A device and method for impact strengthening of complex metal component surfaces
By using an intelligent impact strengthening device for complex component metal surfaces, combined with industrial robots and automated control, high-precision and uniform strengthening of complex component surfaces is achieved. This solves the problems of uneven strengthening effect and increased surface roughness in existing technologies, and improves fatigue performance and surface quality.
Patent Information
- Application Number
- CN202410516984.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-04-28
AI Technical Summary
Existing technologies are insufficient for efficient and uniform surface mechanical strengthening of complex components, resulting in uneven strengthening effects and increased surface roughness, which cannot meet the processing requirements of complex curved surfaces.
An intelligent impact strengthening device for complex metal components is adopted, which combines industrial robots and automated control technology. It achieves precise control of impact force through voice coil motors and force sensors, and real-time cooling through a cooling system. The processing path is planned using the point-line-area integral method to achieve high-precision and intelligent automated strengthening.
It significantly improves the fatigue performance of complex component surfaces, reduces surface roughness, introduces residual compressive stress and gradient microstructure, enhances surface strength and hardness, and expands the applicability of the device and the universality of materials.
Smart Images

Figure CN118207406B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal surface treatment technology, specifically a device and method for impact strengthening of complex metal components. Background Technology
[0002] Fatigue fracture of metal components is generally divided into three stages: crack initiation, crack propagation, and instantaneous fracture. The fatigue life of a component is mainly composed of crack initiation life and crack propagation life; instantaneous fracture does not contribute to the lifespan. Numerous fatigue failure cases and material fatigue test data show that for the vast majority of components, fatigue crack initiation life accounts for 90% or even more than 99% of the total lifespan. Therefore, improving the crack initiation life of metal component surfaces is key to improving the surface fatigue reliability of metal components. Currently, the main surface fatigue resistance treatment methods at home and abroad can be summarized into four categories: 1) Mechanical: surface mechanical strengthening; 2) Electrical: surface induction hardening; 3) Optical: surface laser strengthening; 4) Chemical: surface carburizing and nitriding. Among these, surface mechanical strengthening is the most widely used due to its technical versatility and significant fatigue resistance effect. Currently, metal surface mechanical strengthening mainly includes shot peening, ultrasonic impact, and rolling strengthening. Although shot peening can strengthen complex curved surface components, it increases surface roughness after treatment and may even introduce small folding defects and microcracks. Ultrasonic impact testing is widely used for various complex components due to its portability. It is mostly performed handheld, but handheld impact introduces numerous uncontrollable factors during testing, making it difficult to control the impact force and resulting in uneven strengthening effects. Furthermore, ultrasonic impact increases surface roughness. Ultrasonic surface finishing strengthens the surface by maintaining a fixed preload on the workpiece surface, suitable for self-rotating rod-shaped samples. However, it leaves rolling marks on complex curved surfaces, resulting in poor surface strengthening. Roller burnishing is only suitable for rod-shaped samples and is difficult to use for components with complex curved surfaces.
[0003] Therefore, in order to achieve mechanical strengthening of the metal surface of complex components, it is necessary to develop an intelligent surface fatigue resistance treatment device to strengthen components of different materials and shapes. Summary of the Invention
[0004] The purpose of this invention is to provide an impact strengthening device and method for complex metal component surfaces, enabling intelligent and high-precision surface treatment of components of different shapes. By combining surface life extension equipment with automated control technology, it can adaptively process the workpiece surface, thereby achieving high-precision and intelligent automated strengthening of complex component surfaces. After treatment, the surface strength and hardness of the metal can be significantly improved, the surface roughness reduced, residual compressive stress introduced, a gradient microstructure obtained, and fatigue performance enhanced.
[0005] The technical solution adopted by the present invention to achieve the above objectives is: an impact strengthening device for the metal surface of complex components, comprising: a workbench, a control cabinet, an industrial robot, an impact device, a cooling system, and a control panel;
[0006] The control panel is connected to the industrial robot via a control cabinet, and the industrial robot is located on one side of the workbench.
[0007] The impact device is located at the end of the robotic arm of the industrial robot and moves above the worktable surface through the robotic arm. The movement range of the impact device covers the worktable surface.
[0008] The cooling system is connected to the control panel and is used to receive control from the control panel to cool the workpiece to be processed on the worktable in real time.
[0009] The impact device includes: a device housing, a voice coil motor, a connector, a force sensor, and a punch.
[0010] The device housing is provided with a connector at the tail end, and the connector is fixedly connected to the end of the robotic arm of the industrial robot.
[0011] The voice coil motor is mounted on a motor mounting bracket inside the device housing. Springs are provided on both sides of the motor mounting bracket. The springs are fixed to the inner wall of the bottom of the device housing, so that the motor mounting bracket can move back and forth inside the device housing to buffer and protect the voice coil motor.
[0012] A through hole is provided on the end face of the device housing opposite to the connector. The output end of the voice coil motor is located in the through hole and is connected to the force sensor.
[0013] The force sensor is adapted to the through hole, and a punch for impact strengthening of the metal surface is vertically provided at the detection end of the force sensor.
[0014] The workbench is a square plate structure with four slides on it. The slides on opposite sides are symmetrical to each other and are not connected to each other.
[0015] Four slides form a cross shape; a slider is slidably mounted on each slide; the slider is equipped with bolts to fix itself to the worktable, so that the four sliders can clamp the workpiece to be processed located at the center of the worktable.
[0016] The cooling system includes: an air compressor and a cooling device;
[0017] The cooling device is located on the workbench and is connected to an air compressor located on one side of the workbench.
[0018] The air compressor is connected to the control panel, which controls the start and stop of the air compressor to cool the workpiece processed by the cooling device.
[0019] An impact strengthening method for a complex component metal surface impact strengthening device includes the following steps:
[0020] 1) Establish the tool coordinate system and determine its orientation;
[0021] 2) Determine the relative positions of the robot and the workpiece to be processed;
[0022] 3) The control panel determines the processing position and processing path as needed, adjusts the robot's pose through the control cabinet, plans the reinforcement range, path and movement step length, and conducts simulation collision verification;
[0023] 4) The control cabinet controls the movement of the industrial robot. When the industrial robot moves to the surface of the workpiece, the control panel sets the amplitude and frequency of the voice coil motor of the impact device. The impact force is controlled by the amplitude, and the robot's moving speed is determined by the frequency and step size.
[0024] 5) During the impact strengthening process of the workpiece, the control panel controls the cooling system to cool the workpiece in real time;
[0025] 6) Repeat steps 3) to 5) to perform multiple impact reinforcements. When performing multiple impact reinforcements, different types of punches or different impact forces can be selected.
[0026] Before step 1), the mover of the voice coil motor is locked in advance. During the strengthening process, this position is used as the balance point for the reciprocating vibration of the voice coil motor.
[0027] Step 1) specifically includes:
[0028] The origin of the tool coordinate system is determined by the XYZ 4-point method. The TCP to be measured is moved from 4 different directions to a reference cusp. The control cabinet calculates the TCP of the tool from different flange position values of the industrial robot. Then, the attitude of the tool coordinate system is determined by the ABC world coordinate system method.
[0029] Step 2) specifically includes:
[0030] The workpiece to be processed is fixed on the worktable. The punches of the impact device are moved sequentially to three different vertices of the workpiece and the XYZ coordinates in the robot coordinate system are recorded. The workpiece model is then transformed into the robot coordinate system by rotation and translation using the three-point method to ensure that the reference of the robot and the workpiece to be processed are consistent.
[0031] The process of adjusting the robot's pose via the control cabinet, planning the reinforcement range, path, and step length, and performing simulated collision verification includes the following steps:
[0032] 1-1) Determine the lead wires according to the processing path required. The processing path can be a vertical lead wire or a parallel lead wire, and adjust the processing area and step size.
[0033] 1-2) Generate normal phases based on the processing path, and import the path with normal phases into the industrial robot motion planning interface;
[0034] 1-3) Adjust the entry and exit point information of the industrial robot, modify the processing sequence, and perform simulation collision verification; if no collision occurs in the simulation collision verification, proceed to step 1-4); if a collision occurs in the simulation collision verification, return to step 1-1).
[0035] 1-4) Export the processing path verified by the simulation collision to the industrial robot, and the industrial robot realizes automated operation according to the edited processing path.
[0036] In step 4), the amplitude and frequency ranges of the voice coil motor of the impact device are 0-5mm and 0-100Hz, respectively.
[0037] The present invention has the following beneficial effects and advantages:
[0038] 1. This invention uses an intelligent robotic arm to replace the bulky machine tool-type processing structure, which can perform impact strengthening on complex components. At the same time, the impact force can be adjusted within a wide range, which can meet the needs of different materials and metals with different hardening capabilities, and greatly expand the universality of the device in terms of component shape and material.
[0039] 2. This invention utilizes the point-line-area integral method to stably control the impact force acting on the workpiece, resulting in a smooth, flat, and densely uniform hardened layer on the surface of the processed component, achieving a surface "smoothness, tightness, and strength" match.
[0040] 3. This invention can complete path planning offline, perform simulated collision verification, and achieve intelligent processing through automated control technology, while improving reinforcement efficiency. Attached Figure Description
[0041] Figure 1 This is a schematic diagram of the impact strengthening device for complex component metal surfaces according to the present invention;
[0042] Figure 2 This is a detailed diagram of the impact structure of the present invention;
[0043] Figure 3 This is a schematic diagram of the curved high-strength steel processed in Embodiment 1 of the present invention;
[0044] Figure 4 The four-point bending fatigue life of curved high-strength steel after treatment using the method of this invention;
[0045] Figure 5This is a schematic diagram of the 6061 aluminum alloy T-foot weld processed in Embodiment 2 of the present invention;
[0046] Figure 6 The four-point bending fatigue life of 6061 aluminum alloy T-foot weld after treatment using the method of the present invention;
[0047] Among them, 1 is the workbench, 2 is the control cabinet, 3 is the industrial robot, 4 is the impact structure, 5 is the air compressor, 6 is the cooling device, 7 is the control panel, 401 is the voice coil motor, 402 is the connector, 403 is the force sensor, and 404 is the punch. Detailed Implementation
[0048] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments.
[0049] like Figure 1 The diagram shown is a structural schematic of the impact strengthening device for the metal surface of complex components according to the present invention. The impact strengthening device for the metal surface of complex components according to the present invention includes: a workbench 1, a control cabinet 2, an industrial robot 3, an impact device 4, a cooling system, and a control panel 7.
[0050] The control panel 7 is connected to the industrial robot 3 via the control cabinet 2, and the industrial robot 3 is located on one side of the workbench.
[0051] The impact device 4 is located at the end of the robotic arm of the industrial robot 3. It moves above the surface of the worktable 1 driven by the robotic arm, and the range of motion of the impact device 4 covers the surface of the worktable 1.
[0052] The cooling system is connected to the control panel 7 and is used to receive control from the control panel 7 to cool the workpiece to be processed on the worktable 1 in real time.
[0053] Impact device 4 includes: device housing, voice coil motor 401, connector 402, force sensor 403, and punch 404;
[0054] The device housing is provided with a connector 402 at the rear, which is fixedly connected to the end of the robotic arm of the industrial robot 3.
[0055] The voice coil motor 401 is mounted on a motor mounting bracket inside the device housing. Springs are provided on both sides of the motor mounting bracket. The springs are fixed to the inner wall of the bottom of the device housing, so that the motor mounting bracket can move back and forth inside the device housing to buffer and protect the voice coil motor 401.
[0056] A through hole is provided on the end face of the device housing on the side opposite to the connector 402. The output end of the voice coil motor 401 is located in the through hole and is connected to the force sensor 403.
[0057] Force sensor 403 is adapted to the through hole, and a punch 404 for impact strengthening of metal surface is vertically provided at the detection end of force sensor 403. Industrial robot 3 can link all axes to ensure that punch 404 is perpendicular to the workpiece surface, can handle complex shaped components, achieve conformal strengthening, and has a wide range of applications.
[0058] The workbench 1 is a square plate structure with four slides. The slides on opposite sides are symmetrical to each other and are not connected to each other.
[0059] Four slides form a cross shape; a slider is slidably mounted on each slide; the slider is equipped with bolts to fix itself to the worktable 1, so that the four sliders can clamp the workpiece to be processed located at the center of the worktable, and the workpiece loading and unloading is simple.
[0060] The cooling system includes an air compressor 5 and a cooling device 6. The cooling system uses air cooling, which can avoid contamination of the sample caused by other types of cooling such as water cooling and oil cooling.
[0061] The cooling device 6 is located on the workbench 1 and is connected to the air compressor 5 located on one side of the workbench 1.
[0062] The air compressor 5 is connected to the control panel 7 so that the air compressor 5 can be started and stopped by the control panel 7, so as to provide air to the cooling device 6 to cool the workpiece.
[0063] This invention discloses a method for impact strengthening of complex component metal surfaces using the aforementioned device. The method involves applying the impact strengthening device to the surface of complex components for impact strengthening treatment to extend their fatigue life. The method includes the following steps:
[0064] Before step 1), it is also necessary to lock the mover of the voice coil motor 401 in advance. During the strengthening process, this position is used as the balance point for the reciprocating vibration of the voice coil motor.
[0065] 1) Establish the tool coordinate system and determine its orientation:
[0066] The origin of the tool coordinate system is determined by the XYZ 4-point method. The TCP to be measured is moved from 4 different directions to a reference cusp. The control cabinet 2 calculates the TCP of the tool from the different flange position values of the industrial robot 3. Then, the attitude of the tool coordinate system is determined by the ABC world coordinate system method.
[0067] 2) Determine the relative positions of the robot and the workpiece to be processed;
[0068] The workpiece to be processed is fixed on the worktable 1. The punch 404 of the impact device 4 is moved sequentially to three different vertices of the workpiece to be processed, and its XYZ coordinate values in the robot coordinate system are recorded. The workpiece model is transformed into the robot coordinate system by rotation and translation operations through the three-point method to ensure that the reference of the robot and the workpiece to be processed are consistent.
[0069] 3) The control panel 7 determines the processing position and processing path as needed, adjusts the robot's posture through the control cabinet 2, plans the reinforcement range, path and movement step length, and performs simulation collision verification.
[0070] 3-1) Determine the lead wires according to the processing path required. The processing path can be a vertical lead wire or a parallel lead wire, and adjust the processing area and step size.
[0071] 3-2) Generate the normal phase based on the processing path, and import the path with the normal phase into the motion planning interface of the industrial robot.
[0072] 3-3) Adjust the entry and exit point information of the industrial robot, modify the processing sequence, and perform simulation collision verification; if no collision occurs in the simulation collision verification, proceed to step 3-4); if a collision occurs in the simulation collision verification, return to step 3-1.
[0073] 3-4) Export the processing path verified by the simulation collision to the industrial robot 3. The industrial robot (3) performs automated operation according to the edited processing path.
[0074] 4) Control cabinet 2 controls the movement of industrial robot 3. When industrial robot 3 moves to the surface of workpiece, control panel 7 sets the amplitude and frequency of voice coil motor 401 of impact device 4. The impact force is controlled by amplitude, and the robot's moving speed is determined by frequency and step size.
[0075] The amplitude and frequency range of the voice coil motor 401 with the impact device 4 are 0-5mm and 0-100Hz, respectively.
[0076] 5) During the impact strengthening process of the workpiece, the control panel 7 controls the cooling system to cool the workpiece in real time;
[0077] 6) Repeat steps 3) to 5) to perform multiple impact reinforcements. When performing multiple impact reinforcements, different types of 404 punches can be selected or different impact forces can be changed.
[0078] Example 1:
[0079] like Figure 3 The diagram shown is a schematic of the curved high-strength steel processed in Embodiment 1 of the present invention. This embodiment takes curved high-strength steel as an example to perform surface impact strengthening. The specific steps are as follows:
[0080] Step 1: Establish the tool coordinate system. First, install a 0.2mm diameter circular flat bottom punch to fix the voice coil mover in a suitable position. Use the XYZ 4-point method to determine the origin (TCP) of the tool coordinate system, and the ABC world coordinate system method to determine the orientation of the tool coordinate system.
[0081] Step 2: Determine the relative positions of the robot and the workpiece. Fix the curved high-strength steel workpiece on the worktable, and use a punch to move it sequentially to three different vertices of the workpiece, recording its XYZ values in the world coordinate system. Then, using the three-point method in offline programming software, transform the workpiece model into the robot coordinate system through a series of operations such as rotation and translation.
[0082] Step 3: Offline programming. Determine the machining location, with a step size of 0.1mm, and process a 25mm wide curved surface. Perform offline programming and simulation collision verification.
[0083] Step 4: Strengthening treatment. When the robot moves to the workpiece surface, set the amplitude and frequency of the voice coil motor to 15Hz, the impact force to 40kg, and the robot's moving speed to 1.5mm / s;
[0084] Step 5: After processing, remove the sample from the platform, cut it into fatigue samples with a width of 6mm, and conduct fatigue tests on it.
[0085] like Figure 4 The figure shows the four-point bending fatigue life of high-strength curved steel after treatment using the method of this invention. Four-point bending fatigue tests were conducted on the original state, the steel after shot peening, and the steel after treatment using this invention. The fatigue life was measured at a stress ratio of 0.1 and a maximum bending stress of 2500 MPa. Figure 4 As shown in the figure, the average fatigue life after treatment with the present invention is 16.6 times higher than that after shot peening and 32.9 times higher than that of the untreated original state.
[0086] Example 2:
[0087] like Figure 5 The diagram shown is a schematic of the 6061 aluminum alloy T-foot weld processed in Embodiment 2 of the present invention. This embodiment takes the 6061 aluminum alloy T-foot weld as an example and performs surface impact strengthening. The specific steps are as follows:
[0088] Step 1: Cut the weld site of the T-foot weld into an R25 arc and model it using 3D software;
[0089] Step 2: Establish the tool coordinate system. First, install a 0.2mm diameter circular flat bottom punch to fix the voice coil mover in a suitable position. Use the XYZ 4-point method to determine the origin (TCP) of the tool coordinate system, and the ABC world coordinate system method to determine the orientation of the tool coordinate system.
[0090] Step 3: Determine the relative positions of the robot and the workpiece. Fix the curved high-strength steel workpiece on the worktable, and use a punch to move it sequentially to three different vertices of the workpiece, recording its XYZ values in the world coordinate system. Then, using the three-point method in the offline programming software, transform the workpiece model into the robot coordinate system through a series of operations such as rotation and translation.
[0091] Step 4: Offline programming. Determine the machining location, with a step size of 0.1mm, and process a 50mm wide curved surface. Perform offline programming and simulation collision verification.
[0092] Step 4: Strengthening treatment. When the robot moves to the workpiece surface, set the amplitude and frequency of the voice coil motor to 15Hz, the impact force to 10kg, and the robot's moving speed to 1.5mm / s;
[0093] Step 5: After processing, remove the sample from the platform, cut it into fatigue samples with a width of 10mm, and conduct fatigue tests on it.
[0094] like Figure 6 The figure shows the four-point bending fatigue life after the 6061 aluminum alloy T-foot weld was treated using the method of the present invention.
[0095] Tensile fatigue tests were conducted on the original state, the shot-peened state, and the state after treatment with this invention. The fatigue life was measured at a stress ratio of 0.1 and a maximum stress of 80 MPa. Figure 6 As shown in the figure, the average fatigue life after treatment with this invention is 34.2 times higher than that after shot peening and 18.9 times higher than that of the untreated state. In summary, this invention demonstrates a good fatigue life extension effect.
[0096] The above description is merely an embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, extensions, etc., made within the spirit and principles of the present invention are included within the scope of protection of the present invention.
Claims
1. A device for impact strengthening of complex component metal surfaces, characterized in that, include: Workbench (1), control cabinet (2), industrial robot (3), impact device (4), cooling system, control panel (7); The control panel (7) is connected to the industrial robot (3) through the control cabinet (2), and the industrial robot (3) is located on one side of the workbench; The impact device (4) is located at the end of the robotic arm of the industrial robot (3), and moves above the surface of the worktable (1) driven by the robotic arm, and the range of motion of the impact device (4) covers the surface of the worktable (1). The impact device (4) includes: a device housing, a voice coil motor (401), a connector (402), a force sensor (403), and a punch (404). The device housing is provided with a connector (402) at the tail end, and the connector (402) is fixedly connected to the end of the robotic arm of the industrial robot (3); The voice coil motor (401) is mounted on a motor mounting bracket inside the device housing. Springs are provided on both sides of the motor mounting bracket. The springs are fixed to the inner wall of the bottom of the device housing, so that the motor mounting bracket moves back and forth inside the device housing to buffer and protect the voice coil motor (401). A through hole is provided on the end face of the device housing opposite to the connector (402), and the output end of the voice coil motor (401) is located in the through hole and connected to the force sensor (403); The force sensor (403) is adapted to the through hole, and the detection end of the force sensor (403) is vertically provided with a punch (404) to strengthen the impact on the metal surface. The workbench (1) is a square plate structure. Four slides are provided on the workbench (1). The slides on opposite sides are symmetrical to each other and are not connected to each other. Four slides form a cross shape; a slider is slidably provided on each of the slides; the slider is provided with bolts to fix itself on the worktable (1) so as to realize that the four sliders clamp the workpiece to be processed located at the center of the worktable; The cooling system is connected to the control panel (7) and is used to receive the control of the control panel (7) to cool the workpiece to be processed on the workbench (1) in real time. The cooling system includes an air compressor (5) and a cooling device (6). The cooling device (6) is located on the workbench (1) and is connected to the air compressor (5) located on one side of the workbench (1); The air compressor (5) is connected to the control panel (7) so that the air compressor (5) can be started and stopped by the control panel (7) so as to provide air to the cooling device (6) to cool the workpiece.
2. The impact strengthening method of the impact strengthening device for complex component metal surface according to claim 1, characterized in that, Includes the following steps: 1) Establish the tool coordinate system and determine its orientation; 2) Determine the relative positions of the robot and the workpiece to be processed; 3) The control panel (7) determines the processing position and processing path as needed, adjusts the robot's pose through the control cabinet (2), plans the reinforcement range, path and movement step length, and performs simulation collision verification; 4) The control cabinet (2) controls the movement of the industrial robot (3). When the industrial robot (3) moves to the surface of the workpiece, the control panel (7) sets the amplitude and frequency of the voice coil motor (401) of the impact device (4). The impact force is controlled by the amplitude, and the robot's moving speed is determined by the frequency and step size. 5) During the impact strengthening process of the workpiece, the control panel (7) controls the cooling system to cool the workpiece in real time; 6) Repeat steps 3) to 5) to perform multiple impact reinforcements. When performing multiple impact reinforcements, different types of punches (404) can be selected or different impact forces can be changed.
3. The impact strengthening method of the impact strengthening device for complex component metal surface according to claim 2, characterized in that, Before step 1), the mover of the voice coil motor (401) is locked in advance. During the strengthening process, this position is used as the balance point for the reciprocating vibration of the voice coil motor.
4. The impact strengthening method of the impact strengthening device for complex component metal surface according to claim 2, characterized in that, Step 1) specifically refers to: The origin of the tool coordinate system is determined by the XYZ 4-point method. The TCP to be measured is moved from 4 different directions to a reference cusp. The control cabinet (2) calculates the TCP of the tool from the different flange position values of the industrial robot (3). Then, the attitude of the tool coordinate system is determined by the ABC world coordinate system method.
5. The impact strengthening method of the impact strengthening device for complex component metal surface according to claim 2, characterized in that, Step 2) specifically refers to: The workpiece to be processed is fixed on the worktable (1). The punch (404) of the impact device (4) is used to move to three different vertices of the workpiece in sequence, and the coordinates XYZ values in the robot coordinate system are recorded. The workpiece model is transformed into the robot coordinate system by rotation and translation operations through the three-point method to ensure that the reference of the robot and the workpiece to be processed are consistent.
6. The impact strengthening method of the impact strengthening device for the metal surface of complex components according to claim 2, characterized in that, The process of adjusting the robot's pose, planning the reinforcement range, path, and step length via the control cabinet (2), and performing simulated collision verification includes the following steps: 1-1) Determine the lead wires according to the processing path required. The processing path can be a vertical lead wire or a parallel lead wire, and adjust the processing area and step size. 1-2) Generate normal phases based on the processing path, and import the path with normal phases into the motion planning interface of the industrial robot (3); 1-3) Adjust the entry and exit point information of the industrial robot, modify the processing sequence, and perform simulated collision verification; if no collision occurs during the simulated collision verification, proceed to step 1-4); if a collision occurs during the simulated collision verification, return to step 1-1). 1-4) Export the processing path verified by the simulation collision to the industrial robot (3), and the industrial robot (3) realizes automated operation according to the edited processing path.
7. The impact strengthening method of the impact strengthening device for the metal surface of complex components according to claim 2, characterized in that, In step 4), the amplitude and frequency range of the voice coil motor (401) of the impact device (4) are 0-5mm and 0-100Hz, respectively.
Citation Information
Patent Citations
Efficient laser shock peening control method based on technological parameter matching
CN115572812A
Metal plate surface integral impact anti-fatigue device and strengthening method
CN117403054A