Semiconductor structure and method for manufacturing the same

Through the improved inlay method, the CMP process is reduced in the semiconductor structure, and the stripping process and low-k value dielectric materials are used to solve the problems of high resource consumption and cost in the inlay process, and the efficient formation of interconnect structures and conductive lines is achieved. In the manufacture of high-frequency signal transmission and 3D MMIC.

CN118136601BActive Publication Date: 2024-11-01林君明
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311508200.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-10-04
Filing Date
2023-11-14
Publication Date
2024-11-01
Estimated Expiration
2043-11-14

AI Technical Summary

Technical Problem

The use of chemical mechanical polishing (CMP) technology in the existing mosaic process is time-consuming and cost-effective, and may lead to reliability problems. More economical and resource-saving methods are urgently needed to form interconnect structures and conductive lines.

Method used

Using the improved inlay method, the conductive terminals and conductive lines are formed in the front and rear section processes through the peeling process, reducing the use of the CMP process, and using low-k value dielectric materials and multi-layer insulating layer structure to form interconnection substrates and interconnections. The body combines the plating and removal of the photoresist layer and the conductive material to achieve the formation of the interconnect structure.

Benefits of technology

It significantly reduces the number of CMP processes, saves resources and time, improves the cost-effectiveness of semiconductor structures, and is suitable for high-frequency signal transmission and 3D MMIC manufacturing, improving process efficiency and circuit performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118136601B_ABST
    Figure CN118136601B_ABST
Patent Text Reader

Abstract

The present invention provides a semiconductor structure and a method for manufacturing the same. The semiconductor structure includes a conductive circuit of an Nth metal layer, a first insulating layer, a dielectric layer, a second insulating layer, an interconnection substrate and an interconnection body. The first insulating layer is on the conductive circuit and does not cover a portion of the conductive circuit. The dielectric layer is on the first insulating layer and does not cover the portion of the conductive circuit. The second insulating layer is on the dielectric layer and does not cover the portion of the conductive circuit. The interconnection substrate is laterally surrounded by the dielectric layer, the first insulating layer and the second insulating layer. The top surface of the interconnection substrate and the top surface of the second insulating layer are coplanar.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims priority to and benefits of U.S. regular application No. 18 / 480,567 filed on October 4, 2023, the contents of which are incorporated herein by reference in their entirety.

[0002] The present invention relates to a semiconductor structure, and more particularly to a semiconductor structure including an interconnect structure manufactured by an improved damascene method, wherein the method can reduce the use of a chemical-mechanical polishing (CMP) process. Background Art

[0003] Damascene processes are well-known semiconductor processes for manufacturing copper interconnect structures. Copper damascene processes provide a solution for forming conductive traces coupled to vias without etching the copper. Dual damascene processes allow for the simultaneous formation of conductive vias and conductive traces through a single copper deposition process. Generally, these damascene processes require a CMP process to flatten the surface of the copper layer. However, the CMP process is very time consuming and may cause reliability issues, and the slurry introduced to polish the metal is expensive. Therefore, there is an urgent need in the art for more cost-effective and resource-reducing methods to form interconnect structures and conductive lines. Summary of the invention

[0004] One aspect of the present invention discloses a semiconductor structure. The semiconductor structure includes: a conductive line of the Nth metal layer, a first insulating layer, a dielectric layer, a second insulating layer, an interconnect substrate and an interconnect body, wherein N is an integer equal to or greater than 1. The first insulating layer is on the conductive line and does not cover a portion of the conductive line. The dielectric layer is on the first insulating layer and does not cover the portion of the conductive line and a portion of the first insulating layer. The second insulating layer is on the dielectric layer and does not cover the portion of the conductive line. The interconnect substrate is laterally surrounded by the dielectric layer, the first insulating layer and the second insulating layer. The top surface of the interconnect substrate and the top surface of the second insulating layer are coplanar. The interconnect body is on the second insulating layer and contacts the top surface of the interconnect substrate.

[0005] Another aspect of the present invention provides a method for manufacturing a semiconductor structure. The method includes receiving a wafer having a conductive line of an Nth metal layer at a surface of the wafer, wherein N is an integer equal to or greater than 1; forming a first insulating layer on the surface of the wafer and not covering a portion of the conductive line; forming a dielectric layer (such as using a low-k dielectric material) on the first insulating layer; forming a second insulating layer on the dielectric layer and the first insulating layer, wherein the second insulating layer includes at least a base region, which is above the portion of the conductive line; and forming an interconnect substrate in the base region. The operation of forming the interconnect substrate in the base region includes forming a photoresist layer on the second insulating layer, wherein the base region of the second insulating layer is not covered by the photoresist layer; forming at least one conductive material on the photoresist layer, the second insulating layer and the conductive line, wherein the upper surface of the conductive material on the conductive line is substantially coplanar with the upper surface of the second insulating layer; and removing the conductive material on the second insulating layer by removing the photoresist layer to form the interconnect substrate by using a lift-off process. Furthermore, another photolithography process is applied, and a lift-off process is applied again in order to form the interconnect body and the conductive traces on the area having a different substrate from that without the interconnect. The results of the proposed improved damascene method are similar to those of the single damascene method. That is, the interconnect substrate and the conductive traces on the interconnect substrate can be formed by two lift-off processes, respectively. Therefore, the number of CMP processes can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] A more complete understanding of the present disclosure may be derived by referring to the detailed description and claims when considered in conjunction with the drawings, wherein like reference numerals refer to similar elements throughout the drawings.

[0007] Figure 1 is a semiconductor structure according to an embodiment of the present invention;

[0008] FIG. 2A to FIG. 2D is a cross-sectional view of a process for forming an input / output terminal of a CMOS transistor according to an embodiment of the present invention;

[0009] Figure 3 yes Figure 1 A cross-sectional view of the fabrication of a semiconductor structure interconnect substrate;

[0010] FIG. 4A to FIG. 4B is a cross-sectional view of an interconnect substrate manufacturing process according to an embodiment of the present invention;

[0011] Figure 5is a cross-sectional view of a metal layer according to an embodiment of the present invention;

[0012] Figure 6 is a cross-sectional view of a metal layer according to another embodiment of the present invention;

[0013] Figure 7 is a cross-sectional view of a metal layer having a surface area capable of increasing current flow according to another embodiment of the present invention;

[0014] Figure 8 is a cross-sectional view of a metal layer having a surface area capable of increasing current flow according to another embodiment of the present invention;

[0015] Fig. 9 is a cross-sectional view of a metal layer as a coaxial cable according to another embodiment of the present invention;

[0016] Fig.10 is a top view of a metal layer as a coaxial cable according to another embodiment of the present invention;

[0017] Fig.11 is a cross-sectional view of a metal layer as a pair of waveguides according to another embodiment of the present invention;

[0018] Fig.12 is a top view of the metal layer as a coaxial cable according to another embodiment of the present invention. DETAILED DESCRIPTION

[0019] The following description is accompanied by the drawings which are incorporated in this specification and constitute a part thereof, and they illustrate embodiments of the disclosed content, but the disclosed content is not limited to these embodiments. In addition, the following embodiments can be properly integrated to make another embodiment complete.

[0020] Reference to "one embodiment," "an embodiment," "exemplary embodiment," "other embodiments," "another embodiment," etc. indicates that the embodiment(s) of the disclosed content described so far may include a particular feature, structure, or characteristic, but not every embodiment is required to include that particular feature, structure, or characteristic. Furthermore, repeated use of the phrase "in the embodiment" does not necessarily refer to the same embodiment, although it may.

[0021] In order to make the disclosure of the present invention fully understandable, detailed steps and structures are provided in the following description. Obviously, the practice of the disclosure of the present invention is not limited to the specific details known to those skilled in the art. In addition, known structures and steps are not described in detail so as not to limit the disclosure of the present invention. The preferred embodiments of the disclosure of the present invention will be described in detail below. However, in addition to the implementation mode, the disclosure of the present invention may also be widely implemented in other embodiments. The scope of the disclosure of the present invention is not limited to the implementation mode, but is defined by the claims.

[0022] The embodiments disclosed in the present invention provide methods for manufacturing semiconductor structures, and the semiconductor structures described therein. The methods for manufacturing the semiconductor structures described therein include a modified version of a damascene process, which is capable of simultaneously forming conductive terminals in the front-end-of-line (FEOL) process and forming conductive lines in the back-end-of-line (BEOL) process by utilizing one or more lift-off processes, so as to reduce the use of a CMP process. Therefore, a large amount of resources and time required for the CMP process can be saved. Furthermore, the semiconductor structure provided by the embodiments disclosed in the present invention is suitable for high-frequency signal transmission, and can even be applied to form a monolithic microwave integrated circuit (MMIC) or a 3D MMIC.

[0023] Figure 1 A semiconductor structure 100 according to an embodiment of the present disclosure is shown. The semiconductor structure 100 includes a wafer 102; a conductive line 104 formed in the wafer 102; an interlayer dielectric layer 110; an interconnect substrate 122 formed in the interlayer dielectric layer 110 and in contact with the conductive line 104; and a metal layer 130 including an interconnect body 124 formed on the interconnect substrate 122. In an embodiment of the present invention, the conductive line 104 may be in the Nth metal layer, and the interconnect body 124 may be a part of the conductive line in the (N+1)th metal layer (i.e., the metal layer 130). In such a case, the interconnect structure 120 including the interconnect substrate 122 and the interconnect body 124 may provide a vertical electrical connection between the conductive lines in the metal layers of two different levels. That is, the interconnect structure 120 may provide additional electrical connections to the conductive line 104 so that the conductive line 104 may be coupled to other conductive traces or external circuits.

[0024] In the following description, the components of the semiconductor structure 100 will be described individually and separately. First, some possible manufacturing methods and structures of the conductive line 104 will be described, and then some possible manufacturing methods and structures of the interconnect substrate 122 will be presented. Finally, some possible manufacturing methods and structures of the metal layer 130 or the like will be described.

[0025] In an embodiment of the present invention, the conductive line 104 may be an input / output electrode (i.e., including a source, a drain, and a gate) of a field effect transistor (FET) formed in the wafer 102, or other terminals of other types of transistors. In such cases, the conductive line 104 is formed in the front end of the line (FEOL) and may include copper, cobalt, ruthenium, aluminum, tungsten, other conductors, or a combination thereof. However, the content disclosed in the present invention is not limited thereto. In some embodiments, the conductive line 104 may be part of a metal layer manufactured in the back end of the line (BEOL).

[0026] In some embodiments, before forming the interlayer dielectric layer 110 and the interconnect substrate 122 on the conductive circuit 104 and the wafer 102, if the surfaces of the conductive circuit 104 and the wafer 102 are not flat and cannot meet the requirements of the depth of focus (DoF) of the photolithography, a polishing process (such as a CMP process) may be performed to promote the formation of the interlayer dielectric layer 110 and the interconnect substrate 122. However, in order to reduce the use of the CMP process, so as to reduce the cost and time required, the content disclosed in the present invention will also propose a method for forming the conductive circuit 104 in the wafer 102 and making its surface flat enough to meet the DoF requirements.

[0027] In some embodiments, if the uneven surface of the conductive line 104 and the wafer 102 can be planarized by a spin on glass (SoG) process to reduce the use of a CMP process, the SoG process with a lower cost may be preferred. However, if the surface unevenness of the conductive line 104 and the wafer 102 exceeds the planarization capability of the SoG process, a lift-off process for depositing a metal material (such as tungsten) on the wafer 102 at a high temperature may be considered first, so that the conductive line 104 and the wafer 102 can have a flat surface after they are formed.

[0028] One embodiment of the present disclosure provides a method M1 for fabricating input / output electrodes (at high temperature) of a transistor by utilizing a lift-off process. FIG. 2A to FIG. 2D 2 is a cross-sectional view showing a process of forming a CMOS transistor and an input / output electrode according to method M1. Figure 2AIn the embodiment, the NMOS transistor T1 and the PMOS transistor T2 are formed in a P-type substrate 10. The NMOS transistor T1 includes a P-type well 11 formed in the substrate 10; and two N-type doped regions 14 (i.e., source / drain) formed in the P-type well 11. The PMOS transistor T2 includes an N-type well 12 formed in the substrate 10; and two P-type doped regions 15 (i.e., source / drain) formed in the N-type well 12. Figure 2A As shown in FIG. 1 , the NMOS transistor T1 and the PMOS transistor T2 can be separated by a shallow trench isolation (STI) structure 13. In the embodiment of the present invention, a method M1 is used to form the input / output electrodes (i.e., input / output plugs) of the transistors T1 and T2. The method M1 includes the following steps S110 to S190.

[0029] S110: Figure 2A As shown in FIG. 1 , an interlayer dielectric layer 16 is formed on the transistors T1 and T2 formed on the P-type substrate 10 .

[0030] S120: Figure 2B As shown in FIG. 1 , a first silicate glass layer 18 is formed on the interlayer dielectric layer 16 .

[0031] S130 : forming a first silicon nitride (SiN) layer 19 on a portion of the first silicate glass layer 18 disposed on the first terminals 17 of the transistors T1 and T2 .

[0032] S140 : forming a second silicate glass layer 20 on the first silicate glass layer 18 and the first SiN layer 19 .

[0033] S150 : forming a second SiN layer 21 on the second silicate glass layer 20 .

[0034] S160 : Forming a first opening H1 on the second terminals 14 and 15 of the transistors T1 and T2 .

[0035] S162 : depositing a layer of TiN (not shown) and a first layer of electrode metal 22 (including tungsten, cobalt, or ruthenium) to fill the first opening H1 .

[0036] S170 : removing the exposed portion of the second silicate glass layer 20 .

[0037] S180: Figure 2C As shown in FIG. 1 , a second opening H2 is formed on the first terminals of the transistors T1 and T2 .

[0038] S182: depositing a TiN layer (not shown) and a second electrode metal layer 23 (including tungsten, cobalt, or ruthenium) to fill the second opening H2.

[0039] S190: Remove the first SiN layer 19 and the second SiN layer 21. Figure 2D .

[0040] The brief introduction of method M1 is as follows. Figure 2A As shown in FIG. 1 , an interlayer dielectric layer 16 is formed on transistors T1 and T2 ( S120 ). After forming the interlayer dielectric layer 16 , as shown in FIG. Figure 2B As shown in , the following are formed in sequence: a first silicate glass layer 18, a first SiN layer 19 (S130), a second silicate glass layer 20 (S140) and a second SiN layer 21 (S150). It should be noted that the first SiN layer 19 is formed only on the portion of the first silicate glass layer 18 disposed on the first terminals 17 of the transistors T1 and T2 in the first silicate glass layer 18. In addition, in step S160, the second SiN layer 21 is patterned to form a first opening H1 on the second terminals 14 and 15 of the transistors T1 and T2, respectively. In an embodiment of the present invention, the depth of the second terminals 14 and 15 is disposed deeper than the first terminal 17. For example, the first terminal 17 may be the gate of the transistors T1 and T2, and the second terminals 14 and 15 may be the source / drain of the transistors T1 and T2.

[0041] It is noted that since the interlayer dielectric layer 16, the first silicate glass layer 18, the first SiN layer 19, the second silicate glass layer 20 and the second SiN layer 21 may be formed by a high temperature process in the FEOL, the lift-off method is also described as a "lift-off process for high temperature forming material" in the disclosure of the present invention.

[0042] Next, in step S162, Figure 2C As shown in FIG. 1 , a layer of TiN (2-10 nm, not shown) and a layer of electrode metal 22 (including tungsten, cobalt, or ruthenium) may be deposited on the second SiN layer 21 to fill the first opening H1 on the second terminals 14 and 15 of the transistors T1 and T2, thereby forming an input / output electrode coupled to the second terminals 14 and 15 of the transistors T1 and T2. In some embodiments, the layer of TiN may be a wetting layer for tungsten deposition, and the layer of TiN may have a thickness of, for example but not limited to, 2 nm to 10 nm.

[0043] After forming the input / output electrodes coupled to the second terminals 14 and 15 of the transistors T1 and T2, in step S170, the exposed portion of the second silicate glass layer 20 may be removed by deep reactive ion etching (DRIE). In such a case, the second SiN layer 21, TiN (not shown), and the electrode metal layer 22 formed on the exposed second silicate glass layer 20 may also be removed. In some embodiments, the silicate glass layers 18 and 20 may preferably be phospho-silicate glass (PSG) layers. Alternatively, the silicate glass layers 18 and 20 may be boron-phospho-silicate glass (BPSG) layers.

[0044] Afterwards, a lithography process may be sequentially performed to etch the first SiN layer 19, the first silicate glass layer 18, and the interlayer dielectric layer 16 partially formed on the first terminal 17, so that in step S180, a second opening H2 is formed on the first terminal 17. Next, in step S182, another layer of TiN (not shown) and another layer of electrode metal 23 (including tungsten, cobalt, or ruthenium) are deposited so as to Figure 2C Finally, in step S190, the SiN layers 19 and 21 are removed by DRIE, and thus the TiN (not shown) and the unwanted portions of the second electrode metal layer 23 are also removed. In this way, the input / output electrodes of the transistors T1 and T2 are formed, and their surfaces are as shown in FIG. Figure 2D The surfaces of the silicate glass layers 18 and 20 are substantially coplanar as shown in FIG. That is, method M1 allows for the formation of a flat surface in the FEOL by utilizing a lift-off process of a high temperature formed material to reduce the use of a CMP process. In some embodiments, Figure 1 The conductive circuit 104 in the wafer 102 may be an input / output electrode of the transistor, and the method M1 may be used to form the conductive circuit 104 on the wafer 102 and make it have a flat surface. However, the content disclosed in the present invention is not limited thereto.

[0045] Note that in other embodiments, the aforementioned electrodes (i.e., tungsten plugs) may also be filled in the manner of another embodiment. If the thickness of the electrodes (including tungsten, cobalt, or ruthenium) on the source and drain is greater than the thickness of the electrode on the gate by a thickness difference ΔT1, the electrodes on the gate, source, and drain may first be filled with the same thickness at the same time (in some embodiments, a TiN barrier layer may also be filled before depositing tungsten). Next, a first lift-off process after high-temperature formation of the material may be performed to form an electrode on the gate. In this case, portions of the electrodes on the source and drain will also be formed. Afterwards, another photoresist layer (not shown) may be applied to cover the gate and a first opening H1 may be formed on the source and drain. Next, the remaining portions of the electrodes on the source and drain may be filled in the first opening H1, and the thickness of the filling is equal to the thickness difference ΔT1 (in this embodiment, since a previously deposited TiN barrier layer may already exist at the sidewalls of the first opening H1 on the source and drain, a TiN barrier layer may not be deposited separately during this filling). Finally, a second stripping process after high-temperature formation of the material can be performed in sequence to form the rest of the electrode on the source and drain. In this way, an electrode thicker than the electrode on the gate can be formed on the source and drain, and there is a thickness difference ΔT1 between the two electrodes. In some embodiments, such a process can be repeated r times (where r is an integer greater than 1) to form electrodes with r different thicknesses. A more preferred method is that these electrodes can be formed in the order of their thickness, that is, the thinnest electrode should be formed first, and the thickest electrode should be formed last, so that only r processes are required and the process efficiency can be improved.

[0046] exist Figure 1 After the conductive line 104 (such as a tungsten plug) in the wafer 102 has been formed in the above method, and the surface of the conductive line 104 and the wafer 102 meet the DoF requirement, Figure 1 and Figure 3 The interconnect structure 120 shown in FIG. 1 , including an interconnect substrate 122 and an interconnect body 124 (eg, copper), may also be formed by another lift-off process to reduce the use of an expensive CMP process.

[0047] In the embodiment of the present invention, before forming the interconnect body 124, an interlayer dielectric layer 110 may be formed first. The interlayer dielectric layer 110 includes a first insulating layer 112, a dielectric layer 114, and a second insulating layer 116. The first insulating layer 112 is formed on the wafer 102, and the dielectric layer 114 is formed on the first insulating layer 112, while not covering at least a portion of the first insulating layer 112. The second insulating layer 116 is formed on the dielectric layer 114 and the first insulating layer 112, and the second insulating layer 116 may cover the sidewall of the dielectric layer 114.

[0048] In some embodiments, the first and second insulating layers 112 and 116 may include the same material, such as silicon oxynitride (SiOxNY), and the dielectric layer 114 may include, for example but not limited to, a low-k value (i.e., low dielectric constant) material, wherein the dielectric constant of the dielectric layer 114 may be less than the dielectric constants of the first and second insulating layers 112 and 116. For example, the dielectric constant of silicon oxynitride is greater than 3, and the dielectric constant of the dielectric layer 114 is less than 2.5. The dielectric layer 114 may include methylsilsesquioxane (MSQ), fluorocarbonsilsesquioxane (FSQ), and / or other suitable materials. In some embodiments, since the low-k value dielectric material may be a low hardness material, the second insulating layer 116 may surround the dielectric layer 114 to provide structural support for the dielectric layer 114.

[0049] Hereinafter, an improved damascene method M2 for manufacturing the interconnect substrate 122 will be described in detail according to an embodiment of the present invention. Figure 3 The cross-sectional view of the interconnect substrate 122 manufactured according to the method M2 is shown. The method M2 includes the following steps S210 to S240.

[0050] S210 : forming a first insulating layer 112 .

[0051] S220 : forming a dielectric layer 114 on the first insulating layer 112 while not covering at least a portion of the first insulating layer 112 .

[0052] S230 : forming a second insulating layer 116 on the dielectric layer 114 and the first insulating layer 112 .

[0053] S240 : forming an interconnection substrate 122 in the first insulating layer 112 and the second insulating layer 116 .

[0054] The method M2 is briefly described as follows: In some embodiments, the method M2 can be implemented to manufacture the semiconductor structure 100 .

[0055] In step S210 , a first insulating layer 112 is formed on the conductive circuit 104 . In the embodiment of the present invention, the first insulating layer 112 may be patterned by a photolithography process to form an opening 113 to expose at least a portion of the conductive circuit 104 .

[0056] Next, in step S220, a dielectric layer 114 is formed on the first insulating layer 112. In an embodiment of the present invention, the dielectric layer 114 may be patterned by a lithography process to form an opening 115, thereby exposing at least a portion of the first insulating layer 112 and at least a portion of the conductive line 104. The opening 115 formed in the dielectric layer 114 is projected onto the opening 113 previously formed in the first insulating layer 112. In some embodiments, the dielectric layer 114 may be thicker than the first insulating layer 112. For example, but not limited to, the thickness of the first insulating layer 112 may be between 100 nm and 150 nm, and the thickness of the dielectric layer 114 may be between 200 nm and 400 nm.

[0057] In step S230, the second insulating layer 116 is formed on the dielectric layer 114 and the first insulating layer 112. In the embodiment of the present invention, the second insulating layer 116 can be patterned by a lithography process to form an opening 117, thereby exposing at least a portion of the conductive line 104 to be coupled to the interconnect substrate 122. The opening 117 is a base region 119 (e.g., a portion of the second insulating layer 116 formed by the substrate 119) of the second insulating layer 116 located above the exposed portion of the conductive line 104. Figure 4A In some embodiments, the opening 113 of the first insulating layer 112 is completely included in the opening 117. Figure 3 As shown in , since the second insulating layer 116 surrounds the dielectric layer 114 and covers the sidewalls of the dielectric layer 114 , the second insulating layer 116 can provide structural support for the dielectric layer 114 , thereby maintaining the structural stability of the semiconductor structure 100 .

[0058] In some embodiments, the first and second insulating layers 112 and 116 may include silicon oxynitride. In such cases, since the formation of silicon oxynitride may require a deposition temperature as high as about 350° C., the dielectric layer 114 may include a material that can withstand temperatures exceeding about 350° C. to ensure the stability of the dielectric layer 114 during the formation of the second insulating layer 116.

[0059] like Figure 3 As shown in some embodiments, after forming the second insulating layer 116 in step S230, the interconnect substrate 122 is formed in the substrate region 119 of the first and second insulating layers 112 and 116 by filling the opening 117. In an embodiment of the present invention, the use of the CMP process can be reduced through step S240 of forming the interconnect substrate 122. According to an embodiment of the present invention, step S240 may include the following sub-steps S241 to S245 (method M3). FIG. 4A to FIG. 4B It is a cross-sectional view showing the process of interconnecting the substrate 122 according to sub-steps S241 to S245.

[0060] S241 : patterning the photoresist layer PR1 on the second insulating layer 116 so that the photoresist layer PR1 does not cover the base region 119 in the first insulating layer 112 and the second insulating layer 116 .

[0061] S242: forming a barrier layer 1221 on the photoresist layer PR1 and in the base region 119.

[0062] S243 : forming a copper-phosphorus alloy layer 1222 on the barrier layer 1221 .

[0063] S244 : a copper layer 1223 is plated on the copper-phosphorus alloy layer 1222 to fill the base region 119 .

[0064] S245: removing the photoresist layer PR1, and a portion of the barrier layer 1221, a portion of the copper-phosphorus alloy layer 1222, and a portion of the copper layer 1223 stacked on the photoresist layer PR1.

[0065] The brief introduction of method M3 is as follows. Figure 4A As shown in step S241, the photoresist layer PR1 is applied on the second insulating layer 116 and patterned to form an opening PR1-1 without covering the base region 119. In the embodiment of the present invention, the patterned photoresist layer PR1 can be patterned using the same mask as that used to pattern the second insulating layer 116. Therefore, Figure 4A The width of the opening PR1-1 shown in FIG. 1 is equal to Figure 3 , the width of the opening 113 of the first insulating layer 112 and the width of the opening 117 of the second insulating layer 116 are shown in FIG. In such a case, since the mask used for patterning the opening 113 of the insulating layers 112 and 116 can be reused for patterning the opening PR1-1 of the photoresist layer PR1, the cost of producing a new mask can be saved.

[0066] After forming the opening PR1-1 of the photoresist layer PR1, at least one conductive material may be applied on the wafer including the photoresist layer PR1 to form the interconnect substrate 122. In the embodiment of the present invention, the following three types of conductive materials may be used. Figure 4B The first conductive material shown: the barrier material layer 1221 is formed on the photoresist layer PR1, and Figure 4A The base region 119 (eg, Figure 3 In this case, the barrier material layer 1221 contacts one side of the first insulating layer 112 and one side of the second insulating layer 116, and also contacts the conductive line 104. Figure 4B In the embodiment of the present invention, the barrier material 1221 may include, for example but not limited to, titanium nitride (TiN).

[0067] In step S243, if Figure 4B The second conductive material: copper-phosphorus alloy layer 1222 is formed on the barrier layer 1221. In the embodiment of the present invention, the copper-phosphorus alloy layer 1222 can be regarded as a wetting layer required in the subsequent copper deposition step. In addition, the copper-phosphorus alloy layer 1222 can be formed by performing an electroless-plating process. Since the copper-phosphorus alloy layer 1222 has good wetting ability, it can form a good film covering the barrier layer 1221 and a good adhesion layer for the subsequent deposition of the third conductive material copper. In addition, in order to prevent the barrier material layer 1221 and the copper-phosphorus alloy layer 1222 from adhering to the sidewall of the photoresist layer PR1, a suitable additive (such as a quencher or inhibitor) can also be introduced into the plating solution.

[0068] After forming the copper-phosphorus alloy layer 1222, the copper layer 1223 is plated on the copper-phosphorus alloy layer 1222. Figure 4B In step S244, the Figure 3 Then, in step S245, the photoresist layer PR1 and the barrier layer 1221, the copper-phosphorus alloy layer 1222 and the copper layer 1223 on the photoresist layer PR1 are removed. Figure 3 As shown in FIG. 1 , the interconnection substrate 122 in the semiconductor structure 100 can be formed by such a lift-off operation method.

[0069] Therefore, by using the above-mentioned improved inlay method M2 and appropriately controlling the thickness of the plating material, the number of required CMP processes can be significantly reduced. In some embodiments, the thickness of the plated copper can be controlled by an AI learning and monitoring method. In this way, the use of the CMP process can be greatly reduced, and therefore, the resources required for the CMP process (such as water, slurry, electricity, manpower, conductive materials, etc.), and the additional design of redundant loads (dummy loads) can be saved. Therefore, the cost and yield of the semiconductor structure can be optimized, which is also in line with the spirit of corporate social responsibility (Environmental, social, and governance, ESG).

[0070] In some embodiments, in order to ensure that the unnecessary portions of the barrier layer 1221, the copper-phosphorus alloy layer 1222, and the copper layer 1223 on the photoresist layer PR1 can be removed without damaging the necessary portions of the barrier layer 1221, the copper-phosphorus alloy layer 1222, and the copper layer 1223 formed in the base region, the photoresist layer PR1 may be a negative photoresist. Since the negative photoresist will become insoluble in the photoresist developer after exposure, and the opening of the photoresist layer PR1 may have an undercut shape (not shown), which can reduce the connection between the unnecessary portions (such as the barrier layer 1221, the copper-phosphorus alloy layer 1222, and the copper layer 1223 on the photoresist layer PR1) and the necessary portions (such as the copper layer 1223 in the base region 119). This is because the undercut shape of the opening PR1-1 can prevent the copper layer 1223 from being attached to the sidewalls of the photoresist layer PR1 during the plating process.

[0071] Furthermore, in some embodiments, in order to further reduce the connection between the unnecessary parts of the plated metal and the required parts, two photoresist layers can be introduced. For example, after applying and patterning the photoresist layer PR1 to have an opening PR1-1, another additional photoresist layer can be applied and patterned thereon to have an opening. The additional photoresist layer may include a negative photoresist material, which is different from the material of the lower photoresist layer PR1, and the developer of the two is mutually exclusive. In such a case, after patterning the upper additional photoresist layer, the photoresist developer of the photoresist layer PR1 can be applied to further etch the photoresist layer PR1 and expand the opening PR1-1. Since the additional photoresist is insoluble in the photoresist developer of the photoresist layer PR1, the opening width of the additional photoresist will not change. In this way, by applying two photoresist layers, a lower layer with a larger undercut structure can be formed, and the stripping operation of a thicker copper layer can be carried out more smoothly (that is, a thicker copper layer can be plated through this method). In some embodiments, the copper layer 1223 may be replaced by a cobalt layer, a ruthenium layer, or an alloy layer containing at least one of the aforementioned metal materials. Figure 5 , and relevant instructions will be provided below.

[0072] In an embodiment of the present invention, the interconnect substrate 122 is formed in the semiconductor structure 100 to provide a vertical electrical connection between conductive lines in two different levels of metal layers. In this case, the interconnect substrate 122 can be regarded as a conductive via, and the interconnect body 124 can be a part of the conductive line of the metal layer 130. However, the content disclosed in the present invention is not limited to this. In some embodiments, the interconnect substrate 122 is not necessarily a via coupled between conductive lines in different metal layers; instead, the interconnect substrate 122 may be advantageously used to make passive components of 3D MMIC. For example, compared with conventional MMICs that are usually formed on silicon interposers (such as PI) or PCBs, the methods and semiconductor structures provided by the embodiments of the present invention allow designers to use semiconductor processes for manufacturing the interconnect substrate 122 to manufacture 3D MMICs with better performance, and to obtain smaller dimensions, higher accuracy (such as bandwidth and gain) and better yield.

[0073] Specifically, the method for forming the interconnect substrate 122 disclosed in the present invention can be flexibly applied to the passive components of the integrated multi-layer 3D MMIC. For example, the interconnect substrate 122 can be used to make: a waveguide, a bandpass filter, a bandstop filter, a resonator with parallel or series parasitic inductance and capacitance, a π-type or T-type impedance matching filter. Furthermore, by using an improved inlay method that can reduce the use of CMP processes, embedded passive components in 3D MMICs can also be formed in a lower cost manner. Furthermore, since these embedded passive components can be perpendicular to other planar components in the semiconductor structure, most of the current formed on the interconnect substrate 122 in the passive components of the 3D MMIC will flow in the longitudinal direction, and therefore, the electromagnetic field generated by these 3D MMICs can be perpendicular to the electromagnetic field generated by the planar semiconductor components, thereby significantly reducing the mutual interference between the circuits.

[0074] In addition, the interconnect substrate 122 introduced for fabricating 3D MMICs may have larger dimensions than conventional copper vias. For example, the interconnect substrate 122 may have a diameter in the range of 1 μm to 500 μm, and a thickness in the range of 10 μm to 400 μm, while other conventional tungsten plugs or copper vias on the wafer may only have a diameter in the range of 10 nm to 100 nm, and a thickness in the range of 10 nm to 1 μm.

[0075] After forming the interconnect substrate 122, a substrate such as Figure 1The metal layer 130 and the dielectric layer 140 for insulation are shown in FIG. In the embodiment of the present invention, since the copper plating (including electro-plating and electroless plating) process allows accurate thickness control, for example, by AI learning and monitoring methods, the thickness of the copper layer 1223 can be controlled to be substantially the same as the depth of the substrate region 119. The surface of the interconnect body 124 and the surface of the insulating layer 116 can be substantially coplanar, and therefore, the dielectric layer 140 can be formed on the upper surfaces of the flat interconnect body 124 and the insulating layer 116 and patterned appropriately.

[0076] After patterning the dielectric layer 140, the metal layer 130 may be formed. In an embodiment of the present invention, the metal layer 130 includes an interconnect body 124 and conductive traces 132 and 134. The interconnect body 124 is disposed on the interconnect substrate 122, and the conductive traces 132 and 134 are disposed on the insulating layer 116. In some embodiments, the conductive traces 132 and 134 may be part of other conductive lines in the metal layer 130.

[0077] In one embodiment of the present invention, the metal layer 130 can be formed by a method similar to that used to form the interconnect substrate 122 (i.e., a lift-off process) as mentioned above. That is, the metal layer 130 can be deposited to fill the opening of the dielectric layer 140, thereby forming the required circuits and reducing the use of the CMP process, thereby simplifying the semiconductor process and reducing resources (such as water, slurry, electricity, manpower, conductive materials, etc.), redundant loads of additional designs, dish effects, reliability issues, time, and costs. Therefore, in some embodiments of the present invention, the formation of the interconnect substrate 122 and the interconnect body 124 are based on the above-mentioned improved damascene method that can reduce the use of the CMP process.

[0078] Furthermore, in some embodiments, since the CMP process is limited by the durability of the chemical mechanical polishing between the thick copper layer and the low dielectric material, the improved damascene method uses the above lift-off process to form the conductive traces 132, 134 and the interconnect body 124 with various thicknesses, and even greater than the thickness of the conductive traces formed by the conventional method. Therefore, the conductive traces 132, 134 and the interconnect body 124 have a lower resistance. In some embodiments, such thicker and lower resistance conductive traces 132 and 134 are particularly desired for forming the outer regions of the wafer and high power devices.

[0079] In addition, in the embodiment of the present invention, since the thickness of the interconnect body 124 is the same as the thickness of the conductive traces 132 and 134, the interconnect body 124 and the conductive traces 132 and 134 can be formed by the same copper plating process and the same lift-off process. However, in some other embodiments, the conductive traces 132, 134 in the metal layer 130 and the interconnect body 124 may also have different thicknesses. For example, if the conductive trace 132 is used to transmit higher power electricity, the thickness of the conductive trace 132 may be greater than the thickness of the general conductive trace 134 and the interconnect body 124 (the thickness of 124 and 134 is equal), and the thickness difference may be, for example, ΔT2, so that the conductive trace 132 can have a lower resistance, thereby improving the power transmission efficiency. A preferred process in such a case is: a copper layer may be plated first to form the conductive trace 134 (in some embodiments, the barrier layer and the copper-phosphorus alloy layer may also be plated with the copper layer) and the interconnect body 124 with the same thickness in the metal layer 130, and to form the first portion of the conductive trace 132. Then, a first lift-off process may be performed to form the conductive trace 134 and the interconnect body 124, and the first portion of the conductive trace 132. Next, another photoresist layer may be applied to cover the conductive trace 134 and the interconnect body 124, but at the same time, an opening is formed on the first portion of the conductive trace 132. Then, another copper layer may be plated in the opening of the photoresist layer (such as on the conductive trace 132) and on the photoresist layer, and the thickness of this other copper layer is equal to the thickness difference ΔT2 (in some embodiments, the barrier layer and the copper-phosphorus alloy layer may also be plated first when the copper layer is plated). Finally, a second lift-off process may then be performed to form the second portion of the higher power conductive trace 132. As a result, the conductive trace 132 having a greater thickness than the conductive trace 134 and the interconnection body 124 and transmitting higher power can be formed, and there is a thickness difference ΔT2 between the two thicknesses.

[0080] In some embodiments, such a process may be repeated multiple times to form conductive traces and / or interconnect bodies with multiple different thicknesses. That is, when there are conductive traces and / or interconnect bodies with q (an integer greater than 1) different thicknesses, the conductive traces and / or interconnect bodies may be formed sequentially according to their thicknesses, wherein the thinnest conductive traces and / or interconnect bodies should be formed first, and the thickest conductive traces and / or interconnect bodies may be formed last, so that only q processes need to be performed to complete the process, thereby improving process efficiency.

[0081] Similarly, the interconnect substrate 122 may also be formed with different thicknesses. For example, if there are interconnect substrates 122 with p (an integer greater than 1) different thicknesses, the method including the metal plating process and the stripping process described in the previous paragraph may be applied and performed p times to form an interconnect substrate with the smallest thickness to form an interconnect substrate with the largest thickness.

[0082] Some more embodiments of the present invention are presented below to illustrate other possible manufacturing methods and structures of the metal layer.

[0083] Figure 5 2 is a cross-sectional view of a metal layer 230 according to an embodiment of the present disclosure. The metal layer 230 includes a conductive trace 232 disposed on the second insulating layer 216 and an interconnect body 224 disposed on the interconnect substrate 222. Figure 5 As shown in , the conductive traces 232 and the interconnect body 224 may be isolated from each other by a dielectric layer 240. In some embodiments, similar to the dielectric layer 140, the dielectric layer 240 may include a low dielectric constant material. In an embodiment of the present invention, the conductive traces 232 and the interconnect body 224 may be formed by a process similar to the aforementioned process of forming the interconnect substrate 122, and the process for forming the metal layer 230 may also be similar to the process of forming the metal layer 130. For example, after forming the insulating layer 216, a photoresist layer may be patterned thereon, and a barrier layer B1, a copper-phosphorus alloy P1, and a copper layer C1 may be sequentially formed thereon. Then, the barrier layer B1, the copper-phosphorus alloy P1, non-essential portions of the copper layer C1, and the photoresist layer, etc., may be removed by a stripping process.

[0084] In one embodiment of the present invention, in order to ensure that unnecessary copper and photoresist layers remaining on the photoresist layer can be removed, the openings of the insulating layer 216 can be filled directly without a single copper layer with a large plating thickness. Instead, the thickness measurement and monitoring by AI learning technology can be used to perform multiple plating processes. Figure 5 As shown in , copper layers C1, C2 and C3 may be formed by three plating processes respectively, and the thickness of each copper layer C1, C2 and C3 may be approximately equal to one third of the thickness of dielectric layer 240. However, the disclosure of the present invention is not limited thereto. In some embodiments, interconnect body 224 or conductive trace 232 may include only one copper layer or other number of copper layers as required. That is, in some embodiments, the opening of insulating layer 216 may be directly filled with: barrier layer B1, copper-phosphorus alloy P1 and copper layer C1, without further plating copper layers C2 and C3.

[0085] After filling the opening of the insulating layer 216 (the opening of the insulating layer 216 may be filled with the entire thickness of the copper layer C1 at one time, or multiple copper layers such as C1, C2, and C3 may be filled in sequence as in the following example), and before forming the third insulating layer 250, another copper-phosphorus alloy layer P2 and another barrier layer B2 may be formed in sequence. In this case, the copper-phosphorus alloy layers P1 and P2 are sandwiched between the copper layers C1, C2, and C3 and the barrier layers B1 and B2, and the copper layers C1, C2, and C3 are confined within the upper and lower barrier layers B1 and B2. The copper-phosphorus alloy layer P2 above the copper layers C1, C2, and C3 can protect the copper layers C1, C2, and C3 from oxidation. In some embodiments, the copper layers C1, C2, and C3 may also be replaced with at least one of the metal materials mentioned above, such as a cobalt layer, a ruthenium layer, or an alloy layer. In some embodiments, if the process is not fully developed, offline measurement can be performed after each copper layer C1, C2 or C3 is plated. In this case, each time the copper layer C1, C2 or C3 is plated, a layer of copper-phosphorus alloy can be formed thereon to protect the copper layer C1, C2 or C3. However, the content disclosed in the present invention is not limited thereto.

[0086] Furthermore, in the embodiment of the present invention, if the metal layer 230 is a top metal layer, a polyimide layer 260 may be further formed on the third insulating layer 250 to form a flat top surface ( Figure 5 The upper structure and the lower structure for connecting to an external circuit and a ground point are not shown). However, the present disclosure is not limited thereto.

[0087] In some embodiments, conductive traces in semiconductor structures may be used for high frequency signal transmission. In such embodiments, skin effect may become significant, resulting in low signal transmission efficiency. In the present disclosure, to improve signal transmission efficiency, low-k dielectrics may be formed in conductive traces and / or interconnect bodies to increase the total surface area of ​​the traces and interconnect bodies, thereby improving signal transmission efficiency, as described below.

[0088] Figure 6 is a cross-sectional view of a metal layer 330 according to another embodiment of the present invention. In some embodiments, the metal layer 330 can be used to replace the metal layer 130. In some embodiments, as Figure 6 As shown in FIG. 3 , a dielectric layer 340 is formed on the second insulating layer 316 and the interconnect substrate 322. In an embodiment of the present invention, the dielectric layer 340 is patterned to form a plurality of openings 341, 342, 343, and 344, and a dielectric body 345 is left between the openings 341 and 342, and a dielectric body 346 is left between the openings 343 and 344. In some embodiments, the dielectric layer 340 and the dielectric bodies 345 and 346 may include a dielectric material having a low dielectric constant (i.e., a low-k value material).

[0089] like Figure 6 As shown in FIG, after the dielectric layer 340 is patterned, a barrier layer B1, a copper-phosphorus alloy layer P1, and a copper layer C1 may be formed in the openings 341, 342, 343, and 344 of the dielectric layer 340 by a process similar to that previously illustrated. Similarly, another copper layer C2 may be plated on the copper layer C1.

[0090] Furthermore, if Figure 6 As shown in FIG. 1 , another copper layer C3 is deposited on the copper layer C2 and the dielectrics 345 and 346. Next, a copper-phosphorus alloy layer P2 and a barrier layer B2 may be sequentially formed on the copper layer C3 so that the copper layers C1, C2, and C3 are confined within the barrier layers B1 and B2. In this way, the conductive trace 332 and the interconnect body 324 of the metal layer 330 may be formed. In the embodiment of the present invention, as the dielectric 345 is formed within the conductive trace 332 and the dielectric 346 is formed within the interconnect body 324, the surface area of ​​the conductive trace 332 and the surface area of ​​the interconnect body 324 may be increased. In this case, the reduction in signal transmission efficiency caused by the skin effect may be mitigated.

[0091] In some embodiments, Figure 6 As shown in , a third insulating layer 350 may be formed on the metal layer 330. In addition, if the metal layer 330 is a top metal layer, that is, if no further metal layer is to be formed on the metal layer 330, a polyimide layer 360 may be further formed on the third insulating layer 350 to obtain a flat top surface. Figure 6 The upper and lower structures for connection to external circuits and grounding points are not shown)

[0092] like Figure 6 As shown in FIG. 3 , dielectrics 345 and 346 may be formed at the bottom of metal layer 330 . However, the present invention is not limited thereto. In some other embodiments, the dielectric may also be embedded in metal layer 330 .

[0093] Figure 7 FIG. 4 is a cross-sectional view showing another embodiment of the present invention, which has a metal layer 430 with an increased surface area. Figure 7 As shown in FIG. 4 , dielectric layer 440 may be formed on second insulating layer 416 and interconnect substrate 422. In an embodiment of the present invention, patterned dielectric layer 440 is patterned to form openings on the left MMIC to form conductive traces 432 and to form openings on the right MMIC to form interconnect body 424.

[0094] In some embodiments, Figure 7As shown, by performing a process similar to that previously illustrated, a barrier layer B1, a copper-phosphorus alloy layer P1, and a copper layer C1 may be formed in the opening of the dielectric layer 440, thereby forming a conductive trace 432 and an interconnect body 424.

[0095] Next, dielectrics 445 and 446 may be formed on the copper layer C1 by using a photolithography process. Furthermore, a copper layer C2 may be plated on the copper layer C1 and the dielectrics 445 and 446. In this way, the dielectrics 445 and 446 may be embedded in the copper layers C1 and C2 in the conductive traces 432 and the interconnect body 424.

[0096] Furthermore, if Figure 7 As shown, a copper-phosphorus alloy layer P2 and a barrier layer B2 may be formed on the copper layer C2, and a third insulating layer 450 may be formed on the metal layer 430. In addition, if the metal layer 430 is the top metal layer (i.e., if no further metal layer is to be formed on the metal layer 430), a polyimide layer 460 (or the like) may be formed on the third insulating layer 450 to obtain a flat top surface. In some embodiments, a coplanar waveguide (not shown) of a 3D MMIC may be formed on the flat polyimide layer 460. ( Figure 7 The upper and lower structures for connection to external circuits and grounding points are not shown)

[0097] In such Figure 7 In the embodiment shown, dielectrics 445 and 446 may be embedded in the conductive traces 432 and the interconnection body 424; however, the present invention is not limited thereto. In some embodiments, not only more layers of copper metal may be formed, but more dielectrics may also be embedded therein to further increase the surface area of ​​the conductive traces 432 and the interconnection body 424.

[0098] Figure 8 A cross-sectional view of a metal layer 530 with increased surface area is shown in accordance with another embodiment of the present invention. Figure 8 As shown in FIG. 5 , a dielectric layer 540 may be formed on the second insulating layer 516 and the interconnect substrate 522. In the present embodiment, the dielectric layer 540 is patterned to form two openings on the second insulating layer 516 and the MMIC corresponding to the interconnect body 524 to form the conductive trace 532 and the interconnect body 524, respectively.

[0099] At least one dielectric 545 is embedded in each of the conductive traces 532 and the interconnect body 524. In addition, by controlling the thickness of the deposited copper, the copper layer C2 can be formed on the copper layer C1 without covering the dielectric 545. In addition, the surface of the copper layer C2 and the surface of the dielectric 545 can be substantially coplanar. In this case, the copper layer can be formed on the copper layer C2 and the dielectric 545. In addition, another barrier layer B2 and another copper-phosphorus alloy layer P2 can be formed above the copper layer C3. In this way, a flat third insulating layer 550 and a polyimide layer 560 can be formed, as shown in FIG. Figure 8 As shown. ( Figure 8 Not shown are the upper and lower structures for connection to external circuits and grounding points).

[0100] exist Figure 7 and Figure 8 In the embodiment shown in FIG, by embedding the dielectric in the conductive lines (such as the conductive traces 432, 532 and the interconnect bodies 424, 524), the surface area thereof can be increased, making such conductive lines particularly suitable for high frequency applications. On the other hand, by designing appropriate dimensions, the conductive traces 432, 532 and the interconnect bodies 424, 524 can be increased. Figure 7 and Figure 8 The circuits in the invention are applied in filters such as low pass, band pass, high pass and notch filters.

[0101] Although the transmission efficiency of high-frequency signals can be improved by increasing the surface area of ​​the transmission lines, as described above, since the distance between the transmission lines has become shorter as the size of the die decreases, different high-frequency signal transmissions may still interfere with each other, such as electromagnetic interference (EMI), causing problems.

[0102] Fig. 9 A cross-sectional view of a metal layer 630 as a coaxial cable according to another embodiment of the present disclosure is shown. In an embodiment of the present disclosure, the metal layer 630 includes conductive traces 632, 634, and 636 separated by a dielectric layer 640. Among them, the conductive trace 632 can be used to transmit high-frequency signals, and the conductive traces 634 and 636 can be coupled to the ground. In this case, the conductive traces 632, 634, and 636 can be used as a 3D waveguide. However, the present disclosure is not limited to this. In some other embodiments, the conductive traces 632, 634, and 636 can also be used as a π-type or T-type impedance matching filter. ( Fig. 9 Not shown are the upper and lower structures for connection to external circuits and grounding points).

[0103] In some embodiments, the conductive traces 632, 634, and 636 may be formed by the processes described and exemplified above. In this case, each of the conductive traces 632, 634, and 636 may include a first barrier layer B1, a first copper-phosphorus alloy layer P1, at least one copper layer C1, a second barrier layer B2, and a second copper-phosphorus alloy layer P1. However, the present invention is not limited thereto.

[0104] In some embodiments, conductive traces 634 and 636 may extend parallel to conductive trace 632 in order to contain electromagnetic fields caused by high frequency signals transmitted by conductive trace 632 .

[0105] In some embodiments, the conductive traces 632, 634 and 636 may extend laterally along the XY plane; however, the present disclosure is not limited thereto. In other embodiments, the conductive traces may also extend longitudinally along the Z direction, and similar electromagnetic shielding structures may also be introduced at the same time.

[0106] Fig.10 A top view of a metal layer 730 as a coaxial cable according to another embodiment of the present invention is shown. In an embodiment of the present invention, the metal layer 730 includes conductive traces 732 and 734, which extend upward along the direction Z. In this embodiment, the conductive trace 734 coupled to the ground can surround the conductive trace 732 used to transmit high-frequency signals. In this way, the conductive trace 734 can provide a thorough shielding wall (such as a coaxial cable) to reduce EMI problems. However, the present invention is not limited to this. In some other embodiments, the inner conductive trace 732 can be used for grounding, while the outer conductive trace 734 can be used to transmit high-frequency signals, and the circuit can be used in a π-type or T-type impedance matching filter. ( Fig.10 Not shown are the upper and lower structures for connection to external circuits and grounding points).

[0107] Furthermore, in some embodiments, in order to increase the surface area that can provide high-frequency current flow, multiple conductive traces can be introduced to transmit the same high-frequency signal.

[0108] Fig.11A cross-sectional view of a metal layer 830 as a pair of waveguides according to another embodiment of the present disclosure is shown. In an embodiment of the present invention, the metal layer 830 includes conductive traces 832, 834, 836, and 838, which extend along the XY plane. Conductive traces 832 and 834 can be used to transmit the same high-frequency signal, and conductive traces 836 and 838 can be coupled to the ground. In this embodiment, the metal layer 830 can be used as a pair of waveguides for transmitting high-frequency signals, wherein the signal transmission efficiency can be improved due to the increase in the total surface area available for high-frequency current to flow through. On the other hand, the metal layer 830 can also be used as a π-type or T-type impedance matching filter. ( Fig.11 Not shown are the upper and lower structures for connection to external circuits and grounding points).

[0109] Fig.12 A top view of a metal layer 930 as a coaxial cable according to another embodiment of the present disclosure is shown. In an embodiment of the present disclosure, the metal layer 930 includes conductive traces 931, 932, 933, 934, and 936, which extend along the Z direction. The conductive traces 931, 932, 933, and 934 can be used to transmit the same high frequency signal, and the conductive trace 936 can be coupled to the ground.

[0110] In this embodiment, since the conductive trace 936 can surround the conductive traces 931, 932, 933 and 934, the EMI caused by the high-frequency signals transmitted by the conductive traces 931, 932, 933 and 934 can be shielded. Therefore, in some embodiments, multiple conductive traces 931, 932, 933 and 934 can be used as a coaxial cable between a pair of upper and lower circuits. Furthermore, since more conductive traces are introduced to transmit the same high-frequency signal, the total surface area through which the high-frequency current flows can be further increased. Through appropriate design, this basic circuit can be applied to one of the pins of a semiconductor (such as Si) interposer (such as TSV), thereby reducing the coupling between the pins. On the other hand, the inner conductive traces 931, 932, 933 and 934 can also be grounded, while the outer conductive trace 936 can be used to transmit high-frequency signals. At this time, the circuit can be applied as one of the π-type or T-type impedance matching filters. ( Fig.12 Not shown are the upper and lower structures for connection to external circuits and grounding points).

[0111] In summary, the semiconductor structure and the manufacturing method thereof provided by the embodiments of the present invention allow the formation of interconnect structures and conductive traces to reduce the number of times the CMP process is performed on copper. Therefore, the manufacturing time and cost can be reduced. In addition, since the interconnect structures and / or conductive traces in the semiconductor structure can be used to make 3D MMICs, not only can the circuit area be reduced but also the circuit performance can be improved. Furthermore, by embedding the dielectric in the conductive traces and the interconnect structures, the surface area of ​​the conductive traces and the interconnect structures can be increased. In this way, the transmission efficiency of high-frequency signals can also be improved.

[0112] Although the present invention and its advantages have been described in detail, it should be understood that various changes, substitutions, and modifications can be made herein without departing from the spirit and scope of the disclosed content as defined by the appended claims. For example, many of the processes discussed above can be implemented in different ways and replaced by other processes or combinations thereof.

[0113] Furthermore, the scope of the present invention is not intended to be limited to the specific embodiments of the processes, machines, manufactures, compositions of matter, means, methods, and steps described in this specification. As will be readily apparent to one skilled in the art from the disclosure of the present invention, processes, machines, manufactures, compositions of matter, means, methods, or steps now existing or to be developed that perform substantially the same functions or achieve substantially the same results as the corresponding embodiments described herein may be utilized in accordance with the present invention. Accordingly, the appended claims are intended to include within their scope such processes, machines, manufactures, compositions of matter, means, methods, and steps.

[0114] Explanation of symbols

[0115] 10:P type substrate; substrate

[0116] 11: P-type well

[0117] 12: N-type well

[0118] 13: Shallow Trench Isolation (STI) Structure

[0119] 14: N-type doped region; second terminal

[0120] 15: P-type doped region; second terminal

[0121] 16,110: Interlayer dielectric layer

[0122] 17: First terminal

[0123] 18: first silicate glass layer; silicate glass layer

[0124] 19: first silicon nitride (SiN) layer; SiN layer

[0125] 20: second silicate glass layer; silicate glass layer

[0126] 21: second SiN layer; SiN layer

[0127] 22: electrode metal; electrode metal layer

[0128] 23: electrode metal; electrode metal layer; second electrode metal layer

[0129] 100:Semiconductor structure

[0130] 102: Wafer

[0131] 104: Conductive circuit

[0132] 112: insulating layer; first insulating layer

[0133] 113,115,117,341,342,343,344: Opening

[0134] 114,140,240,340,440,540,640: Dielectric layer

[0135] 116,216: insulating layer; second insulating layer

[0136] 119: Basal area

[0137] 120: Interconnection structure

[0138] 122,222,322,422,522: Interconnect substrate

[0139] 1221: barrier layer; barrier material

[0140] 1222: Copper-phosphorus alloy layer

[0141] 1223: Copper layer

[0142] 124,224,324,424,524: Interconnected Ontologies

[0143] 130,230,330,430,530,630,730,830,930:Metal layer

[0144] 132,134,232,332,432,532,632,634,636,832,834,836,838: Conductive traces

[0145] 250,350,450,550: The third insulation layer

[0146] 260,360,460,560: Polyimide layer

[0147] 316,416,516: Second insulation layer

[0148] 345,346,445,446,545: Dielectric

[0149] 732: conductive trace; inner conductor

[0150] 734: conductive trace; outer conductor

[0151] 931,932,933,934: Conductive trace; Internal conductive trace

[0152] 936: conductive trace; external conductive trace

[0153] H1, H2: first hole; second hole

Claims

1. A semiconductor structure, characterized in that: Include: A conductive line of an Nth metal layer, wherein N is an integer equal to or greater than 1; A first insulating layer, which is on the conductive circuit and does not cover a portion of the conductive circuit; a first dielectric layer on the first insulating layer and not covering the portion of the conductive line and a portion of the first insulating layer; a second insulating layer on the first dielectric layer and not covering the portion of the conductive line; an interconnect substrate laterally surrounded by the first dielectric layer, the first insulating layer, and the second insulating layer, wherein a top surface of the interconnect substrate and a top surface of the second insulating layer are coplanar; an interconnect body overlying the second insulating layer and contacting the top surface of the interconnect substrate; and a second dielectric layer configured to isolate the interconnect body from the conductive traces overlying the second insulating layer; The interconnection entity comprises: a first barrier layer directly contacting the interconnect substrate and the sidewalls of the second dielectric layer; at least one conductive layer surrounded by the barrier layer; a first copper-phosphorus alloy layer sandwiched between the first barrier layer and the at least one conductive layer; a second copper-phosphorus alloy layer formed on the at least one conductive layer; as well as A second barrier layer is formed on the second copper-phosphorus alloy layer.

2. The semiconductor structure of claim 1, wherein a dielectric constant of the first dielectric layer is smaller than dielectric constants of the first insulating layer and the second insulating layer.

3. The semiconductor structure of claim 1, wherein the interconnect substrate comprises: a barrier layer directly contacting the first insulating layer and the second insulating layer; a copper layer surrounded by the barrier layer; and A copper-phosphorus alloy layer is sandwiched between the barrier layer and the copper layer.

4. The semiconductor structure of claim 1, further comprising: a first conductive trace on the second insulating layer; The interconnect body and the first conductive trace are part of a conductive line of an N+1th metal layer and are laterally separated by a second dielectric layer, and the first conductive trace overlaps the first dielectric layer along a stacking direction of the semiconductor structure.

5. The semiconductor structure of claim 4, further comprising: A dielectric body is formed in the first conductive trace or the interconnect body.

6. The semiconductor structure of claim 4, further comprising a second conductive trace adjacent to the first conductive trace, the first conductive trace being configured to transmit a high frequency signal, the second conductive trace being coupled to ground, and the first conductive trace being separated from the second conductive trace by a second dielectric layer.

7. The semiconductor structure of claim 6 wherein said second conductive trace surrounds said first conductive trace.

8. The semiconductor structure of claim 7, further comprising a third conductive trace configured to transmit the high frequency signal together with the first conductive trace, the second conductive trace surrounding the first conductive trace and the third conductive trace, and the first conductive trace being separated from the third conductive trace by the second dielectric layer.

9. The semiconductor structure of claim 6, further comprising a fourth conductive trace coupled to the ground, the first conductive trace being disposed between the second conductive trace and the fourth conductive trace, and the first conductive trace being separated from the fourth conductive trace by the second dielectric layer.

10. The semiconductor structure of claim 9, further comprising a fifth conductive trace configured to transmit the high frequency signal together with the first conductive trace, and the first conductive trace and the fifth conductive trace are arranged between the second conductive trace and the fourth conductive trace.

11. The semiconductor structure of claim 4, wherein a thickness of said interconnect body is different from a thickness of said first conductive trace.

12. The semiconductor structure of claim 1, wherein said at least one conductive layer comprises at least one metallic material of copper, cobalt, and ruthenium.

13. The semiconductor structure of claim 1, wherein a multi-layer 3D monolithic microwave integrated circuit is formed within the semiconductor structure, and the multi-layer 3D monolithic microwave integrated circuit comprises the interconnect substrate.

14. The semiconductor structure of claim 1, wherein the interconnect substrate is a portion of a waveguide, a bandpass filter, a bandstop filter, a π-type impedance matching filter, or a T-type impedance matching filter.

15. A method for manufacturing a semiconductor structure, characterized in that: Include: A receiving wafer having a conductive trace of an Nth metal layer at a surface thereof, wherein N is an integer equal to or greater than 1; forming a first insulating layer on the surface of the wafer and not covering a portion of the conductive circuit; forming a first dielectric layer on the first insulating layer and not covering the portion of the conductive line and a portion of the first insulating layer; forming a second insulating layer on the first dielectric layer and the first insulating layer, wherein the second insulating layer comprises at least one base region, the base region is located above the portion of the conductive line and does not cover the portion of the conductive line; forming an interconnect substrate in the substrate region, comprising: forming a photoresist layer on the second insulating layer, wherein the base region of the second insulating layer is not covered by the photoresist layer; forming at least one conductive material on the photoresist layer, the second insulating layer and the conductive circuit, wherein the upper surface of the conductive material on the conductive circuit is substantially coplanar with the upper surface of the second insulating layer; and removing the conductive material on the second insulating layer by removing the photoresist layer to form the interconnect substrate; forming a second dielectric layer on the second insulating layer; forming a first conductive trace on the second insulating layer; as well as forming an interconnect body on the interconnect substrate; wherein the interconnect substrate is laterally surrounded by the first dielectric layer, the first insulating layer and the second insulating layer; wherein the interconnect body and the first conductive trace are separated by the second dielectric layer; and The step of forming the interconnect body on the interconnect substrate comprises: forming a first barrier layer in direct contact with the interconnect substrate and the sidewalls of the second dielectric layer; forming a first copper-phosphorus alloy layer; forming at least one conductive layer surrounded by the barrier layer, wherein the first copper-phosphorus alloy layer is sandwiched between the first barrier layer and the at least one conductive layer; forming a second copper-phosphorus alloy layer on the at least one conductive layer; as well as A second barrier layer is formed on the second copper-phosphorus alloy layer.

16. The method of claim 15, wherein a dielectric constant of the first dielectric layer is smaller than dielectric constants of the first insulating layer and the second insulating layer.

17. The method of claim 15, wherein the operation of forming at least one conductive material on the photoresist layer, the second insulating layer and the conductive line comprises: forming a barrier layer in the base region, wherein the barrier layer is in contact with one side of the first insulating layer and one side of the second insulating layer; forming a copper-phosphorus alloy layer on the barrier layer; and A copper layer is plated on the copper-phosphorus alloy layer.

18. The method of claim 17, wherein said operation of plating said copper layer on said copper-phosphorus alloy layer comprises: The copper layer is formed to have a predetermined thickness using electroplating or electroless plating so that a top surface of the second insulating layer formed in the substrate region and a top surface of the interconnect substrate are coplanar.

19. The method of claim 15, The first conductive trace overlaps the first dielectric layer along a stacking direction of the semiconductor structure.

20. The method of claim 15, further comprising: At least one dielectric is formed in the first conductive trace.

21. The method of claim 15, further comprising forming an N+1th metal layer comprising a plurality of conductive traces and a plurality of interconnect bodies having a total of q different thicknesses, wherein: q is an integer greater than 1; The plurality of conductive traces and the plurality of interconnect bodies are formed by q metal plating processes and q different lift-off processes, from conductive traces or interconnect bodies having the smallest thickness to conductive traces or interconnect bodies having the largest thickness.

22. The method of claim 15, wherein the semiconductor structure further comprises a plurality of interconnect substrates having p different thicknesses, p being an integer greater than 1, and the plurality of interconnect substrates are formed by p metal plating processes and p different lift-off processes, from an interconnect substrate having a minimum thickness to an interconnect substrate having a maximum thickness.

23. The method of claim 15, wherein the conductive lines include input / output electrodes of transistors formed in the wafer, and the method further comprises forming the input / output electrodes, comprising: forming an interlayer dielectric layer on a plurality of transistors formed in a substrate of the wafer; forming a first silicate glass layer on the interlayer dielectric layer; forming a first SiN layer on portions of the first silicate glass layer disposed on a plurality of first terminals of the plurality of transistors at a first depth; forming a second silicate glass layer on the first silicate glass layer and the first SiN layer; forming a second SiN layer on the second silicate glass layer; forming a plurality of first openings on a plurality of second terminals of the plurality of transistors at a second depth deeper than the first depth; depositing a first layer of electrode metal to fill the plurality of first openings; removing the exposed portion of the second silicate glass layer; forming a plurality of second openings on the plurality of first terminals of the plurality of transistors; depositing a second layer of electrode metal to fill the plurality of second openings; as well as removing the first SiN layer and the second SiN layer; The electrode metal comprises tungsten, cobalt, or ruthenium.

24. The method of claim 15, wherein the semiconductor structure further comprises a plurality of electrodes having r different thicknesses, r being an integer greater than 1, and the plurality of electrodes are formed by r metal plating processes and r stripping processes, from an electrode having a minimum thickness to an electrode having a maximum thickness.