A method for improving ferroelectric properties by refining the electric domain of ferroelectric materials through swing high pressure sintering
Through rocking high-pressure sintering technology, the problems of densification and grain growth control in the ferroelectric ceramic sintering process are solved, high density and optimized microstructure are achieved, and the ferroelectric and piezoelectric properties are significantly improved, providing PZT95/5 ceramics with Efficient and feasible preparation method.
Patent Information
- Application Number
- CN202410243131.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-04
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-03-04
AI Technical Summary
The existing ferroelectric ceramic sintering process is difficult to achieve high density and fine microstructure, resulting in poor performance of PZT95/5 ceramics. In particular, abnormal grain growth and increased zirconium ion content make densification sintering more difficult and affect material performance.
The rocking high-pressure sintering method is adopted, and through wet ball milling and rocking oscillation sintering technology, the sintering parameters are precisely controlled, the grain growth is suppressed, the microstructure of the ceramic is optimized, and the density and ferroelectric properties are improved.
The ferroelectric performance is significantly improved, the residual polarization strength is increased by 40%, and the piezoelectric performance is increased by 30%, and provides a feasible way to prepare high-performance ferroelectric ceramics on a large scale.
Smart Images

Figure CN118145994B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ferroelectric ceramics, and more specifically, the present invention relates to a method for improving ferroelectric performance by refining the electric domain of ferroelectric materials through swing high-pressure sintering. Background Art
[0002] Lead zirconate titanate (PZT) ceramics are a solid solution composed of lead zirconate (PbZrO3) and lead titanate (PbTiO3), and are an important functional ceramic material. Due to its advantages such as high electromechanical coupling coefficient, high Curie temperature, easy polarization and wide dielectric constant range, it has been widely used in medical imaging, electronic communications, energy technology, aerospace and defense industries. Among them, PZT95 / 5 ceramic materials refer to the general term for piezoelectric ceramic materials with a zirconium-titanium ratio (Zr / Ti) of around 95 / 5. The polarized PZT95 / 5 ceramics can be transformed from a metastable ferroelectric phase to an antiferroelectric phase under low impact pressure, and can instantly release bound charges and output pulse currents. It is the core functional material for the preparation of explosively induced charge storage devices.
[0003] However, the sintering preparation of ceramics is a complex physical and chemical process, and different sintering processes have a significant impact on the performance of ferroelectric ceramics. From a thermodynamic point of view, sintering is a process in which the total energy of the system is reduced. Its essence is atomic diffusion, grain boundary network formation, gas phase elimination and grain connection, etc., which results in powder densification aggregation and grain growth. The sintering process parameters and powder size differences will significantly affect the density and grain size. This is because as the sintered body gradually becomes denser, the volume diffusion is too slow to eliminate the isolated (inside the grain) pores within the sintering time, so the position and size of the pores will become a more critical factor affecting the performance of the sintered body. In addition, differences in sintering processes will affect the migration process of the grain boundaries, leading to abnormal grain growth.
[0004] Commonly used ceramic sintering processes include hot pressing sintering, spark plasma sintering and pressureless sintering. Among them, hot pressing sintering helps to refine grains, reduce pores and the amount of additives used, and improve sintering density and sintering efficiency. However, hot pressing sintering has relatively high requirements for equipment. Excessive pressure or temperature will also cause abnormal growth of grains, which will damage the performance of the material. In the spark plasma sintering process, high-energy pulse current is introduced to activate the powder and the powder is formed and prepared through a series of processes such as thermoplastic deformation and cooling. During the preparation process, the product performance fluctuates greatly, and there are special requirements for the multifunctionality of power supply and equipment. Therefore, it does not meet the requirements of actual production applications. Atmospheric pressure sintering is currently an effective method for large-scale preparation of piezoelectric ceramics, but because the raw material powder is sintered under atmospheric pressure, and the high sintering temperature will cause abnormal growth of grains, resulting in poor performance. PZT95 / 5 ceramic powder is more difficult to sinter than ordinary PZT ceramics. Its lattice structure is stable, the powder activity is low, and the increase in the content of zirconium ions also increases the difficulty of densification sintering. In addition, PbO, one of the important raw materials, has a low melting point and is easy to volatilize, which will also affect its sintering performance. In order to obtain PZT ferroelectric ceramics with high density and fine microstructure, the sintering densification process needs to be decoupled from grain growth. Summary of the invention
[0005] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0006] In order to achieve these purposes and other advantages according to the present invention, a method for improving ferroelectric properties by refining the electric domain of ferroelectric materials by swinging high pressure sintering is provided, comprising the following steps:
[0007] Step 1, weighing the ferroelectric ceramic raw material powder, putting it into a ball mill, performing wet ball milling, pre-sintering, secondary grinding, pressing, and debinding to obtain a ferroelectric ceramic body;
[0008] Step 2, performing rocking oscillation sintering on the prepared ferroelectric ceramic body;
[0009] Step 3: polarize the ceramic sheet obtained by rocking oscillation sintering to obtain a ferroelectric ceramic with enhanced ferroelectric properties.
[0010] Preferably, the specific method of step 1 includes:
[0011] S11. Weigh titanium dioxide, zirconium dioxide, lead tetroxide and niobium pentoxide powders as ferroelectric ceramic raw material powders, use anhydrous ethanol as solvent and zirconium oxide as grinding balls, put the ferroelectric ceramic raw material powders into a ball mill for wet ball milling, wherein the mass fraction of titanium dioxide powder is 1.14%, the mass fraction of zirconium dioxide powder is 33.42%, the mass fraction of lead tetroxide powder is 65.24%, and the mass fraction of niobium pentoxide powder is 0.2%;
[0012] S12, sieving the ball-milled ceramic slurry and pouring it into a container, and drying it in a blast drying oven; pouring the dried ceramic raw material powder into a container, and drying it in a blast drying oven; pouring the dried ceramic raw material powder into a mortar for grinding, sieving it, and placing it in a crucible for pre-firing to obtain a ceramic block;
[0013] S13, grinding the pre-fired ceramic block for a second time, drying it, and sieving it;
[0014] S14, using a press to press the sieved ceramic powder into a round body;
[0015] S15, the specific method of debinding includes: heating from room temperature to a first temperature and keeping the temperature, then heating to a second temperature and keeping the temperature, cooling with the furnace to room temperature and taking out to obtain a ferroelectric ceramic body.
[0016] Preferably, in said S11, the mass ratio of the grinding balls, the ferroelectric ceramic raw material powder and the solvent is 1-2:1.5-3:0.5-1, the wet ball milling time is 12-36 hours, and the wet ball milling speed is 300-400 r / min.
[0017] Preferably, in said S12, the drying temperature is 60-100°C, the drying time is 24-60h, the sieving mesh number is 20-60 mesh, the pre-calcining temperature is 800-900°C, and the sintering time is 2-6h.
[0018] Preferably, in S13, the rotation speed of the secondary ball milling is 360-400 r / min, the secondary ball milling time is 6-24 h, and the sieve mesh number is 20-60 meshes.
[0019] Preferably, in said S14, the pressing pressure of the press is 6-15 MPa, the holding time is 5-20 s, the diameter of the circular blank is 20-40 mm, and the thickness is 1-2 mm.
[0020] Preferably, in S15, during binder removal, the temperature is raised from room temperature to 350-450°C at a heating rate of 5-20°C / min, kept warm for 20-40 minutes, and then raised to 800-900°C at the same heating rate, kept warm for 0.5-2 hours.
[0021] Preferably, the specific method in step 2 includes: setting the sintering temperature to be constant at a third temperature, setting the low pressure of the sintering pressure to be the first pressure, maintaining the pressure for a certain period of time, then increasing the pressure to the second pressure at a first pressure increase rate, maintaining the pressure for the same period of time, and then decreasing the pressure to the low first pressure at a first pressure reduction rate; repeating three cycles in sequence, then cooling with the furnace and taking out the sample.
[0022] Preferably, the third temperature is 1000-1200° C., the first pressure is 90-110 MPa, the holding time is 8-16 min, the first pressure increase rate is 15-25 MPa / min, the second pressure is 150-250 MPa, and the first pressure reduction rate is 15-25 MPa / min.
[0023] Preferably, in the step three, the specific method for polarizing the ceramic sheet obtained by rocking oscillation sintering includes: placing the ceramic sheet in dimethyl silicone oil, heating it to 80-120°C, keeping it warm for 20-40 minutes and applying a DC voltage with an electric field strength of 3 times the coercive field, maintaining the voltage during the cooling process, turning off the polarization voltage when it drops to room temperature, taking out the ceramic sheet, and leaving it for one day so that the charge on the ceramic surface can be fully released.
[0024] The present invention includes at least the following beneficial effects: The present invention successfully optimizes the technical difficulties in the preparation of traditional PZT95 / 5 ceramics by introducing a swinging high-pressure sintering method. This method achieves coordinated control of densification and inhibition of grain growth by precisely controlling the sintering parameters, optimizes the microstructure of the ceramic, and improves the density. Not only does it significantly improve the ferroelectric properties, the residual polarization strength is increased by 40% compared to traditional pressure sintering, but it also achieves an improvement of about 30% in piezoelectric properties, making the ceramic perform better in electrical properties. This innovative preparation method not only effectively solves the challenges brought about by the particularity of PZT95 / 5 ceramics, but also provides an efficient and feasible way for the large-scale preparation of high-performance ferroelectric ceramics, and has broad application prospects.
[0025] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Comparison of pressure curves between conventional pressure sintering and the rocking pressure sintering used in Example 1. DETAILED DESCRIPTION
[0027] The present invention will be further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0028] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0029] Example 1
[0030] This embodiment provides a method for improving ferroelectric performance by refining the electric domain of a ferroelectric material by swinging high pressure sintering, comprising the following steps:
[0031] Step 1, weighing the ferroelectric ceramic raw material powder, putting it into a ball mill, performing wet ball milling, pre-sintering, secondary grinding, pressing, and debinding to obtain a ferroelectric ceramic body; the specific method includes:
[0032] S11. First, an electronic scale is used to weigh TiO2, ZrO2, Pb3O4 and Nb2O5 powders, and the ingredients are prepared according to the stoichiometric ratio of the product, wherein the mass fraction of TiO2 powder is 1.14%, the mass fraction of ZrO2 powder is 33.42%, the mass fraction of Pb3O4 is 65.24%, and the mass fraction of Nb2O5 powder is 0.2%. Anhydrous ethanol is used as a solvent, and the ratio of grinding ball: ferroelectric ceramic raw material powder: solvent is 1:1.5:0.6. The raw materials are placed in a ball mill prepared in advance, zirconium oxide is used as a grinding ball, and wet ball milling is performed for 24 hours at a rotation speed of 350r / min.
[0033] S12, the ceramic slurry after ball milling is sieved and poured into a container, and the temperature is still maintained at 80° C. for 48 hours in a blast drying oven; the dried material is poured into a mortar and manually ground, passed through a 40-mesh sieve, and placed in a crucible to select a suitable temperature for pre-sintering, and the pre-sintering condition is sintering at 850° C. for 3 hours;
[0034] S13, crushing and grinding the pre-burned block, putting it into a ball mill for secondary grinding, ball milling at 400r / min for 12h, and then drying it, and weighing it through a 40-mesh sieve;
[0035] S14, using a press to maintain pressure at 10 MPa for 10 seconds to form a circular blank with a diameter of 30 mm and a thickness of about 1.5 mm;
[0036] S15, perform debinding treatment, heat from room temperature to 380°C at a rate of 10°C / min and keep the temperature for 30 minutes, then heat to 850°C at the same rate and keep the temperature for 1 hour, cool to room temperature and take out;
[0037] Step 2, the prepared ferroelectric ceramic body is subjected to rocking oscillation sintering; the sintering temperature is set to be constant at 1100°C, the low pressure of the sintering pressure is 100MPa, the pressure holding time is 10min, and then the pressure is increased to 300MPa at a pressure increasing rate of 20MPa / min, and the pressure is also held for 10min, and then the pressure is reduced to a low pressure of 100MPa at a pressure reducing rate of 20MPa / min; three cycles are repeated in sequence, and then the sample is taken out after cooling with the furnace; the sintered sample is pre-grinded, and the hysteresis loop of the sintered sample is measured using a ferroelectric analyzer, and the residual polarization intensity and other parameters of the sample are measured by measuring the hysteresis loop and other information.
[0038] Step 3: polarize the ceramic sheet obtained by rocking oscillation sintering. Place the ceramic sheet in dimethyl silicone oil, heat it to 100°C, keep it warm for 30 minutes and apply a DC voltage. The electric field strength is about 3 times the coercive field, and the applied electric field is 3000V / mm. Maintain the voltage during the cooling process. When it drops to room temperature, turn off the polarization voltage and take out the ceramic sheet. Place it for one day to fully release the charge on the ceramic surface before testing the piezoelectric performance to obtain PZT95 / 5 ferroelectric ceramics with enhanced ferroelectric performance.
[0039] Example 2
[0040] This embodiment provides a method for improving ferroelectric properties by refining the electric domains of ferroelectric materials through swing oscillation sintering. The difference from Embodiment 1 is that the low pressure of the swing oscillation sintering in step 2 is 150MPa, the high pressure is 250Mpa, the pressure holding time is 5min, and the rest of the process is the same as Embodiment 1.
[0041] Example 3
[0042] This embodiment provides a method for improving ferroelectric properties by refining the electric domains of ferroelectric materials through swinging high-pressure sintering. The difference from Example 1 is that the low pressure of the swinging oscillation sintering in step 2 is 100 MPa, the high pressure is 250 MPa, the pressure holding time is 5 minutes, and the rest of the process is the same as Example 1.
[0043] Example 4
[0044] This embodiment provides a method for improving ferroelectric properties by refining the electric domains of ferroelectric materials through swing high-pressure sintering. The difference from Embodiment 1 is that the low pressure of the swing oscillation sintering in step 2 is 200 MPa, and the rest of the process is the same as Embodiment 1.
[0045] Comparative Example 1
[0046] This comparative example provides a method for improving ferroelectric properties by refining the electric domains of ferroelectric materials through traditional high-pressure sintering. The difference from Example 1 is that the sintering pressure in step 2 of this comparative example is constant at 150 MPa, the sintering time is 60 min, and the rest of the process is the same as Example 1.
[0047] Comparative Example 2
[0048] This comparative example provides a method for improving ferroelectric properties by refining the electric domains of ferroelectric materials through traditional high-pressure sintering. The difference from Example 1 is that the sintering pressure in step 2 of this comparative example is constant at 250 MPa, the sintering time is 60 min, and the rest of the process is the same as Example 1.
[0049] Comparative Example 3
[0050] This comparative example provides a method for improving ferroelectric properties by refining the electric domains of ferroelectric materials through traditional high-pressure sintering. The difference from Example 1 is that the sintering pressure in step 2 of this comparative example is constant at 300 MPa, the sintering time is 60 min, and the rest of the process is the same as Example 1.
[0051] The residual polarization intensity and piezoelectric performance of the PZT95 / 5 ferroelectric ceramics prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were tested respectively, and the following table was obtained:
[0052]
[0053]
[0054] It can be seen from the above table that compared with the traditional pressure sintering method used in Comparative Examples 1 to 3, the PZT95 / 5 ferroelectric ceramics obtained by the rocking oscillation pressure change sintering method used in Examples 1 to 4 have greater residual polarization intensity and piezoelectric coefficient.
[0055] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.
[0056] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A method for improving ferroelectric properties by refining the electric domain of ferroelectric materials by swinging high pressure sintering, characterized in that: The following steps are involved: Step 1, weighing the ferroelectric ceramic raw material powder, putting it into a ball mill, performing wet ball milling, pre-sintering, secondary grinding, pressing, and debinding to obtain a ferroelectric ceramic body; Step 2, performing rocking oscillation sintering on the prepared ferroelectric ceramic body; Step 3, polarizing the ceramic sheet obtained by the rocking oscillation sintering to obtain a ferroelectric ceramic with enhanced ferroelectric properties; The specific method of step one includes: S11. Weigh titanium dioxide, zirconium dioxide, lead tetroxide and niobium pentoxide powders as ferroelectric ceramic raw material powders, use anhydrous ethanol as solvent and zirconium oxide as grinding balls, and put the ferroelectric ceramic raw material powders into a ball mill for wet ball milling; wherein the mass fraction of titanium dioxide powder is 1.14%, the mass fraction of zirconium dioxide powder is 33.42%, the mass fraction of lead tetroxide powder is 65.24%, and the mass fraction of niobium pentoxide powder is 0.2%; S12, sieving the ball-milled ceramic slurry and pouring it into a container, and drying it in a blast drying oven; pouring the dried ceramic raw material powder into a container, and drying it in a blast drying oven; pouring the dried ceramic raw material powder into a mortar for grinding, sieving it, and placing it in a crucible for pre-firing to obtain a ceramic block; S13, grinding the pre-fired ceramic block for a second time, drying it, and sieving it; S14, using a press to press the sieved ceramic powder into a round body; S15, the specific method of debinding includes: heating from room temperature to a first temperature, and keeping the temperature, then heating to a second temperature, and keeping the temperature, cooling to room temperature with the furnace, and taking out to obtain a ferroelectric ceramic body; In S11, the mass ratio of the grinding balls, the ferroelectric ceramic raw material powder and the solvent is 1-2:1.5-3:0.5-1, the wet ball milling time is 12-36 hours, and the wet ball milling speed is 300-400 r / min; In S13, the rotation speed of the secondary ball milling is 360-400 r / min, the secondary ball milling time is 6-24 h, and the sieve mesh number is 20-60 mesh; In S14, the pressing pressure of the press is 6-15 MPa, the holding time is 5-20 s, the diameter of the circular blank is 20-40 mm, and the thickness is 1-2 mm; In S15, during debinding, the temperature is raised from room temperature to 350-450°C at a heating rate of 5-20°C / min, and kept at that temperature for 20-40min, and then raised to 800-900°C at the same heating rate, and kept at that temperature for 0.5-2h; The specific method in step 2 includes: setting the sintering temperature to be constant at the third temperature, the low pressure of the sintering pressure to be the first pressure, maintaining the pressure for a certain time, then increasing the pressure to the second pressure at a first pressure increasing speed, maintaining the pressure for the same time, and then decreasing the pressure to the low pressure first pressure at a first pressure decreasing speed; repeating three cycles in sequence, then cooling with the furnace, and taking out the sample; The third temperature is 1000-1200° C., the first pressure is 90-110 MPa, the holding time is 8-16 min, the first pressure increasing speed is 15-25 MPa / min, the second pressure is 150-250 MPa, and the first pressure reducing speed is 15-25 MPa / min; In the step three, the specific method for polarizing the ceramic sheet obtained by rocking oscillation sintering includes: placing the ceramic sheet in dimethyl silicone oil, heating it to 80-120°C, keeping it warm for 20-40 minutes and applying a DC voltage with an electric field strength of 3 times the coercive field, maintaining the voltage during the cooling process, turning off the polarization voltage when it drops to room temperature, taking out the ceramic sheet, and leaving it for one day to allow the charge on the ceramic surface to be fully released.
2. The method for improving ferroelectric properties by refining the electric domain of ferroelectric materials by swing high pressure sintering as claimed in claim 1, characterized in that: In the S12, the drying temperature is 60-100°C, the drying time is 24-60h, the sieving mesh is 20-60 mesh, the pre-calcining temperature is 800-900°C, and the sintering time is 2-6h.