A pre-lithium or pre-sodium electrode and preparation method thereof, and battery

By using pre-lithium or pre-sodium electrodes with a 'sandwich' structure in lithium or sodium-ion batteries, and using encapsulation films and modified current collector layers to improve the environmental adaptability and adhesion of the electrodes, the high cost of lithium or sodium-ion batteries is solved. , the problems of low energy density and short cycle life have been achieved, and the energy density and dynamic performance have been improved.

CN118173712BActive Publication Date: 2024-10-22HENAN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410586793.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-13
Publication Date
2024-10-22
Estimated Expiration
2044-05-13

AI Technical Summary

Technical Problem

Lithium or sodium-ion batteries have high cost, low energy density, low kinetic performance and short cycle life. The existing pre-lithium additives have poor chemical stability in conventional environments, and the silicone-based materials circulating on the market have poor chemical stability in aqueous slurry systems. Being alkaline, it destroys the structure of adhesives such as polyacrylic acid and reduces the structural stability of molded electrodes.

Method used

Pre-lithium or pre-sodium electrodes with a 'sandwich' structure are used. The surface layer is a pre-lithium or pre-sodium encapsulation film, the middle layer is a pre-lithium or pre-sodium negative electrode, and the bottom layer is a modified current collector layer. Through dry or wet methods In the electrode process preparation, materials such as LiF, NaF, organic fluoride and PEG are used to form an encapsulation film to improve environmental adaptability, and the adhesion of the current collector layer is improved through spraying or evaporation processes.

Benefits of technology

It significantly improves the energy density, kinetic performance and cycle life of lithium or sodium-ion batteries, reduces production costs, avoids the reaction of pre-lithium components and slurry solvents, and enhances the structural stability and environmental stability of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118173712B_ABST
    Figure CN118173712B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium or sodium ion batteries, and specifically provides a pre-lithium or pre-sodium electrode and a preparation method and battery thereof. The novel pre-lithium or pre-sodium electrode has a "sandwich" structure, and the surface layer of the electrode is a packaging film of the pre-lithium or pre-sodium electrode, and the main components are LiF (or NaF) and polymerized high molecular fluoride, etc., and have good chemical inertness and structural stability; the middle layer of the electrode is a pre-lithium or pre-sodium negative electrode, which is achieved by rolling lithium or sodium foil or solvated pre-lithium or pre-sodium, and the degree of pre-lithium or pre-sodium is deep, the lithium or sodium ion / electron channels inside the active material are sufficient, and the kinetic and structural stability performance is good; the bottom layer of the electrode is a modified current collector thin layer obtained by spraying or evaporation and other processes, which has the advantages of light weight and high bonding strength. The pre-lithium or pre-sodium electrode has excellent cycle structural stability performance, and improves the first coulomb efficiency, energy density and kinetic performance of lithium or sodium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of negative electrodes of lithium or sodium ion batteries, and in particular relates to a pre-lithium or pre-sodium electrode and a preparation method thereof, and a battery. Background Art

[0002] It has become a consensus among countries around the world that new energy vehicles will replace traditional fuel vehicles, and power batteries have become the main driving force for the rapid growth of China's lithium-ion battery demand. For example, in 2022, China's electric vehicle sales will be 6.887 million units, and the installed capacity of lithium-ion batteries will be 750 GWh, up 95.6% and 126% year-on-year respectively. At the same time, the energy density of sodium-ion batteries is between lithium-ion batteries and lead-acid batteries, but the cost and cycle life are superior to lithium-ion batteries. Therefore, sodium-ion batteries can be used in large-scale energy storage and low-speed transportation fields (such as A00-class and two-wheeled vehicles) to fill the market gap of lithium-ion batteries. Gaogong Industry Research Institute (GGII) predicts that China's sodium-ion battery landing capacity will exceed 15 GWh in 2023, and the landing capacity will exceed 60GWh in 2025, and the market size will reach 30 billion yuan by then. Therefore, it is necessary to accelerate the exploration of new lithium-ion batteries and sodium-ion batteries in the future, and ensure the autonomy of technology and intellectual property rights, which is in line with the needs of cascade utilization of resources. However, the large-scale industrialization of energy storage devices and electric vehicles still faces challenges such as "charging anxiety", "mileage anxiety" and "cost reduction and efficiency improvement". Among them, how to significantly improve the energy density, kinetic performance and cycle life of lithium or sodium ion batteries has attracted much attention from researchers.

[0003] "The dry process of positive and negative electrodes can greatly improve the energy density of lithium or sodium batteries. Pre-lithium will become a milestone in the development history of new energy vehicles. The dry electrode process and pre-lithium or pre-sodium are new breakthroughs in the production and application technology of power batteries." For example, in the traditional "wet coating process" electrode system, the high energy density and high cost performance of lithium batteries are usually not effectively taken into account at the same time, but the transformation of the dry electrode process can make the energy density of lithium-ion batteries reach 350-400 Wh / Kg, an increase of 20% year-on-year, and a 20% reduction in cost. Prior art CN117352662B discloses a dry electrode manufacturing method, an electrode sheet and a battery. Compared with the traditional wet electrode process, the technical solution can effectively achieve the purpose of "reducing costs and increasing efficiency". At the same time, compared with the conventional 7 μm copper foil current collector of commercial lithium or sodium ion batteries, the current collector of the negative electrode can be used as a vapor deposition, thin copper or liquid metal coating to reduce the quality and production cost of lithium or sodium ion batteries, improve the adhesion between the negative electrode active material of lithium or sodium ion batteries and the current collector, and improve the energy density and service life of the battery. In addition, in order to meet consumers' urgent needs for energy storage power stations and the continuous improvement of electric vehicle mileage and service life, the development of pre-lithium or pre-sodium technology for lithium or sodium ion batteries has also aroused great interest in the scientific and industrial communities. For example, Cui Yi and his collaborators prepared a Li-ion battery with a "core-shell" structure through "hot melt-ball milling" and other methods. x Si@Li2O negative electrode material, Li x Si@Li2O material is used as a pre-lithium additive for commercial graphite and silicon-carbon negative electrodes. The first coulombic efficiency and energy density of the two lithium-ion batteries can be increased to 100% and 94%, respectively, which significantly improves the energy density and cycle life of the battery. However, the commercial graphite and silicon-carbon negative electrodes containing pre-lithium additives have poor chemical stability in conventional environments and are not suitable for the production environment of lithium-ion batteries. At the same time, although the pre-lithium silicon-based materials currently circulating on the market have high environmental stability in conventional environments, they have low pre-lithium degrees and are alkaline in aqueous slurry systems, which destroy the structure of adhesives such as polyacrylic acid and reduce the structural stability of the formed electrode. Therefore, their application in the lithium-ion battery market is limited. Therefore, in view of the above problems, it is necessary to develop a pre-lithium or pre-sodium electrode and its preparation method and battery, which is crucial for the development of high-performance lithium or sodium-ion batteries in the future. Summary of the invention

[0004] In view of the limitations of current lithium or sodium ion batteries such as high cost, low energy density, low kinetic performance, and short cycle life, the present invention provides a pre-lithium or pre-sodium electrode. Furthermore, the present invention also provides a preparation method containing the novel pre-lithium or pre-sodium electrode, and a lithium or sodium composite battery thereof.

[0005] To achieve the above-mentioned object of the invention, the technical solution of the present invention is as follows:

[0006] The first aspect of the present invention provides a pre-lithium or pre-sodium electrode, which has a "sandwich" structure, wherein the surface layer is a packaging film of the pre-lithium or pre-sodium electrode, which can isolate the reaction of the pre-lithium active material inside the electrode from the surrounding environment, thereby improving the environmental adaptability of the new electrode; the middle layer is a pre-lithium or pre-sodium negative electrode, and the bottom layer is a modified current collector layer.

[0007] Preferably, the surface packaging film raw materials of the pre-lithium or pre-sodium electrode include one or more of LiF, NaF, and organic fluorides, and the packaging film thickness is 0.1-2 µm; the electrode intermediate layer pre-lithium or pre-sodium negative electrode is prepared by a dry electrode process or a wet electrode process, and the thickness of the pre-lithium or pre-sodium negative electrode is 20-50 µm; the modified current collector layer of the electrode includes one of a copper coating, a liquid metal coating, a traditional copper foil and a coated copper foil, and the thickness is 0.1-10 µm.

[0008] Preferably, the pre-lithium or pre-sodium object of the pre-lithium or pre-sodium electrode includes one or more of silicon-carbon materials, silicon-based materials, graphite materials, silicon-carbon / graphite composite materials, silicon-based / graphite composite materials, lithium titanate or hard carbon-based materials.

[0009] Preferably, the organic fluoride comprises PFPE (perfluoropolyether) with a molecular weight of 2000-5000.

[0010] Preferably, the raw material of the encapsulation film also includes PEG (polyethylene glycol) with a molecular weight of 500-2000.

[0011] Preferably, the packaging film of the novel pre-lithium or pre-sodium electrode is obtained by reacting PFPE, PEG on lithium or sodium metal, lithium or sodium carbon or lithium silicon particles, and then self-polymerizing; the pre-lithium or pre-sodium negative electrode is obtained by co-rolling lithium or sodium foil with graphite, hard carbon-based, silicon-carbon, silicon-oxygen, silicon-carbon / graphite composite, silicon-oxygen / graphite composite electrodes; or by solvating pre-lithium or pre-sodium with graphite, hard carbon-based, silicon-carbon, silicon-oxygen, silicon-carbon / graphite composite, silicon-oxygen / graphite composite electrodes; the modified current collector layer of the electrode is prepared by spraying liquid metal, evaporating copper coating, or rolling conventional copper foil current collector.

[0012] A second aspect of the present invention provides a method for preparing a pre-lithium or pre-sodium electrode, comprising at least the following steps:

[0013] S01. Obtain silicon-carbon ‖ copper foil, silicon-oxygen ‖ copper foil, graphite ‖ copper foil, silicon-carbon / graphite ‖ copper foil, silicon-oxygen / graphite ‖ copper foil, and hard carbon-based ‖ copper foil negative electrodes through a wet electrode process;

[0014] Or silicon-carbon ‖ copper coating, silicon-oxygen ‖ copper coating, graphite ‖ copper coating, silicon-carbon / graphite ‖ copper foil, silicon-oxygen / graphite ‖ copper foil and hard carbon-based ‖ copper coating negative electrode, silicon-carbon ‖ liquid metal coating, silicon-oxygen-carbon ‖ liquid metal coating, graphite ‖ liquid metal coating, silicon-carbon / graphite ‖ liquid metal, silicon-oxygen / graphite ‖ liquid metal, hard carbon ‖ liquid metal coating negative electrode obtained by one or more processes of dry electrode process, evaporation and spraying;

[0015] S02, fully mixing PEG, PFPE and a photoinitiator by stirring to form PEG-PFPE, and then evenly coating the PEG-PFPE on the PET film by spraying or brushing, and then compounding a layer of lithium or sodium metal film to form a Li or Na ‖ PEG-PFPE ‖ PET composite film;

[0016] S03, laminating the metal side of the Li or Na||PEG-PFPE||PET composite film and the negative electrode described in S01, adjusting the roller spacing so that the two are rolled together, the negative electrode described in S01 will undergo a pre-lithium or pre-sodium reaction under the action of lithium or sodium metal, and the PEG-PFPE coating will chemically react with lithium or sodium metal, lithium silicon or lithium or sodium carbon to form an encapsulation film;

[0017] S04. Remove the outer PET film, adjust the wavelength, light intensity and illumination time of the ultraviolet light to treat the electrode surface, so that PEG and lithium or sodium PFPE undergo cross-linking and self-polymerization reaction, thereby obtaining a pre-lithium or pre-sodium electrode with surface encapsulation and composite structure.

[0018] Preferably, the thickness of the pre-lithium or pre-sodium negative electrode layer in the S01 is 20-50 μm.

[0019] Preferably, the modified current collector layer is one of a copper coating, a liquid metal coating, a traditional copper foil and a coated copper foil, and has a thickness of 0.1 - 10 µm.

[0020] Further preferably, the liquid metal in the liquid metal coating comprises Ga, In, Sn in a mass ratio of (0-10):(0-10):(0-10).

[0021] Preferably, the mass ratio of PEG to PFPE in the S02 is (0-10): (0-10), the thickness of the PEG-PFPE coating is adjusted to 0.1 - 2 μm, the amount of photoinitiator benzoin added is 5-50 μL, and the thickness of the lithium or sodium metal layer is 0.1 - 50 μm.

[0022] Preferably, the wavelength of the ultraviolet light in S04 is 100-1000 nm, and the light intensity is 50-500 mW / cm 2, the illumination time is 1 - 60 min.

[0023] The third aspect of the present invention provides a lithium or sodium battery comprising the pre-lithium or pre-sodium electrode, including a pre-lithium or pre-sodium negative electrode and surface packaging technology prepared by a conventional wet coating process, and also including a self-supporting structure pre-lithium negative electrode and surface packaging technology obtained by a dry electrode process.

[0024] Beneficial Effects

[0025] (i) The present invention reduces the mass of the battery and the amount of copper used by applying a thin coating of copper or liquid metal, compared to commercial 7 μm copper current collectors, thereby reducing the production cost of the battery and improving the energy density of the battery.

[0026] (ii) Compared with the commercial 7 μm copper current collector, the thin coating of copper or liquid metal applied by the present invention improves the bonding effect between the active material and the current collector, and also improves the cycle life of the battery.

[0027] (III) During the electrode forming process of commercial pre-lithium powder materials, the problem of residual alkali damaging the adhesive and electrode structure often occurs. The pre-lithium or pre-sodium composite electrode described in the present invention has obvious advantages such as high degree of pre-lithium or pre-sodium and integrity of electrode structure.

[0028] (iv) Compared with the conventional method of adding pre-lithium or pre-sodium additive powder or rolling lithium or sodium foil, the pre-lithium or pre-sodium electrode surface encapsulation film process described in the present invention can effectively avoid the reaction of the pre-lithium or pre-sodium components with the slurry solvent, or the poor stability of the pre-lithium or pre-sodium electrode in a conventional environment.

[0029] (V) The pre-lithium or pre-sodium electrode and its preparation method and battery described in the present invention have a simple process flow and a wide range of applications. First, obtain a negative electrode current collector prepared by a traditional wet process, or a self-supporting negative electrode containing a copper or liquid metal coating prepared by a dry electrode process; then, design a Li or Na‖PEG-PFPE‖PET composite film with a "sandwich" structure, and the middle layer contains a small amount of photoinitiator; finally, roll the composite film together with the obtained negative electrode, and the active material will undergo a pre-lithium or pre-sodium reaction under pressure, remove the PET film and induce a photo-initiated polymerization reaction to obtain a dense packaging film. Based on this, a new electrode with a pre-lithium or pre-sodium packaging film and a composite modified current collector can be obtained, which can improve the energy density, kinetic performance and cycle life of lithium or sodium ion batteries, reduce the production cost of batteries, and achieve the effect of "reducing costs and increasing efficiency".

[0030] (vi) The battery provided by the present invention, including the pre-lithium or pre-sodium electrode, has a large surface loading of active materials and a deep pre-lithium degree, a low production cost, excellent environmental and structural stability, and excellent lithium or sodium ion / electron transport kinetics. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram of the structure of the pre-lithium electrode of Example 1 of the present invention, wherein: 1-encapsulation film, 2-pre-lithium electrode, 3-modified current collector layer.

[0032] Figure 2 This is the first charge and discharge curve of the new pre-lithium graphite composite negative electrode with a "sandwich" structure prepared in Example 1.

[0033] Figure 3 This is the first charge and discharge curve of the new pre-lithium silicon-carbon composite negative electrode with a "sandwich" structure prepared in Example 2.

[0034] Figure 4 This is the first charge and discharge curve of the new pre-lithium silicon-oxygen-carbon composite negative electrode with a "sandwich" structure prepared in Example 3.

[0035] Figure 5 This is the first charge and discharge curve of the new pre-sodium hard carbon composite negative electrode with a "sandwich" structure prepared in Example 4.

[0036] Figure 6 This is a scanning electron microscope image of the surface of the novel pre-lithium graphite composite negative electrode with a "sandwich" structure prepared in Example 1.

[0037] Figure 7 This is a scanning electron microscope image of the surface of the novel pre-lithium silicon-carbon composite negative electrode with a "sandwich" structure prepared in Example 2, wherein Figure 7 The scale bar in (a) is 50 μm, and the scale bar in 7(b) is 10 μm.

[0038] Figure 8 This is a scanning electron microscope image of the surface of the novel pre-lithium silicon-oxygen-carbon composite negative electrode with a "sandwich" structure prepared in Example 3; wherein Figure 8 The scale bar in (a) is 50 μm, and the scale bar in (b) is 30 μm.

[0039] Fig. 9 This is a scanning electron microscope image of the surface of the new pre-sodium hard carbon composite negative electrode with a "sandwich" structure prepared in Example 4. DETAILED DESCRIPTION

[0040] Example 1

[0041] In the first aspect of this example, a pre-lithium electrode is provided, which has a "sandwich" structure. The surface layer is the packaging film of the pre-lithium electrode, which is 0.5μm thick and is composed of a lithium polymer of LiF and PEG-PFPE; the middle layer is a pre-lithium negative electrode prepared by a wet electrode process, which is 20μm thick, and the pre-lithium object is graphite. The bottom layer is a modified current collector layer, which is 10μm thick and is specifically a copper coating obtained by evaporation.

[0042] The second aspect of this example provides a method for preparing a pre-lithium electrode, which specifically comprises the following steps:

[0043] S01, through the combination of wet electrode process and roller pressing process, the negative electrode of graphite ‖ copper foil is obtained;

[0044] S02. PEG, PFPE and photoinitiator benzoin are fully mixed and uniformly formed into PEG-PFPE by stirring, and then PEG-PFPE is uniformly coated on the PET film by spraying, and then a layer of lithium metal film is compounded to form a Li‖PEG-PFPE‖PET composite film; wherein the mass ratio of PEG to PFPE is 1:1, the thickness of the PEG-PFPE coating is adjusted to 0.5 μm, the amount of photoinitiator benzoin added is 5 μL, and the thickness of the lithium metal layer is 10 μm;

[0045] S03, laminating the metal side of the Li|PEG-PFPE|PET composite film and the graphite|copper foil negative electrode described in S01, adjusting the roller spacing so that the two are rolled together; in this process, the graphite|copper foil negative electrode will undergo a pre-lithium reaction under the action of lithium metal, and at the same time, the PEG-PFPE coating will chemically react with lithium metal and lithium carbon to form an encapsulation film to isolate the active ingredients from small molecules such as water samples in the environment to avoid failure reactions;

[0046] S04, remove the outer PET film, adjust the wavelength, light intensity and illumination time of ultraviolet light to treat the electrode surface, where the wavelength of ultraviolet light is 200 nm and the light intensity is 200 mW / cm 2 The illumination time is 30 min, so that PEG and lithiated PFPE undergo cross-linking and self-polymerization reactions, thereby improving the compactness of the encapsulation film and the environmental stability of the pre-lithium electrode, thereby obtaining a pre-lithium graphite composite electrode.

[0047] The molecular weight of the organic fluoride PFPE is 2000-5000.

[0048] The molecular weight of the PEG is 500-2000.

[0049] The third aspect of this example provides a lithium battery comprising the pre-lithium graphite composite electrode described in Example 1.

[0050] Figure 1 This is a schematic diagram of the structure of the pre-lithium electrode of Example 1, wherein: 1- packaging film, 2- pre-lithium electrode, 3- modified current collector layer.

[0051] Figure 2 This is the first charge and discharge curve of the new pre-lithium graphite composite negative electrode with a "sandwich" structure prepared in Example 1.

[0052] Figure 6 This is a scanning electron microscope image of the surface of the novel pre-lithium graphite composite negative electrode with a "sandwich" structure prepared in Example 1.

[0053] Example 2

[0054] In the first aspect of this example, a pre-lithium electrode is provided, which has a "sandwich" structure. The surface layer is the packaging film of the pre-lithium electrode, which is 1 μm thick and is composed of a lithium polymer of LiF and PEG-PFPE; the middle layer is a pre-lithium negative electrode prepared by a dry electrode process, which is 30 μm thick, and the pre-lithium object is silicon carbon; the bottom layer is a modified current collector layer, which is 2 μm thick and is specifically a copper coating obtained by evaporation.

[0055] The second aspect of this example provides a method for preparing a pre-lithium electrode, which specifically comprises the following steps:

[0056] S01, through the dry electrode process and the evaporation process, the negative electrode of silicon carbon ‖ copper foil is obtained;

[0057] S02. PEG, PFPE and photoinitiator benzoin are fully mixed and uniformly formed into PEG-PFPE by stirring, and then PEG-PFPE is uniformly coated on the PET film by spraying, and then a layer of lithium metal film is compounded to form a Li‖PEG-PFPE‖PET composite film; wherein the mass ratio of PEG to PFPE is 2:1, the thickness of the PEG-PFPE coating is adjusted to 1 μm, the amount of photoinitiator benzoin added is 10 μL, and the thickness of the lithium metal layer is 30 μm;

[0058] S03, laminating the metal side of the Li‖PEG-PFPE‖PET composite film and the silicon-carbon‖copper foil negative electrode described in S01, adjusting the roller spacing so that the two are rolled together; in this process, the silicon-carbon‖copper foil negative electrode will undergo a pre-lithium reaction under the action of lithium metal, and at the same time, the PEG-PFPE coating will chemically react with lithium metal and lithium silicon to form an encapsulation film to isolate the active ingredients from small molecules such as water samples in the environment to avoid failure reactions;

[0059] S04, remove the outer PET film, adjust the wavelength, light intensity and illumination time of ultraviolet light to treat the electrode surface, where the wavelength of ultraviolet light is 250 nm and the light intensity is 250 mW / cm 2 The illumination time is 40 min, so that PEG and lithiated PFPE undergo cross-linking and self-polymerization reactions, thereby improving the compactness of the encapsulation film and the environmental stability of the pre-lithium electrode, thereby obtaining a pre-lithium silicon-carbon composite electrode.

[0060] The molecular weight of the organic fluoride PFPE is 2000-5000.

[0061] The molecular weight of the PEG is 500-2000.

[0062] The third aspect of this example provides a lithium battery comprising the pre-lithium silicon-carbon composite electrode described in Example 2.

[0063] Figure 3 This is the first charge and discharge curve of the new pre-lithium graphite composite negative electrode with a "sandwich" structure prepared in Example 1.

[0064] Figure 7 This is a scanning electron microscope image of the surface of the novel pre-lithium graphite composite negative electrode with a "sandwich" structure prepared in Example 1; wherein Figure 7 The scale bar in (a) is 50 μm, and the scale bar in 7(b) is 10 μm.

[0065] Example 3

[0066] In the first aspect of this example, a pre-lithium electrode is provided, which has a "sandwich" structure. The surface layer is a packaging film of the pre-lithium electrode, which has a thickness of 2μm and is composed of a lithium polymer of LiF and PEG-PFPE; the middle layer is a pre-lithium negative electrode prepared by a dry electrode process, which has a thickness of 40μm, and the pre-lithium object is silicon oxygen carbon; the bottom layer is a modified current collector layer, which has a thickness of 2μm, specifically a liquid metal coating, and the liquid metal has a mass ratio of Ga:In:Sn=7:2:1, which is obtained by spraying.

[0067] The second aspect of this example provides a method for preparing a pre-lithium electrode, which specifically comprises the following steps:

[0068] S01. The negative electrode of silicon-oxygen-carbon liquid metal is prepared by combining the dry electrode process and the spraying process;

[0069] S02. PEG, PFPE and photoinitiator benzoin are fully mixed and uniformly formed into PEG-PFPE by stirring, and then PEG-PFPE is uniformly coated on the PET film by spraying, and then a layer of lithium metal film is compounded to form a Li‖PEG-PFPE‖PET composite film; wherein the mass ratio of PEG to PFPE is 3:1, the thickness of the PEG-PFPE coating is adjusted to 2 μm, the amount of photoinitiator benzoin added is 15 μL, and the thickness of the lithium metal layer is 35 μm;

[0070] S03, laminating the metal side of the Li‖PEG-PFPE‖PET composite film and the silicon oxygen carbon‖liquid metal negative electrode described in S01, adjusting the roller spacing so that the two are rolled together; in this process, the silicon oxygen carbon‖copper foil negative electrode will undergo a pre-lithium reaction under the action of lithium metal, and at the same time, the PEG-PFPE coating will chemically react with lithium metal and lithium silicon to form an encapsulation film to isolate the active ingredients from small molecules such as water samples in the environment to avoid failure reactions;

[0071] S04, remove the outer PET film, adjust the wavelength, light intensity and illumination time of ultraviolet light to treat the electrode surface, where the wavelength of ultraviolet light is 300 nm and the light intensity is 300 mW / cm 2 The illumination time is 50 min, so that PEG and lithiated PFPE undergo cross-linking and self-polymerization reactions, thereby improving the compactness of the encapsulation film and the environmental stability of the pre-lithium electrode, thereby obtaining a pre-lithium silicon-oxygen-carbon composite electrode.

[0072] The molecular weight of the organic fluoride PFPE is 2000-5000.

[0073] The molecular weight of the PEG is 500-2000.

[0074] The third aspect of this example provides a lithium battery comprising the pre-lithium silicon-oxygen-carbon composite electrode described in Example 3.

[0075] Figure 4 This is the first charge and discharge curve of the new pre-lithium graphite composite negative electrode with a "sandwich" structure prepared in Example 1.

[0076] Figure 8 This is a scanning electron microscope image of the surface of the novel pre-lithium graphite composite negative electrode with a "sandwich" structure prepared in Example 1; wherein Figure 8 The scale bar in (a) is 50 μm, and the scale bar in (b) is 30 μm.

[0077] Example 4

[0078] In the first aspect of this example, a pre-sodium electrode is provided, which has a "sandwich" structure. The surface layer is a packaging film of the pre-sodium electrode, which has a thickness of 2 μm and is composed of sodium polymers of NaF and PEG-PFPE; the middle layer is a pre-sodium negative electrode prepared by a dry electrode process, which has a thickness of 50 μm, and the pre-sodium object is hard carbon. The bottom layer is a modified current collector layer, which has a thickness of 2 μm and is specifically a liquid metal coating. The liquid metal has a mass ratio of Ga:In:Sn=6:2:2 and is obtained by spraying.

[0079] The second aspect of this example provides a method for preparing a pre-sodium electrode, which specifically comprises the following steps:

[0080] S01. The hard carbon ‖ liquid metal negative electrode is obtained by compounding the dry electrode process and the spraying process;

[0081] S02, PEG, PFPE and photoinitiator benzoin are fully mixed and uniformly formed by stirring to form PEG-PFPE, and then PEG-PFPE is uniformly coated on the PET film by spraying, and then a layer of sodium metal film is compounded to form a Na‖PEG-PFPE‖PET composite film; wherein the mass ratio of PEG to PFPE is 3:1, the thickness of the PEG-PFPE coating is adjusted to 2 μm, the amount of photoinitiator benzoin added is 20 μL, and the thickness of the sodium metal layer is 10 μm;

[0082] S03, laminating the metal side of the Na‖PEG-PFPE‖PET composite film and the hard carbon‖liquid metal negative electrode described in S01, adjusting the roller spacing so that the two are rolled together; in this process, the hard carbon‖liquid metal negative electrode will undergo a pre-sodium reaction under the action of sodium metal, and at the same time, the PEG-PFPE coating will chemically react with the sodium metal and sodium carbon to form an encapsulation film to isolate the active ingredients from small molecules such as water samples in the environment to avoid failure reactions;

[0083] S04, remove the outer PET film, adjust the wavelength, light intensity and illumination time of ultraviolet light to treat the electrode surface, where the wavelength of ultraviolet light is 400 nm and the light intensity is 400 mW / cm 2 The illumination time is 60 min, so that PEG and sodium-modified PFPE undergo cross-linking and self-polymerization reactions, thereby improving the density of the encapsulation film and the environmental stability of the pre-sodium electrode, thereby obtaining a pre-sodium hard carbon composite electrode.

[0084] The molecular weight of the organic fluoride PFPE is 2000-5000.

[0085] The molecular weight of the PEG is 500-2000.

[0086] The third aspect of this example provides a sodium battery comprising the pre-sodium hard carbon composite electrode described in Example 4.

[0087] Figure 5 This is the first charge and discharge curve of the new pre-sodium graphite composite negative electrode with a "sandwich" structure prepared in Example 1.

[0088] Fig. 9 This is a scanning electron microscope image of the surface of the new pre-sodium graphite composite negative electrode with a "sandwich" structure prepared in Example 1.

Claims

1. A pre-lithium or pre-sodium electrode, characterized in that The surface layer of the pre-lithium or pre-sodium electrode is a packaging film of the pre-lithium or pre-sodium electrode, the raw material of the surface packaging film includes organic fluoride, and the thickness of the packaging film is 0.1-2 µm; the middle layer is a pre-lithium or pre-sodium negative electrode, which is prepared by a dry electrode process or a wet electrode process, and the pre-lithium or pre-sodium object includes one or more of silicon-carbon materials, silicon-based materials, graphite materials, silicon-carbon / graphite composite materials, silicon-based / graphite composite materials, lithium titanate and hard carbon-based materials, and the thickness of the pre-lithium or pre-sodium negative electrode is 20-50 µm, and the bottom layer is a modified current collector layer, and the modified current collector layer includes one of a copper coating, a liquid metal coating, a traditional copper foil and a coated copper foil, and the thickness is 0.1-10 µm; The organic fluoride comprises PFPE; The raw materials of the encapsulation film also include PEG; The packaging film of the pre-lithium or pre-sodium electrode is obtained by self-polymerization of PFPE and PEG after reacting with lithium or sodium metal, lithium or sodium carbon or lithium silicon particles; the pre-lithium or pre-sodium negative electrode is prepared by co-rolling lithium or sodium foil with one of graphite, hard carbon-based, silicon-carbon, silicon-oxygen, silicon-carbon / graphite composite or silicon-oxygen / graphite composite electrodes; Or it is obtained by solvating pre-lithium or pre-sodium with one of graphite, hard carbon-based, silicon-carbon, silicon-based, silicon-carbon / graphite composite, and silicon-based / graphite composite electrodes; the modified current collector layer is obtained by spraying liquid metal, evaporating copper coating or rolling conventional copper foil current collector; The method for preparing the pre-lithium or pre-sodium electrode comprises at least the following steps: S01. Obtain silicon-carbon ‖ copper foil, silicon-oxygen ‖ copper foil, graphite ‖ copper foil, silicon-carbon / graphite ‖ copper foil, silicon-oxygen / graphite ‖ copper foil or hard carbon-based ‖ copper foil negative electrode by wet electrode process; Or through one or more processes of dry electrode process, evaporation, and spraying, obtain silicon-carbon ‖ copper coating, silicon-oxygen ‖ copper coating, graphite ‖ copper coating, silicon-carbon / graphite ‖ copper foil, silicon-oxygen / graphite ‖ copper foil and hard carbon-based ‖ copper coating negative electrode, silicon-carbon ‖ liquid metal coating, silicon-oxygen carbon ‖ liquid metal coating, graphite ‖ liquid metal coating, silicon-carbon / graphite ‖ liquid metal, silicon-oxygen / graphite ‖ liquid metal, hard carbon ‖ liquid metal coating negative electrode; S02, fully mixing PEG, PFPE and a photoinitiator by stirring to form PEG-PFPE, and then evenly coating the PEG-PFPE on the PET film by spraying or brushing, and then compounding a layer of lithium or sodium metal film to form a Li or Na ‖ PEG-PFPE ‖ PET composite film; S03, laminating the metal side of the Li or Na|PEG-PFPE|PET composite film and the negative electrode described in S01, adjusting the roller spacing so that the two are rolled together, and the negative electrode described in S01 will undergo a pre-lithium or pre-sodium reaction under the action of lithium or sodium metal; S04. Remove the outer PET film, adjust the wavelength, light intensity and illumination time of ultraviolet light to treat the electrode surface, so that PEG and PFPE can undergo cross-linking and self-polymerization reaction, thereby obtaining a pre-lithium or pre-sodium electrode with surface encapsulation and composite structure.

2. The pre-lithium or pre-sodium electrode according to claim 1, characterized in that The liquid metal in the liquid metal coating includes Ga, In, and Sn.

3. The pre-lithium or pre-sodium electrode according to claim 2, characterized in that The mass ratio of Ga, In and Sn is (0-10): (0-10): (0-10).

4. The pre-lithium or pre-sodium electrode according to claim 3, characterized in that The mass ratio of PEG to PFPE in the S02 is (0-10): (0-10), the thickness of the PEG-PFPE coating is adjusted to 0.1 - 2 μm, the amount of photoinitiator added is 5-50 μL, and the thickness of the lithium or sodium metal layer is 0.1 - 50 μm.

5. The pre-lithium or pre-sodium electrode according to claim 4, characterized in that The wavelength of the ultraviolet light in the S04 is 100 - 1000 nm, and the light intensity is 50 - 500 mW / cm 2 , the illumination time is 1 - 60 min.

6. A lithium or sodium composite battery comprising the pre-lithium or pre-sodium electrode according to claim 5.