A PP coffee machine shell material containing PCR and preparation method thereof

By combining polypropylene and ABS resin with recycled plastic and adding tougheners, etc., a stable blend structure is formed, which solves the problem of aging of the recycled plastic structure, improves the heat resistance and impact resistance of the coffee machine shell material, and extends the Extended service life, achieving higher environmental protection and performance improvement.

CN118126449BActive Publication Date: 2024-10-01JIAN GUOHENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410261619.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-07
Publication Date
2024-10-01
Estimated Expiration
2044-03-07

AI Technical Summary

Technical Problem

When recycled plastics are used to prepare coffee machine casing materials, structural aging leads to a reduction in strength, toughness, impact resistance, hardness and other properties. The service life is short, making it difficult to meet the needs of long-term use.

Method used

The PP coffee machine shell material containing PCR is used. By combining polypropylene, ABS resin and recycled plastic, toughening agents, antioxidants, reinforcing fillers and compatibilizers are added to form a stable blend structure and improve the heat resistance of the material. properties, impact resistance and aging resistance, extending service life.

Benefits of technology

Significantly improve the strength, impact resistance, wear resistance and aging resistance of the coffee machine shell material, extend the service life, reduce the waste of waste plastics, and improve environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004731094510000061
    Figure BDA0004731094510000061
  • Figure BDA0004731094510000071
    Figure BDA0004731094510000071
  • Figure BDA0004731094510000072
    Figure BDA0004731094510000072
Patent Text Reader

Abstract

The present application belongs to the technical field of coffee machine shell material processing, in particular, a PP coffee machine shell material containing PCR and a preparation method thereof, which is prepared from the following raw materials in weight percentage: PCR 35-52%, PP 28-35%, toughening agent 1-3%, antioxidant 0.5-1%, reinforcing filler 5-10%, ABS resin 6-10%, compatibilizer 2-3% and dispersant 3-6%. In the present application, by combining polypropylene, ABS resin, reinforcing filler and recycled plastic, the problems of poor strength, toughness, impact resistance, hardness and aging resistance of recycled plastic can be effectively improved, so that the coffee machine shell material has good strength, toughness, impact resistance, hardness and aging resistance, is not easy to be damaged, and can be used for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of coffee machine shell material processing, and in particular to a PP coffee machine shell material containing PCR and a preparation method thereof. Background Art

[0002] The amount of waste plastics used is large, and a large amount of waste plastics are generated. In the past, incineration and landfill were usually used to deal with waste polypropylene, which caused great pollution to the environment. With the popularization of environmental protection policies, people no longer use incineration and landfill to deal with waste plastics. Instead, they modify waste plastics through chemical or physical methods so that waste plastics can be reused. PCR plastic is a recycled plastic, and its full name is Post-Consumer Recycled material, which means "post-consumer recycled material". PCR plastic is made from plastic products used by consumers, such as lunch boxes, shampoo bottles, mineral water bottles, etc., which are collected, cleaned, processed and other steps to make plastic raw materials. The use of PCR plastic can reduce the consumption of new plastics, reduce carbon dioxide emissions, and protect environmental resources.

[0003] As the number of people who love coffee increases, coffee machines have gradually become one of the most common household appliances, and the number of people using them has greatly increased. The structure of a coffee machine usually includes a water tank, a coffee powder bin, a filter, a heating element, and a shell. The shell of the coffee machine is used to protect the internal parts of the coffee machine and beautify the appearance. By using recycled plastic to prepare the shell material of the coffee machine, the pollution of waste plastics can be reduced, and the utilization rate of waste plastics can be improved.

[0004] However, the structural aging of recycled plastics causes their strength, toughness, impact resistance, hardness, shrinkage rate, etc. to decrease to varying degrees. When used to make coffee machine shell materials, they are easily damaged, have a short service life, and need to be replaced in a timely manner. Summary of the invention

[0005] In order to improve the problem of short service life of coffee machine shell materials prepared due to aging of recycled plastic structures, the present application provides a PP coffee machine shell material containing PCR and a preparation method thereof.

[0006] In the first aspect, the present application provides a PP coffee machine shell material containing PCR, which adopts the following technical solution:

[0007] A PP coffee machine shell material containing PCR is prepared from the following raw materials in percentage by weight:

[0008] PCR 35-52%

[0009] PP 28-35%

[0010] Toughener 1-3%

[0011] Antioxidants 0.5-1%

[0012] Reinforcement filler 5-10%

[0013] ABS resin 6-10%

[0014] Compatibilizer 2-3%

[0015] Dispersant 3-6%.

[0016] By adopting the above technical solution, the prepared coffee machine shell material has good strength, toughness, impact resistance, hardness and aging resistance, is not easy to damage, and can be used for a long time. The main material of the present application is mainly recycled plastic, which can reduce the waste of waste plastic and improve environmental protection.

[0017] In this application, PP is polypropylene. By combining polypropylene, ABS resin and recycled plastic, the problems of poor strength, toughness, impact resistance, wear resistance, hardness and aging resistance of recycled plastic can be effectively improved. Polypropylene has good properties such as strength, wear resistance, hardness and rigidity, which can make up for the problems of poor strength, wear resistance, hardness and rigidity of recycled plastic, thereby improving the strength, heat resistance, hardness and rigidity of the coffee shell and reducing the possibility of easy damage to the coffee machine shell. The coffee machine is heated during use, and heating will accelerate the aging of recycled plastics. ABS resin has good heat resistance, toughness and aging resistance. Adding a small amount of ABS resin can further improve the heat resistance, toughness and aging resistance of the coffee machine shell material and extend the service life of the coffee machine shell material. In this application, by adding polypropylene and ABS resin, the heat resistance and mechanical properties of the coffee machine shell material are improved, the aging of recycled plastics is slowed down, and the service life of the coffee machine shell material is extended.

[0018] The compatibility between polypropylene, ABS resin and recycled plastic is poor. By using compatibilizers to increase the compatibility of the three, the adhesion of the three is increased, a stable blending structure is formed, and the organizational structure of the mixed system is improved. The components are mixed more evenly and the organizational structure is more solid. During the molding process, no decomposition occurs and no reaction occurs with other materials. After molding, it has good weather resistance, high stability, and greatly extended service life.

[0019] The reinforcing filler works synergistically with polypropylene and ABS resin to further improve the hardness, strength, impact resistance and wear resistance of the coffee machine shell material, making it less prone to damage during use and having a long service life.

[0020] Preferably, the toughening agent is at least one of dibutyl phthalate, di-n-hexyl azelate, dimethyl sebacate, di-n-butyl sebacate and 2-ethylhexyl adipate. The toughening agent increases the toughness and ductility of the recycled plastic, thereby improving the impact resistance and heat resistance of the coffee machine shell material.

[0021] Preferably, the dispersant is at least one of stearic acid, zinc stearate, calcium stearate, polyethylene wax, oxidized polyethylene wax, and ethylene bis stearamide. The dispersant is conducive to fully mixing the recycled plastic, polypropylene, ABS resin and reinforcing filler to form a coffee machine shell material with a stable and uniform structure.

[0022] Preferably, the antioxidant is antioxidant 168, antioxidant 1520, antioxidant 1790, antioxidant 2246 or antioxidant 1076. By adding the above oxidants, the antioxidant property of the coffee machine shell material is improved, the oxidation rate of the coffee machine shell material is slowed down, and the service life of the coffee machine shell material is extended.

[0023] Preferably, pretreatment is required before use in PCR, and the pretreatment steps are as follows:

[0024] 1) Stir water and starch at 60-80° C. until transparent, add an acid starch modifier, continue stirring for 1-2 hours, add an alkaline solution, adjust the pH to 6.5-7.5, dry, and crush to obtain modified starch;

[0025] 2) drying the PCR, mixing the dried PCR, the silane coupling agent and the modified starch, and then extruding and granulating the PCR through a twin-screw extruder to obtain the prefabricated PCR.

[0026] The anti-aging performance, mechanical properties and processing properties of PCR are all poor. By using modified starch and silane coupling agent to modify PCR, one is to improve the compatibility of PCR with polypropylene and ABS resin, and further form a stable blending structure, so that the structure of the coffee machine shell material is strong and durable, not easy to damage. The second is to improve the mechanical properties of recycled plastics such as strength, impact resistance and wear resistance. In this application, water and starch are stirred to make the starch gelatinized, and then an acid starch modifier is added to stir, so that the hydrogen bond force between starch molecules is weakened, and the compatibility of modified starch and PCR is improved, thereby improving the mechanical properties of recycled plastics. In order to further improve the bonding force between modified starch and recycled plastics, in order to improve the anti-aging performance and mechanical properties of PCR, PCR, silane coupling agent and modified starch are mixed and granulated in this application, so that the wear resistance, impact resistance and wear resistance of the coffee machine shell material are greatly improved, and the service life of the coffee machine shell material is further extended.

[0027] Preferably, the weight portions of raw materials used to prepare the PCR are as follows:

[0028] 20-30 parts starch

[0029] 40-50 parts water

[0030] 3-6 parts of acid starch modifier

[0031] 4-8 parts alkaline solution

[0032] PCR 35-45 copies

[0033] Silane coupling agent 2-5 parts.

[0034] By adopting the above technical scheme, the amount of raw materials used in the preparation of PCR is optimized, and the processing performance, aging resistance and mechanical properties of PCR are further improved, so that the coffee machine shell material has a firm structure, good impact resistance, wear resistance and durability, and is not easily damaged after long-term use.

[0035] Preferably, the starch is at least one of corn starch, sweet potato starch, wheat starch, tapioca starch and pea starch.

[0036] Preferably, the PCR is at least one of consumer recycled polypropylene, consumer recycled polyamide, consumer recycled polycarbonate or consumer recycled polyethylene.

[0037] By using the above-mentioned PCR combination, the pollution of waste plastics can be reduced. At the same time, by using different recycled plastics in combination, the utilization rate of waste plastics can be improved, and the strength, impact resistance, wear resistance and aging resistance of the coffee machine shell material can be further improved.

[0038] Preferably, the acid starch modifier is at least one of formic acid, adipic acid, succinic acid, malic acid, tartaric acid, lauric acid, stearic acid, and oleic acid.

[0039] The above acid starch modifiers will form hydrogen bonds with starch molecules to weaken the hydrogen bonding between starch molecules, improve the compatibility of starch and PCR, and thus improve the mechanical properties of recycled plastics.

[0040] Preferably, the PP has a melt index of 20-40 g / 10 min at 230°C / 2.16 kg and a density of ≤0.93 g / cm 3 , simply supported beam notch impact ≥7KJ / m 2 .

[0041] By adopting the above technical solution, the parameters of polypropylene are optimized, the problems of poor strength, toughness, impact resistance, hardness and aging resistance of recycled plastics are further improved, and the strength, impact resistance, wear resistance and aging resistance of the coffee machine shell material are improved.

[0042] Preferably, the content of butadiene in the ABS resin is 5-30%, the content of styrene is 40-60%, and the content of acrylonitrile is 30-35%.

[0043] By adopting the above technical solution, the parameters of ABS resin are optimized, and the heat resistance of ABS resin is further improved by increasing or decreasing the content of styrene, so that the coffee machine shell material has good heat resistance, strength, impact resistance and wear resistance.

[0044] Preferably, the reinforcing filler is at least one of silicon dioxide, glass fiber, calcium carbonate, talcum powder, titanium dioxide, quartz stone, ceramic powder, aluminum oxide and barium sulfate.

[0045] By adopting the above technical solution, the mechanical properties such as strength, hardness and wear resistance of the coffee machine shell material are further improved, and the service life of the coffee machine shell material is extended.

[0046] Preferably, the compatibilizer is at least one of polyolefin long chain grafted maleic anhydride, glycidyl methacrylate, styrene grafted maleic anhydride and ABS grafted maleic anhydride.

[0047] By adopting the above technical scheme, the compatibility of recycled plastic, polypropylene and ABS resin is improved, so that the three can be fully compatible and mixed, which is beneficial to the processing of coffee machine shell materials, and thus obtain a coffee machine shell material with good strength, impact resistance, wear resistance and aging resistance.

[0048] In a second aspect, the present application provides a method for preparing a PP coffee machine shell material containing PCR, using the following technical solution:

[0049] A method for preparing a PP coffee machine shell material containing PCR, comprising the following preparation steps:

[0050] S1, putting PCR, PP, ABS resin, reinforcing filler, toughening agent, antioxidant, compatibilizer and dispersant into a high-speed mixer and mixing at high speed to obtain a mixture;

[0051] S2. The mixture is extruded and granulated through a twin-screw extruder, the extruder barrel temperature is 200-230° C., the die head temperature is 240-250° C., the main engine speed is 200-250 r / min, and the feeding speed is 10-25 r / min to obtain master batches, and then the master batches are injection molded to obtain PP coffee machine shell materials containing PCR.

[0052] By adopting the above technical solution, the various components can be fully and evenly mixed, further improving the hardness, strength, impact resistance, heat resistance and wear resistance of the coffee machine shell material, slowing down the aging of recycled plastics, and extending the service life of the coffee machine shell material.

[0053] In summary, this application has the following beneficial effects:

[0054] 1. The present application prepares a coffee machine shell material by mixing PCR, PP, ABS resin, toughening agent, antioxidant, reinforcing filler, compatibilizer and dispersant in a specific ratio, wherein the properties of good strength, good wear resistance and weather resistance of polypropylene are utilized, and the good heat resistance, toughness and aging resistance of ABS resin are utilized to improve the strength, heat resistance, hardness and stiffness of recycled plastics, thereby improving the strength, heat resistance, hardness and stiffness of the coffee shell, slowing down the aging of recycled plastics, and extending the service life of the coffee machine shell material. The compatibility between polypropylene, ABS resin and recycled plastic is increased by a compatibilizer, so that the components are mixed more evenly, thereby forming a stable blending structure, thereby improving the impact resistance, strength, wear resistance and aging resistance of the coffee machine shell material.

[0055] 3. The present application heats and stirs water and starch to gelatinize the starch, and then gelatinizes the starch with a silane coupling agent and PCR to prepare prefabricated PCR, thereby improving the anti-aging performance, mechanical properties and processing performance of PCR, thereby greatly improving the wear resistance, impact resistance and durability of the coffee machine shell material, and improving durability. DETAILED DESCRIPTION

[0056] Example

[0057] Example 1

[0058] A PP coffee machine shell material containing PCR is prepared by the following preparation method:

[0059] S1, 350g of PCR, 350g of PP, 100g of ABS resin, 100g of reinforcing filler (silicon dioxide), 30g of toughening agent (dibutyl phthalate), 10g of antioxidant (antioxidant 168), 30g of compatibilizer (glycidyl methacrylate) and 30g of dispersant (stearic acid) were put into a high-speed mixer and mixed at high speed to obtain a mixture;

[0060] S2. The mixture is extruded and granulated through a twin-screw extruder. The extruder barrel temperature is 200° C., the die temperature is 240° C., the main engine speed is 200 r / min, and the feeding speed is 10 r / min to obtain master batches. The master batches are then injection molded to obtain PP coffee machine shell materials containing PCR.

[0061] PCR is consumer recycled polypropylene, with a melt index of 10g / 10min at 230℃ / 2.16kg and a density of 0.91g / cm 3 , simply supported beam notch impact is 5KJ / m 2 .

[0062] The melt index of PP at 230℃ / 2.16kg is 20g / 10min and the density is 0.93g / cm 3 , simply supported beam notch impact 7KJ / m 2 .

[0063] The butadiene content of ABS resin is 5%, the styrene content is 40%, the acrylonitrile content is 30%, and the molecular weight is 5000.

[0064] The difference between Example 2-3 and Example 1 is that the types of raw materials, amounts and experimental parameters for preparing the PP coffee machine shell material containing PCR are partially different. The specific differences are shown in Table 1:

[0065] Table 1 Raw material types, amounts and experimental parameters for preparing PP coffee machine shell materials containing PCR in Examples 1-3

[0066]

[0067]

[0068] The density of consumer recycled polyamide is 1.14 g / cm 3 , glass transition temperature is 45°C and tensile strength is 50MPa.

[0069] The glass transition temperature of recycled polycarbonate is 45°C and the density is 1.2g / cm 3 , simply supported beam notch impact is 44KJ / m 2 .

[0070] The grafting rate of ABS grafted with maleic anhydride is 1.2%.

[0071] The grafting rate of maleic anhydride grafted onto polypropylene was 0.9%.

[0072] Example 4

[0073] A PP coffee machine shell material containing PCR. The difference between this embodiment and embodiment 1 is that the PCR needs to be pretreated before use. The pretreatment steps are as follows:

[0074] 1) Stir 400 g of water and 200 g of starch at 60° C. until a transparent state is obtained, then add 30 g of an acid starch modifier (tartaric acid), continue stirring for 1 h, then add 40 g of an alkaline solution (15% sodium carbonate solution by mass), adjust the pH to 6.5, dry, and crush to obtain modified starch;

[0075] 2) 350 g of PCR was dried, and then the dried PCR, 20 g of silane coupling agent (vinyl triethoxysilane) and modified starch were mixed, and then extruded and granulated by a twin-screw extruder to obtain prefabricated PCR.

[0076] The difference between Example 5-6 and Example 4 is that the types of raw materials, amounts and experimental parameters for preparing prefabricated PCR are partially different. The specific differences are shown in Table 2:

[0077] Table 2 Types of raw materials, amounts and experimental parameters for preparing prefabricated PCR in Examples 4-6

[0078]

[0079]

[0080] The melt index of recycled polypropylene at 230℃ / 2.16kg is 10g / 10min and the density is 0.91g / cm 3 , simply supported beam notch impact is 5KJ / m 2 .

[0081] Example 7

[0082] A PP coffee machine shell material containing PCR. The difference between this embodiment and Example 1 is that PCR is 150g of consumer recycled polypropylene and 100g of consumer recycled polyamide, and the types, amounts and experimental parameters of other raw materials are consistent with those in Example 1.

[0083] Example 8

[0084] A PP coffee machine shell material containing PCR. The difference between this embodiment and embodiment 1 is that the melt index of PP under the conditions of 230°C / 2.16kg is 40g / 10min, and the density is 0.89g / cm 3 , simply supported beam notch impact is 9KJ / m 2 The types, amounts and experimental parameters of the remaining raw materials are consistent with those in Example 1.

[0085] Example 9

[0086] A PP coffee machine shell material containing PCR. The difference between this embodiment and Example 4 is that PCR is 250g of consumer recycled polypropylene and 100g of consumer recycled polyamide, and the types, amounts and experimental parameters of other raw materials are consistent with those in Example 4.

[0087] Comparative Example

[0088] Comparative Example 1

[0089] A PP coffee machine shell material containing PCR. The difference between this embodiment and embodiment 1 is that PP and ABS resin are replaced with an equal amount of polyethylene, and the types, amounts and experimental parameters of other raw materials are consistent with those in embodiment 1.

[0090] The molecular weight of polyethylene is 5000.

[0091] Comparative Example 2

[0092] A PP coffee machine shell material containing PCR. The difference between this embodiment and embodiment 1 is that PP is replaced with an equal amount of polyethylene, and the types, amounts and experimental parameters of other raw materials are consistent with those in embodiment 1.

[0093] The molecular weight of polyethylene is 5000.

[0094] Comparative Example 3

[0095] A PP coffee machine shell material containing PCR. The difference between this embodiment and embodiment 1 is that ABS resin is replaced with an equal amount of polyethylene, and the types, amounts and experimental parameters of other raw materials are consistent with those in embodiment 1.

[0096] The molecular weight of polyethylene is 5000.

[0097] Comparative Example 4

[0098] A PP coffee machine shell material containing PCR. The difference between this embodiment and embodiment 1 is that the acid starch modifier is replaced by ethylene glycol, and the types, amounts and experimental parameters of other raw materials are consistent with those of embodiment 4.

[0099] Comparative Example 5

[0100] A PP coffee machine shell material containing PCR. The difference between this embodiment and embodiment 4 is that the acid starch modifier is replaced by a sodium hydroxide solution with a mass fraction of 10%, and the types, amounts and experimental parameters of other raw materials are consistent with those of embodiment 4.

[0101] Comparative Example 6

[0102] A PP coffee machine shell material containing PCR. The difference between this embodiment and embodiment 4 is that in step 1), 400g of water, 200g of starch and 30g of acid starch modifier (tartaric acid) are stirred at 60°C until a transparent state is obtained, stirring is continued for 1-2h, and then an alkaline solution is added to adjust the pH to 6.5-7.5, and the mixture is dried and crushed to obtain modified starch.

[0103] Performance testing

[0104] The tensile strength, impact resistance, wear resistance and aging performance tests were performed on the PCR-containing PP coffee machine shell materials prepared in Examples 1-9 and Comparative Examples 1-6.

[0105] Test method / test method Tensile strength: The tensile strength test is carried out according to the test method in ISO 527-2 "Determination of tensile properties of plastics".

[0106] Impact performance test: According to GB / T 1843-2008 / ISO 180:2000 "Determination of cantilever beam impact strength of plastics"

[0107] The impact strength is tested using the test method in.

[0108] Abrasion resistance test: Use Taber linear abrasion tester and CS-10 eraser. Under a load of 500g, set the friction parameter to 50 times / minute for friction. Record the number of times when scratches appear.

[0109] Aging test: According to the test method in GB / T7141-2008 "Plastic Thermal Aging Test Method", an artificial accelerated aging test was conducted, with an aging temperature of 90°C and an aging time of 500h, and then the tensile strength, impact performance and wear resistance were tested. The experimental data are shown in Table 3:

[0110] Table 3 Experimental data of Examples 1-9 and Comparative Examples 1-6

[0111]

[0112] It can be seen from Examples 1-9 and Comparative Examples 1-6 in combination with Table 3 that the present application prepares a coffee machine shell material by mixing PCR, PP, ABS resin, toughening agent, antioxidant, reinforcing filler, compatibilizer and dispersant in a specific proportion, thereby improving the tensile strength, impact resistance, wear resistance and aging resistance of the coffee machine shell material, and effectively extending the service life of the coffee machine shell material.

[0113] Comparing Example 1 with Comparative Examples 1-3, the tensile strength, impact strength and wear resistance of Comparative Examples 1-3 before aging are not as good as those of Example 1, and the rate of change of the tensile strength, impact strength and wear resistance values ​​of Comparative Examples 1-3 after aging is significantly greater than that of Example 1, indicating that the use of PCR, PP and ABS resins in combination in this application can well improve the tensile strength, impact strength, wear resistance and aging resistance of the coffee machine shell material.

[0114] Comparing Example 1 with Example 4, the tensile strength, impact strength and wear resistance of Example 4 before aging are better than those of Example 1, and the numerical change rate of the tensile strength, impact strength and wear resistance of Example 4 after aging is much smaller than that of Example 1, indicating that treating PCR by the method of the present application is beneficial to improving the tensile strength, impact strength, wear resistance and aging resistance of the coffee machine shell material.

[0115] Compared with Example 4, the tensile strength, impact strength and wear resistance of Example 9 before aging are slightly better than those of Example 4, and the numerical change rate of tensile strength, impact strength and wear resistance of Example 9 after aging is slightly smaller than that of Example 4, indicating that pretreatment of different types of PCR can improve the tensile strength, impact strength, wear resistance and aging resistance of the coffee machine shell material.

[0116] Compared with Comparative Examples 4-6, the tensile strength, impact strength and wear resistance of Comparative Examples 4-6 before aging are not as good as those of Example 4, and the rate of change of the tensile strength, impact strength and wear resistance values ​​of Comparative Examples 4-6 after aging is significantly greater than that of Example 4, indicating that the prefabricated PCR prepared by the formula and preparation method of the present application has a positive effect on improving the tensile strength, impact strength, wear resistance and aging resistance of the coffee machine shell material.

[0117] Compared with Example 1, the tensile strength, impact strength and wear resistance of Example 7 before aging are slightly better than those of Example 1, and the numerical change rate of the tensile strength, impact strength and wear resistance of Example 7 after aging is slightly smaller than that of Example 1, indicating that the tensile strength, impact strength, wear resistance and aging resistance of the coffee machine shell material can be further improved by optimizing the type of PCR.

[0118] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A PP coffee machine housing material containing PCR, characterized in that: Prepared from the following raw materials in weight percentage: PCR 35-52% PP 28-35% ABS resin 6-10% Reinforcement filler 5-10% Toughener 1-3% Antioxidant 0.5-1% Compatibilizer 2-3% Dispersant 3-6%; Before using PCR, pretreatment is required. The pretreatment steps are as follows: 1) Stir water and starch at 60-80°C until transparent, add acid starch modifier, continue stirring for 1-2h, add alkaline solution, adjust pH to 6.5-7.5, dry, and crush to obtain modified starch; 2) drying the PCR, mixing the dried PCR, silane coupling agent and modified starch, and then extruding and granulating the PCR through a twin-screw extruder to obtain prefabricated PCR; The weight parts of the raw materials used to prepare the PCR are as follows: 20-30 parts starch 40-50 parts water 3-6 parts of acid starch modifier 4-8 parts alkaline solution PCR 35-45 copies Silane coupling agent 2-5 parts; The PCR is consumer recycled polypropylene; The alkaline solution is a sodium carbonate solution with a mass fraction of 15%; The starch is one of corn starch, sweet potato starch or wheat starch; The acid starch modifier is one of adipic acid, tartaric acid or oleic acid; The PP has a melt index of 20-40 g / 10 min at 230°C / 2.16 kg and a density of ≤0.93 g / cm 3 , simply supported beam notch impact ≥7KJ / m 2 ; The ABS resin contains 5-30% butadiene, 40-60% styrene and 30-35% acrylonitrile; The compatibilizer is at least one of polyolefin long chain grafted maleic anhydride, glycidyl methacrylate, styrene grafted maleic anhydride and ABS grafted maleic anhydride; The reinforcing filler is at least one of silicon dioxide, glass fiber, calcium carbonate, talcum powder, titanium dioxide, quartz stone, ceramic powder, aluminum oxide and barium sulfate.

2. A method for preparing the PP coffee machine shell material containing PCR as claimed in claim 1, characterized in that: The method comprises the following preparation steps: S1, putting PCR, PP, ABS resin, reinforcing filler, toughening agent, antioxidant, compatibilizer and dispersant into a high-speed mixer and mixing at high speed to obtain a mixture; S2. The mixture is extruded and granulated through a twin-screw extruder, the extruder barrel temperature is 200-230° C., the die head temperature is 240-250° C., the main engine speed is 200-250 r / min, and the feeding speed is 10-25 r / min to obtain master batches, and then the master batches are injection molded to obtain PP coffee machine shell materials containing PCR.