Method for producing graphite by using paper to save water

By softening paper or waste paper in dimethyl sulfoxide and mixing with polyacrylonitrile and carbide graphitization at high temperatures, the problem of producing low-density graphite at low cost and low water consumption is solved, and suitable for insulating materials is achieved. Efficient graphite production overcomes the challenges of water consumption and production time.

CN118176164BActive Publication Date: 2024-11-19NIPPON KORNMEYER CARBON GROUP GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280042061.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-11-19
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

The prior art is difficult to produce low-density graphite at low cost and efficiently, and has low efficiency in using water resources, especially when using waste paper as raw material.

Method used

The paper or waste paper is softened in dimethyl sulfoxide and mixed with polyacrylonitrile, then polymerized in water, and then carbonized and graphitized at high temperatures to form low-density graphite without additional adhesive. Reduce water use.

Benefits of technology

It has achieved low-cost and low water consumption for low production of low-density graphite, which is suitable for insulating materials, and has overcome the problem of long hardening time of polyacrylonitrile through mass production, reducing production costs and water resource consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118176164B_ABST
    Figure CN118176164B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for water-saving production of low-density graphite as an insulating material from paper (preferably waste paper). This is achieved by soaking paper / waste paper, shredded paper or paper strips in a container containing dimethyl sulfoxide to produce paper fibers; adding polyacrylonitrile to the dissolved paper fibers and stirring until a paste or a mixture with a consistency similar to that of a paste is formed; placing the paste in a mold and then squeezing excess liquid out of the paste by pressing to form a paper mass; then soaking the paper mass in water for a specified time to harden the polyacrylonitrile until the polyacrylonitrile polymerizes and forms a hardened paper mass; pre-drying the hardened paper mass in air at a temperature up to 100°C; stabilizing the hardened paper mass by heating it to 250°C in air to remove residual moisture; carbonizing the hardened and dried paper mass in an oven at >1000°C and then graphitizing it at >2000°C to form a low-density graphite block.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for producing low-density graphite as an insulating material by using paper in a water-saving manner, and the method preferably uses waste paper.

[0002] Waste paper is generated in large quantities and can not only be recycled but also used to produce graphite for a variety of applications.

[0003] The purpose of the present invention is to provide a low-cost, simple and sustainable method for producing low-density graphite using paper in a water-saving manner. The method preferably uses waste paper. The produced graphite can be used as an insulating material and the use of water can be minimized.

[0004] The purpose of the present invention can be achieved by the following method:

[0005] - Place the paper / waste, shredded paper or paper strips in a suitable container with dimethyl sulfoxide (DMSO) to soften until it dissolves into fibers,

[0006] - adding polyacrylonitrile (PAN) to paper fibers dissolved in dimethyl sulfoxide and stirring until a paste or a mixture having a paste-like consistency is formed,

[0007] - placing the paste into suitable moulds and then squeezing the excess liquid out of the paste by pressing, or isostatically pressing the paste into paper balls,

[0008] - The paper ball is removed from the mold to harden the polyacrylonitrile and soaked in water for a specified time until the polyacrylonitrile polymerizes and forms a hardened paper ball,

[0009] - pre-dry the hardened paper mass in air at temperatures up to ~100°C,

[0010] - The hardened paper mass is heated to 250°C in air to stabilize it and remove the remaining moisture,

[0011] - The hardened and dried paper mass is placed in an oven to carbonize it at >1000°C and then graphitize it at >2000°C (up to 3000°C) to form a low-density graphite block.

[0012] The optimum temperature for graphitization is 2500°C, wherein the high temperature treatment is usually carried out in the absence of air, in a vacuum, or in the presence of an inert gas.

[0013] The method does not require the addition of a binder such as sugar, syrup, or starch, and thus requires very little water. The method is therefore a method for producing low-density graphite at a very low cost, and the produced graphite is suitable for use as an insulating material or for other purposes.

[0014] The only drawback of the present invention is that the hardening / polymerization of the polyacrylonitrile may take up to 2 weeks, but this drawback can be easily offset by mass production.

[0015] The present invention is further described below with reference to an embodiment and drawings. The following drawings show:

[0016] Figure 1 : Shredded paper dissolves into fibers in a container;

[0017] Figure 2 : The dissolved paper is mixed with a binder having a paste-like consistency;

[0018] Figure 3 :Will Figure 2 The mixture shown after isostatic pressing and hardening; and

[0019] Figure 4 : The hardened paper ball undergoes graphitization.

[0020] In order to produce graphite from paper / waste paper, shredded paper or paper strips 1, the paper 1 is first soaked in a suitable container 2 containing dimethyl sulfoxide (DMSO) and softened for a long time until the paper 1 is dissolved into fibers ( Figure 1 ). This process may take several days.

[0021] Next, the softened paper fibers soaked in dimethyl sulfoxide are placed in a suitable mixing device and mixed therein, and polyacrylonitrile (PAN) is added during stirring until a paste 3 or a mixture having a consistency similar to a paste is formed ( Figure 2 ).

[0022] In the next step, the paste 3 is placed in a suitable mold and then the excess liquid is squeezed out of the paste by pressing, or the paste is isostatically pressed to form a paper ball 4 ( Figure 3 ).

[0023] The paper ball 4 is then removed from the press and completely immersed in water for a specified period of time to harden the polyacrylonitrile until the polyacrylonitrile polymerizes and forms a hardened paper ball 4, which is then dried in air. The hardening or polymerization of the polyacrylonitrile in the paper ball 4 may take up to two weeks, but this disadvantage can be easily offset by mass production.

[0024] This polyacrylonitrile polymerization process is the only step that uses a small amount of water, and the water can be reused many times, so the water consumption can be reduced to a minimum.

[0025] Since the subsequent carbonization or graphitization of the hardened paper mass 4 is carried out at very high temperatures, there is a risk that the solvent and water used to harden the paper mass 4 will release gases and vapors, which may ultimately lead to more or less noticeable cracking of the final product. For this reason, the hardened paper mass 4 (pre-dried and hardened in air) should be slowly heated in an oven to stabilize it in an air atmosphere, so that it is heated to 250° C. over a longer period of time, in order to remove the remaining solvent and moisture in the paper mass 4 as completely as possible.

[0026] The hardened and dried paper ball 4 is then placed in an oven to carbonize it at a temperature of >1000°C and then graphitized at a temperature of >2000°C (up to 3000°C) to form a low-density graphite block 5, wherein the optimal temperature for graphitization is about 2500°C.

[0027] Of course, high temperature processing must be performed in the absence of air, in vacuum, or with an inert gas.

[0028] A particular advantage of this method is that no binders such as sugars, syrups or starches need to be used.

[0029] Since only small amounts of water are needed, and only to harden the polyacrylonitrile, this is a particularly cost-effective method for producing low-density graphite, which is well suited for use as an insulation material or other applications.

[0030] Reference numerals

[0031] 1: Paper / waste paper, shredded paper or paper strips

[0032] 2: Container

[0033] 3: Paste

[0034] 4: Paper Ball

[0035] 5: Graphite block

Claims

1. A method for producing low-density graphite as an insulating material using paper in a water-saving manner, characterized by: - Place waste paper, shredded paper or paper strips in a suitable container filled with dimethyl sulfoxide (DMSO) to soften until they dissolve into fibers. - adding polyacrylonitrile (PAN) to paper fibers dissolved in dimethyl sulfoxide and stirring until a paste or a mixture having a paste-like consistency is formed, - placing the paste or mixture into suitable moulds and isostatically pressing the paste or mixture into a paper mass, - The paper ball is removed from the mold to harden the polyacrylonitrile and soaked in water for a specified time until the polyacrylonitrile polymerizes and forms a hardened paper ball, - pre-drying the hardened paper mass in air at a temperature up to 100° C. to obtain a pre-dried hardened paper mass, - stabilizing the pre-dried hardened paper mass by heating it to 250°C in air to remove the remaining moisture and obtain a hardened and dried paper mass, - The hardened and dried paper mass is carbonized in an oven at >1000°C and then graphitized at >2000°C to form a low density graphite block.

2. The method according to claim 1, characterized in that: The graphitization of the carbonized paper mass is carried out at a temperature of 2500°C.

3. The method according to claim 1 or 2, characterized in that: The high temperature treatment of the hardened and dried paper mass is usually carried out in the absence of air, in a vacuum, or in the presence of an inert gas.