid waste mentioned in S1 includes any one of the following: waste aluminum electrolyte, furnace bottom sediment, and anode covering material, wherein each element is predominantly Na3AlF6, Na5Al3F6, etc. 14 Li₂NaAlF₆, Li₃Na₃AlF₆ 12 It exists in one or more forms of Na2MgAlF7 and LiCaAlF7, with a Li content of 0-3%. In other words, this invention is applicable to the treatment of most solid waste from aluminum plants, not just single electrolyte waste, thus having wider applicability. Furthermore, the process does not only recover lithium but also effectively recovers almost all valuable elements in the waste, such as aluminum, calcium, sodium, and potassium, resulting in stronger industrialization prospects.
[0052] Furthermore, the first reactant includes one or more of the following: CaCl2*nH2O (n=0-12), calcium nitrate, calcium formate, and calcium propionate. The first reactant is low in cost, and since only one calcium salt additive is used in the roasting conversion process, it saves costs and simplifies the raw materials.
[0053] The first auxiliary sintering agent includes one or more of sodium carbonate, sodium bicarbonate, sodium fluoride, potassium fluoride, ammonium fluoride, and ammonium bifluoride. These are readily available and inexpensive.
[0054] Further, in S2, the mass mixing ratio of the powder to the first reactant should be 1:(1-10), preferably 1:1-1:3. The calcination temperature should be 300-600℃, preferably 450-550℃, and the calcination time should be 1-5h, preferably 2-3h.
[0055] Furthermore, in S4, the liquid-to-solid ratio of water immersion should be 1-50, the water immersion temperature should be 20-90°C, and the immersion time should be 1-5 hours, preferably 2-3 hours.
[0056] Furthermore, in S5, the mass ratio of the impregnation residue to the first auxiliary sintering agent should be 1:(2-10), the calcination temperature should be 160-800℃, preferably 200-600℃, and the calcination time should be 1-6h, preferably 2-4h.
[0057] Further, in S6, the aluminum concentration in the aluminate should be 0.2-2 mol / L, preferably 1-1.8 mol / L. The acid in the acid leaching is any organic or inorganic acid, and both the aluminate and the acid are leaching agents. The pH of the leaching agent should be between 0 and 4, and the liquid-to-solid ratio should be between 3 and 20, preferably 5-10. The leaching temperature is 20-90℃, preferably 30-60℃. The leaching time is 2-6 hours.
[0058] Furthermore, in step S7, the pH can be adjusted using sodium hydroxide, potassium hydroxide, or ammonia, with the final pH maintained between 5 and 13.
[0059] Furthermore, in S7, the calcination temperature should be 300-600℃, preferably 400-550℃, the calcination time should be 3-5h, and the mixing ratio should be 1:1-5.
[0060] To better understand the above technical solutions, exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the drawings, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that the present invention can be understood more clearly and thoroughly, and that the scope of the present invention can be fully conveyed to those skilled in the art.
[0061] It should be noted that the drying in the following embodiments of the present invention is carried out at 90°C for 12 hours. Evaporation is carried out at 100°C until a solid precipitates.
[0062] Example 1:
[0063] S1. First, waste aluminum electrolyte (Na: 24.79wt%, Al: 14.40wt%, F: 54.19wt%, K: 2.50wt%, Ca: 1.06wt%) from an aluminum plant in Liaoning Province is crushed and then sieved to separate the particles with a particle size ≤200 mesh, thus producing powder. It should be noted that the purpose of crushing the waste electrolyte is to ensure a more complete reaction. Sieving to a particle size of ≤200 mesh facilitates subsequent reactions; finer particles allow for more complete reaction. Powder with a particle size greater than 200 mesh is returned to the pulverizing device for further processing.
[0064] S2. Weigh 40g of anhydrous calcium chloride (first reactant) and 20g of electrolyte (mass ratio 2:1) and mix them evenly to obtain a powder mixture.
[0065] S3. The powder mixture from S2 is calcined at 550°C for 2 hours to obtain the first calcined residue.
[0066] S4. The first calcined residue from S3 is subjected to water leaching at a liquid-to-solid ratio of 50, a water leaching temperature of 80°C, and a water leaching time of 2 hours. After leaching, the residue is filtered and dried to obtain the water-leached residue. It should be noted that...
[0067] The aqueous extract obtained in S4, after calcium removal and evaporation, yields a salt primarily composed of sodium chloride. Of course, different salts can be obtained depending on the chosen reactants.
[0068] S5. The water-leached residue from S4 is mixed with sodium carbonate (first auxiliary sintering agent) at a mass ratio of 1:3 and then calcined at 550°C for 2 hours to obtain the second calcined residue.
[0069] S6. Using an aluminum salt solution with pH=2.00 and an aluminum concentration of 1.2 mol / L, the second roasted slag was leached at 35°C for 4 hours, and the leachate and leaching slag were obtained by filtration.
[0070] S7. Add 5% sodium hydroxide solution to the leachate to adjust the pH to 5, and filter to obtain filter residue and filtrate. Dry the obtained filter residue and then calcine it at 500℃ for 3 hours to obtain aluminum fluoride. The purity of aluminum fluoride is 99.18%, and the recovery rate of aluminum fluoride is 99.63%.
[0071] Example 2:
[0072] The method is the same as in Example 1, except that:
[0073] The powder used in S1 is the sediment from the waste furnace bottom of an aluminum plant.
[0074] The mass ratio of the first reactant to the powder used in S2 is 4:1, the calcination temperature of the powder mixture is 600℃, and the calcination time is 4h.
[0075] During the water immersion process of the first roasted slag in S4, the liquid-to-solid ratio is 10, the water immersion temperature is 20℃, and the water immersion time is 1.
[0076] The first auxiliary sintering agent used in S5 is potassium fluoride, with a mixing ratio of 1:5, and is calcined at 450℃ for 1 hour.
[0077] The aluminum salt leaching process in S6 uses an aluminum salt solution with pH=1 and 1.5M, and leaches at 40℃ for 3 hours.
[0078] In S7, 10% ammonia solution was used to adjust the pH, with a final pH of 6.00. The calcination temperature for preparing aluminum fluoride was 450℃, and the calcination time was 4 hours. The purity of the aluminum fluoride was 99.02%, and the recovery rate was 99.33%.
[0079] Example 3:
[0080] The method is the same as in Example 1, except that:
[0081] The powder used in S1 is waste anode covering material from an aluminum plant.
[0082] The mass ratio of the first reactant to the powder used in S2 is 1:1, the calcination temperature is 400℃, and the calcination time is 1h.
[0083] During the S4 water immersion process, the liquid-to-solid ratio is 20, the water immersion temperature is 90℃, and the water immersion time is 3 hours.
[0084] The purity of aluminum fluoride was 99.18%, and the recovery rate was 99.08%.
[0085] Example 4:
[0086] The method is the same as in Example 1, except that:
[0087] The mass ratio of the first reactant to the electrolyte used in S2 is 10:1, the calcination temperature is 300℃, and the time is 5h.
[0088] During the S4 water immersion process, the liquid-to-solid ratio is 30, the water immersion temperature is 50℃, and the water immersion time is 5 hours.
[0089] In S7, the calcination temperature for preparing aluminum fluoride is 300℃ and the calcination time is 5h.
[0090] The purity of aluminum fluoride is 99.65%, and the recovery rate of aluminum fluoride is 98.75%.
[0091] Example 5:
[0092] The method is the same as in Example 1, except that:
[0093] The mass ratio of the first reactant to the electrolyte used in S2 is 6:1, the calcination temperature is 400℃, and the calcination time is 2h.
[0094] During the S4 water immersion process, the liquid-to-solid ratio was 40, the water immersion temperature was 70℃, and the water immersion time was 2 hours.
[0095] In S7, the calcination temperature for preparing aluminum fluoride is 450℃ and the calcination time is 3h.
[0096] The purity of aluminum fluoride is 99.05%, and the recovery rate of aluminum fluoride is 99.27%.
[0097] Example 6:
[0098] The method is the same as in Example 1, except that: |
[0099] The mass ratio of the first reactant to the electrolyte used in S2 is 7:1.
[0100] During the S4 water immersion process, the liquid-to-solid ratio is 15, the water immersion temperature is 60℃, and the water immersion time is 2 hours.
[0101] The purity of aluminum fluoride is 99.12%, and the recovery rate of aluminum fluoride is 99.40%.
[0102] Example 7:
[0103] The method is the same as in Example 1, except that: |
[0104] The mass ratio of the first reactant to the electrolyte used in S2 is 8:1.
[0105] During the S4 water immersion process, the liquid-to-solid ratio is 30, the water immersion temperature is 50℃, and the water immersion time is 3 hours.
[0106] The purity of aluminum fluoride is 99.36%, and the recovery rate of aluminum fluoride is 99.25%.
[0107] Example 8:
[0108] The mass ratio of the first reactant to the electrolyte used in S2 is 4:1.
[0109] During the S4 water immersion process, the liquid-to-solid ratio was 35, the water immersion temperature was 30℃, and the water immersion time was 4 hours.
[0110] The S6 acid leaching process uses a 1.5M nitric acid solution with pH=1, and the leaching is carried out at 40℃ for 3 hours.
[0111] The purity of aluminum fluoride is 98.95%, and the recovery rate of aluminum fluoride is 99.67%.
[0112] Comparative Example 1:
[0113] S1. First, waste aluminum electrolyte (Na: 24.79wt%, Al: 14.40wt%, F: 54.19wt%, K: 2.50wt%, Ca: 1.06wt%) from an aluminum plant in Liaoning Province is crushed and then sieved to separate the particles with a particle size ≤200 mesh, thus preparing powder. It should be noted that the purpose of crushing the waste cathode is to ensure a more complete reaction. Sieving to a particle size of ≤200 mesh facilitates subsequent reactions; finer particles allow for more complete reaction. Powder with a particle size greater than 200 mesh is returned to the powder preparation unit for further processing.
[0114] S2. Weigh 40g of anhydrous calcium chloride (first reactant) and 20g of electrolyte (mass ratio 2:1) and mix them evenly to obtain a powder mixture.
[0115] S3. The powder mixture from S2 is calcined at 800°C for 2 hours to obtain the first calcined residue.
[0116] S4. The first roasted residue from S3 is subjected to water leaching at a liquid-to-solid ratio of 50, a water leaching temperature of 80°C, and a water leaching time of 2 hours. After leaching, the residue is filtered and dried to obtain the water-leached residue. It should be noted that the water leaching solution obtained in S4 is evaporated after calcium removal to obtain a salt mainly composed of sodium chloride.
[0117] S5. The water-leached residue from S4 is mixed with sodium carbonate (first auxiliary sintering agent) at a mass ratio of 1:3 and then calcined at 550°C for 2 hours to obtain the second calcined residue.
[0118] S6. Using an aluminum salt solution with pH=2.00 and an aluminum concentration of 1.2 mol / L, the second roasted slag was leached at 35°C for 4 hours, and the leachate and leaching slag were obtained by filtration.
[0119] S7. Add 5% sodium hydroxide solution to the leachate to adjust the pH to 5, and filter to obtain filter residue and filtrate. Dry the obtained filter residue and then calcine it at 500℃ for 3 hours to obtain aluminum fluoride. The purity of aluminum fluoride is 97.96%, and the recovery rate of aluminum fluoride is 93.18%.
[0120] Comparative Example 2:
[0121] S1. First, waste aluminum electrolyte (Na: 24.79wt%, Al: 14.40wt%, F: 54.19wt%, K: 2.50wt%, Ca: 1.06wt%) from an aluminum plant in Liaoning Province is crushed and then sieved to separate the particles with a particle size ≤200 mesh, thus preparing powder. It should be noted that the purpose of crushing the waste cathode is to ensure a more complete reaction. Sieving to a particle size of ≤200 mesh facilitates subsequent reactions; finer particles allow for more complete reaction. Powder with a particle size greater than 200 mesh is returned to the powder preparation unit for further processing.
[0122] S2. Weigh 40g of anhydrous calcium chloride (first reactant) and 20g of electrolyte (mass ratio 2:1) and mix them evenly to obtain a powder mixture.
[0123] S3. The powder mixture in S2 is calcined at 200°C for 2 hours to obtain the first calcined residue.
[0124] S4. The first roasted residue from S3 is subjected to water leaching at a liquid-to-solid ratio of 50, a water leaching temperature of 80°C, and a water leaching time of 2 hours. After leaching, the residue is filtered and dried to obtain the water-leached residue. It should be noted that the water leaching solution obtained in S4 is evaporated after calcium removal to obtain a salt mainly composed of sodium chloride.
[0125] S5. The water-leached residue from S4 is mixed with sodium carbonate (first auxiliary sintering agent) at a mass ratio of 1:3 and then calcined at 550°C for 2 hours to obtain the second calcined residue.
[0126] S6. Using an aluminum salt solution with pH=2.00 and an aluminum concentration of 1.2 mol / L, the second roasted slag was leached at 35°C for 4 hours, and the leachate and leaching slag were obtained by filtration.
[0127] S7. Add 5% sodium hydroxide solution to the leachate to adjust the pH to 5, and filter to obtain filter residue and filtrate. Dry the obtained filter residue and then calcine it at 500℃ for 3 hours to obtain aluminum fluoride. The purity of aluminum fluoride is 94.68%, and the recovery rate of aluminum fluoride is 90.63%.
[0128] According to the above embodiments, the aluminum fluoride recovery rate of Example 8 is the highest. Specifically, the mass ratio of the first reactant to the electrolyte is 4:1 to obtain a powder mixture. The powder mixture is calcined at 550°C for 2 hours to obtain the first calcined residue. The first calcined residue is then water-leached at a liquid-to-solid ratio of 35, a water-leaching temperature of 30°C, and a water-leaching time of 4 hours. The water-leached residue from step S4 is then mixed with sodium carbonate (the first auxiliary sintering agent) at a mass ratio of 1:3 and calcined at 550°C for 2 hours to obtain the second calcined residue. The second calcined residue is then acid-leached using a 1.5M nitric acid solution with a pH of 1 and an aluminum salt solution with an aluminum concentration of 1.2 mol / L at 40°C for 3 hours. The residue is then filtered to obtain a leachate and a leachate residue. Step S7: A 5% sodium hydroxide solution is added to the leachate to adjust the pH to 5, and the solution is filtered to obtain a filter residue and a filtrate. The obtained filter residue was dried and then calcined at 500°C for 3 hours to obtain aluminum fluoride. Under these conditions, the concentration and recovery rate of aluminum fluoride were optimal.
[0129] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for recovering aluminum fluoride from solid waste from aluminum electrolysis, characterized in that: The method includes the following steps: S1. Pulverize solid waste to make powder; The solid waste mentioned in S1 includes any one of the following: waste aluminum electrolyte, furnace bottom sediment, and anode covering material, wherein each element is predominantly Na3AlF6 or Na5Al3F6. 14 Li₂NaAlF₆, Li₃Na₃AlF₆ 12 It exists in one or more forms of Na2MgAlF7 and LiCaAlF7, with a Li content of 0-3%; S2. The powder from S1 is mixed with the first reactant to obtain a powder mixture, wherein the first reactant is CaCl2·nH2O, n=0-12; In S2, the mass mixing ratio of the powder to the first reactant is 1:(1-10). S3. The powder mixture in S2 is roasted at a certain temperature to obtain the first roasted residue, and the certain temperature range is between 300℃ and 600℃. S4. The first roasted residue in S3 is soaked in water, and after soaking, it is filtered to obtain water-soaked residue and water-soaked liquid. S5. The water-impregnated residue from S4 is mixed with the first auxiliary sintering agent to obtain the second calcined residue. The first auxiliary sintering agent includes ammonium fluoride or ammonium bifluoride. S6. Add the second roasted residue from S5 to the leaching agent for leaching, filter, and obtain leaching solution and leaching residue. The leaching agent is an aluminate solution or acid. S7. Adjust the pH of the leachate from S6 and filter it to obtain filter residue and filtrate. Calcine the obtained filter residue to obtain aluminum fluoride. The pH is adjusted with ammonia water, and the final pH is maintained between 5 and 13.
2. The method for recovering aluminum fluoride from solid waste from aluminum electrolysis as described in claim 1, characterized in that: The leaching residue obtained in S6 is then fed into the second roasted residue for leaching.
3. The method for recovering aluminum fluoride from solid waste from aluminum electrolysis as described in claim 1, characterized in that: In S7, the obtained filtrate is recycled to S6.
4. The method for recovering aluminum fluoride from solid waste from aluminum electrolysis as described in any one of claims 1-3, characterized in that: If the aqueous extract obtained in S4 contains lithium ions, calcium removal is performed first, followed by evaporation to extract lithium salt.
5. The method for recovering aluminum fluoride from solid waste from aluminum electrolysis as described in claim 1, characterized in that: The roasting time in S3 is 1-5 hours.
6. The method for recovering aluminum fluoride from solid waste from aluminum electrolysis as described in claim 1, characterized in that: In S4, the liquid-to-solid ratio for water immersion is 1-50, the water immersion temperature is 20-90℃, and the immersion time is 1-5h.
7. The method for recovering aluminum fluoride from solid waste from aluminum electrolysis as described in claim 1, characterized in that: In S5, the mass ratio of the water-impregnated residue to the first auxiliary sintering agent is 1:(2-10), the calcination temperature is 160-800℃, and the calcination time is 1-6h.
8. The method for recovering aluminum fluoride from solid waste from aluminum electrolysis as described in claim 1, characterized in that: In the aluminate solution in S6, the aluminum concentration is 0.2-2 mol / L, the acid is an organic acid or an inorganic acid, the pH of the leaching agent is 0-4, the liquid-to-solid ratio is 3-20, the leaching temperature is 20-90℃, and the leaching time is 2-6 h.
Citation Information
Patent Citations
Resource treatment method for lithium-rich aluminum electrolyte
CN110240182A
Comprehensive recovery method of waste electrolyte containing lithium and aluminum
CN114438329A
Resourceful treatment method for waste electrolyte containing lithium and aluminum
CN115216630A
Lithium extraction method of lithium-containing waste aluminum electrolyte
CN115198111A
Method for complete resource utilization of waste aluminum electrolysis anode covering material or / and furnace bottom sediment
CN115872427A