A method and system for comprehensive recovery of lead anode mud

By treating lead anode mud with hydrochloric acid, oxidant, and sodium salt solution, and combining specific temperature and pH control, the efficient separation and recovery of precious metals in lead anode mud has been achieved. This solves the problems of large equipment size and low efficiency in existing technologies, and enables the production of high-purity products and the recycling of wastewater.

CN118222837BActive Publication Date: 2026-11-10CHIFENG YUNTONG NON FERROUS METAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410365083.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2026-11-10
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

Existing technologies for treating lead anode mud suffer from problems such as large and complex equipment, low efficiency, unsatisfactory precious metal recovery rate, and inability to effectively separate antimony and bismuth.

Method used

A combination of hydrochloric acid, oxidant, and sodium salt solution is used to treat lead anode mud. Through a series of steps such as pre-soaking, antimony and bismuth precipitation, copper replacement, slurrying, neutralization, and antimony precipitation, combined with specific temperature and pH control, the metal elements are separated and purified.

Benefits of technology

It achieves efficient separation and recovery of precious metals in lead anode mud, with copper, antimony and bismuth leaching rates exceeding 98% and antimony and bismuth recovery rates exceeding 99%. The products are of high purity, the wastewater can be recycled, and the entire process is controllable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118222837B_ABST
    Figure CN118222837B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of lead anode mud recycling technology, specifically relating to a method and system for the comprehensive recycling of lead anode mud. The method includes steps such as pre-leaching, antimony and bismuth precipitation, copper replacement, slurrying, neutralization, and antimony precipitation. Using the system and method disclosed in this invention, the content of gold and silver leached into the liquid from the lead anode mud can be reduced to less than 20 mg / L. The leaching residue is smelted using a re-fire method, and all small amounts of lead leached into the liquid can be recovered. The copper, antimony, and bismuth leaching rate reaches over 98%, and the recovery rate reaches over 99%. Furthermore, antimony and bismuth can be recovered and purified separately. The process combines wet and pyrometallurgical treatment, is controllable and highly effective, and the wastewater can be recycled and replenished, reaching a leading level in China.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lead anode mud recycling technology, specifically relating to a method and system for the comprehensive recycling of lead anode mud. Background Technology

[0002] Lead anode slime, a byproduct of lead electrolysis, contains numerous valuable metals such as gold, silver, lead, copper, antimony, and bismuth, making it an important economic growth point for smelting enterprises. Traditionally, the main method for processing this material is pyrometallurgy. In this process, lead anode slime is usually added to a reduction furnace along with copper-removed materials, and through a series of steps, such as blowing and silver electrolysis, the precious metals are ultimately recovered. However, the equipment used in this traditional method has several drawbacks: firstly, it typically requires large-scale material handling capacity, resulting in bulky and complex equipment; secondly, this equipment generates a large amount of waste and emissions during operation; and finally, due to the multiple processing steps involved, the overall process is inefficient, and the recovery rate of precious metals is not ideal.

[0003] To overcome the drawbacks of pyrometallurgical processes, hydrometallurgical processes were extensively studied and gradually matured in the late 1980s. Hydrometallurgical processes typically involve pretreating lead anode slime with acidic solutions to remove base metals, followed by the extraction of precious metals through chemical methods. Although hydrometallurgical processes are superior to pyrometallurgical processes in some aspects, such as the recovery rate of valuable metals, they still face many challenges in processing lead anode slime. For example, existing hydrometallurgical processing units often cannot effectively separate antimony and bismuth, two elements that are very similar in chemical properties, leading to a complex and inefficient separation process. Furthermore, existing hydrometallurgical units often cannot achieve precise control during large-scale production, thus affecting the quality of the final product. Summary of the Invention

[0004] To address the problems existing in the prior art, this invention provides a method and system for the comprehensive recovery of lead anode mud, specifically including the following:

[0005] This invention discloses a method for the comprehensive recovery of lead anode mud, comprising the following steps:

[0006] (1) Pre-impregnation: Add hydrochloric acid solution, oxidant and sodium salt solution to lead anode mud, stir and react at 65-85℃ for 50-120 min, then separate solid and liquid to obtain pre-impregnation solution;

[0007] (2) Antimony and bismuth precipitation: Adjust the pre-impregnation solution to pH < 2.5, stir the reaction at 40-60℃ for 30-60 min, and then separate the solid and liquid to obtain the antimony and bismuth precipitation liquid and antimony and bismuth residue;

[0008] (3) Copper replacement: Adjust the temperature of the solution after antimony and bismuth precipitation to 30-50℃, and add alkali to adjust the H.+ The concentration was adjusted to 10-18 g / L, the displacement agent was added, and the mixture was stirred for 30-60 min. Then, the solid and liquid were separated to obtain the copper-displaced liquid and copper slag.

[0009] (4) Slurrying: Water is added to the antimony bismuth slag and stirred to form a slurry;

[0010] (5) Neutralization: Add an alkaline solution to the slurry, stir and react for 40-80 minutes, then separate the solid and liquid to obtain bismuth slag and antimony-containing liquid;

[0011] (6) Antimony precipitation: Add acid solution to antimony-containing liquid, adjust pH to 2.0-2.5, stir reaction at 30-60℃ for 30-60 min, and then perform solid-liquid separation to obtain antimony-precipitated liquid and antimony slag.

[0012] Preferably, in step (1):

[0013] The concentration of the hydrochloric acid is 2.5-4 mol / L; and / or,

[0014] The oxidant is a sodium chlorate solution with a mass concentration of 45-55%; and / or,

[0015] The sodium salt solution is a saturated sodium chloride solution (referring to a saturated solution at room temperature); and / or,

[0016] The mass ratio of the hydrochloric acid solution, oxidant, and sodium salt solution is 1:(0.13-0.3):(0.15-0.25); and / or,

[0017] The liquid-solid mass ratio of the pre-impregnation reaction system is controlled to be (3-5):1; and / or,

[0018] The stirring speed is 180-220 rpm.

[0019] Preferably, in step (2):

[0020] The method for adjusting the pH of the pre-soaking solution is to add water to it; and / or,

[0021] The stirring speed is 140-180 rpm.

[0022] Preferably, in step (3):

[0023] The alkali is sodium hydroxide, potassium hydroxide, and / or sodium carbonate; and / or,

[0024] The replacement agent is iron powder with a particle size of 50-200 mesh; and / or,

[0025] The amount of the replacement agent added is 1.2-1.5 times the copper mass content in the solution after antimony-bismuth precipitation; and / or,

[0026] The stirring speed is 140-180 rpm.

[0027] Preferably, in step (4):

[0028] The mass ratio of water to antimony-bismuth slag is (1-1.5):1; and / or,

[0029] The stirring speed is 80-120 rpm; and / or

[0030] The stirring time is 20-40 minutes.

[0031] Preferably, in step (5):

[0032] The alkaline solution is a sodium hydroxide solution with a concentration of 5-7 mol / L, and the amount of sodium hydroxide added is 0.8-1.4 times the mass content of antimony in the slurry; and / or,

[0033] The stirring speed is 180-220 rpm.

[0034] Preferably, in step (6):

[0035] The acid solution is a hydrochloric acid solution with a concentration of 2-4 mol / L; and / or,

[0036] The stirring speed is 140-180 rpm.

[0037] Another aspect of the present invention discloses a system for the comprehensive recovery of lead anode mud, including a copper recovery system and an antimony-bismuth recovery system.

[0038] The copper recovery system includes a first receiving hopper and a pre-leaching kettle, a first filter press, an antimony and bismuth precipitation kettle, a second filter press, a copper replacement kettle, and a copper replacement filter tank, all equipped with inlets and outlets. The pre-leaching kettle, the first filter press, the antimony and bismuth precipitation kettle, the second filter press, the copper replacement kettle, and the copper replacement filter tank are connected sequentially by pipelines. The first filter press is also equipped with a first slag outlet, and the second filter press is also equipped with a second slag outlet. The first receiving hopper is connected to the first slag outlet of the first filter press.

[0039] The antimony-bismuth recovery system includes an antimony-bismuth slurry tank, a neutralization kettle, a neutralization filter tank, an antimony precipitation kettle, and an antimony precipitation filter tank connected in sequence by pipelines. The antimony-bismuth slurry tank is connected to the second slag outlet of the second filter press.

[0040] The pre-impregnation kettle, antimony and bismuth precipitation kettle, copper replacement kettle, neutralization kettle, and antimony precipitation kettle are all equipped with stirring devices.

[0041] Preferably, the hopper opening of the first hopper is located below the first slag outlet of the first filter press; the slurry tank opening of the antimony-bismuth slurry tank is located below the second slag outlet of the second filter press.

[0042] Preferably, the outlet of the copper replacement filter tank is connected to a first outlet pipe; the antimony precipitation filter tank is connected to a second outlet pipe; the copper recovery system further includes a first centrifugal pump installed on the pipeline between the pre-leaching tank and the first filter press, a second centrifugal pump installed on the pipeline between the antimony and bismuth precipitation tank and the second filter press, and a third centrifugal pump installed on the first outlet pipe; the antimony and bismuth recovery system further includes a fourth centrifugal pump installed on the pipeline between the antimony and bismuth slurry tank and the neutralization tank, a fifth centrifugal pump installed between the neutralization filter tank and the antimony precipitation tank, and a sixth centrifugal pump installed on the second outlet pipe.

[0043] Preferably, the pre-impregnation kettle, the antimony-bismuth precipitation reactor, the copper replacement kettle, and / or the antimony-bismuth slurry tank are all made of bisphenol A fiberglass; and / or,

[0044] The pre-impregnated slag hopper, copper replacement filter tank, neutralization filter tank, and antimony precipitation filter tank are all made of steel lined with PO material; and / or,

[0045] Both the first and second filter presses are water-washed diaphragm filter presses; and / or,

[0046] The neutralization vessel and the antimony precipitation vessel are both glass-lined jacketed reactors; and / or,

[0047] The first, second, third, fourth, fifth, and sixth centrifugal pumps are all engineering plastic pumps; and / or,

[0048] All the pipes mentioned are bisphenol A fiberglass pipes.

[0049] The beneficial effects of this invention are:

[0050] Using the apparatus and method disclosed in this invention, appropriate reagents are selected based on the inherent characteristics of each metal element for separation and purification, achieving the separation of silver and lead from antimony, bismuth, and copper in lead anode mud. The leaching residue, mainly composed of silver chloride and lead sulfate, is smelted by precipitation and remelting. The leaching solution mainly contains copper, antimony, and bismuth, with a copper-antimony-bismuth leaching rate exceeding 98%. After removing impurities from the copper, antimony and bismuth can be recovered and purified separately to produce high-purity products such as antimony trisulfide and bismuth oxychloride, with the bismuth oxychloride purity exceeding 98%. This process combines wet and pyrometallurgical treatment, achieving an antimony and bismuth recovery rate of over 99%. The entire process is controllable and highly effective, and the wastewater can be replenished and recycled, reaching a leading level in China. Attached Figure Description

[0051] Figure 1 This is a schematic diagram of the process flow of the method disclosed in this invention;

[0052] Figure 2 This is a schematic diagram showing the connection relationship of the various devices in the system disclosed in this invention. Detailed Implementation

[0053] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. The embodiments shown below do not limit the scope of the invention as described in the claims. Furthermore, the complete contents of the configurations illustrated in the following embodiments are not limited to those necessary for the solution of the invention as described in the claims.

[0054] Reference Appendix Figure 1 This invention provides a method for the comprehensive recycling of lead anode mud, comprising the following steps:

[0055] (1) Pre-impregnation: Hydrochloric acid solution, oxidant, and sodium salt solution are added to the lead anode mud, and the mixture is stirred and reacted at 65-85℃ (e.g., 68℃, 70℃, 75℃, 78℃, 80℃, 82℃, etc.) for 50-120 min (e.g., 60 min, 80 min, 90 min, 100 min, 110 min, etc.). Solid-liquid separation is then performed to obtain the pre-impregnation solution. The concentration of the hydrochloric acid is 2.5-4 mol / L (e.g., 2.8 mol / L, 3 mol / L, 3.2 mol / L, 3.5 mol / L, 3.8 mol / L, etc.); the oxidant has a mass concentration of 45-55% (e.g., 48%, 50%, 52%, 54%). The solution contains sodium chlorate (%), and the sodium salt solution is a saturated sodium chloride solution (saturated solution at room temperature); the mass ratio of the hydrochloric acid solution, oxidant, and sodium salt solution is 1:(0.13-0.3):(0.15-0.25) (e.g., 1:0.15:0.15, 1:0.18:0.17, 1:0.25:0.2, 1:0.28:0.24, etc.); the liquid-solid mass ratio of the pre-impregnation reaction system is controlled to be (3-5):1 (e.g., 3.5:1, 3.8:1, 4:1, 4.5:1, etc.); the stirring speed is 180-220 rpm (e.g., 190 rpm, 200 rpm, 210 rpm, 215 rpm, etc.).

[0056] (2) Antimony-bismuth precipitation: Adjust the pre-leaching solution to pH < 2.5 (e.g., 1, 1.5, 2, 2.2, etc.), and stir the reaction at 40-60℃ (e.g., 42℃, 45℃, 48℃, 50℃, 52℃, 55℃, 58℃, etc.) for 30-60 min (e.g., 35 min, 40 min, 45 min, 50 min, 55 min, etc.). Then, separate the solid and liquid to obtain the antimony-bismuth precipitation liquid and antimony-bismuth residue. The method for adjusting the pH of the pre-leaching solution is to add water to it. The stirring speed is 140-180 rpm (e.g., 145 rpm, 150 rpm, 155 rpm, 160 rpm, 170 rpm, 175 rpm, etc.).

[0057] (3) Copper replacement: Adjust the temperature of the solution after antimony and bismuth precipitation to 30-50℃ (e.g., 32℃, 35℃, 40℃, 45℃, 48℃, etc.), and add alkali to adjust the H. + The concentration is adjusted to 10-18 g / L (e.g., 12 g / L, 14 g / L, 16 g / L, 17 g / L, etc.), a displacement agent is added, and the mixture is stirred for 30-60 min (e.g., 35 min, 40 min, 45 min, 50 min, 55 min, etc.). Solid-liquid separation is then performed to obtain a copper-displaced liquid and copper slag. The alkali is sodium hydroxide, potassium hydroxide, and / or sodium carbonate. The displacement agent is iron powder with a particle size of 50-200 mesh (e.g., 50 mesh, 100 mesh, 150 mesh, 200 mesh, etc.). The amount of displacement agent added is 1.2-1.5 times (e.g., 1.25 times, 1.3 times, 1.35 times, 1.4 times, 1.45 times, etc.) the mass content of copper in the antimony-bismuth precipitated liquid. The stirring speed is 140-180 rpm (e.g., 145 rpm, 150 rpm, 155 rpm, 160 rpm, 170 rpm, etc.).

[0058] (4) Slurrying: Water is added to the antimony-bismuth slag and stirred to form a slurry; the mass ratio of water to antimony-bismuth slag is (1-1.5):1 (e.g., 1.2:1, 1.3:1, 1.4:1, etc.); the stirring speed is 80-120 rpm (e.g., 85 rpm, 90 rpm, 95 rpm, 100 rpm, 105 rpm, 110 rpm, etc.); the stirring time is 20-40 min (e.g., 25 min, 30 min, 35 min, 38 min, etc.).

[0059] (5) Neutralization: Add an alkaline solution to the slurry and stir for 40-80 min (e.g., 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, etc.), then separate the solid and liquid to obtain bismuth slag and antimony-containing liquid; the alkaline solution is a sodium hydroxide solution with a concentration of 5-7 mol / L (e.g., 5.2 mol / L, 5.5 mol / L, 6 mol / L, 6.2 mol / L, 6.5 mol / L, 6.8 mol / L, etc.), and the amount of sodium hydroxide added is 0.8-1.4 times (e.g., 0.9 times, 1 times, 1.1 times, 1.2 times, 1.3 times, etc.) of the antimony mass content in the slurry; the stirring speed is 180-220 rpm (e.g., 185 rpm, 190 rpm, 195 rpm, 200 rpm, 205 rpm, 210 rpm, etc.).

[0060] (6) Antimony precipitation: Add an acid solution to the antimony-containing solution to adjust the pH to 2.0-2.5 (e.g., 2.1, 2.2, 2.3, 2.4, etc.), and stir the reaction at 30-60℃ (e.g., 35℃, 40℃, 45℃, 50℃, 55℃, etc.) for 30-60 min (e.g., 35 min, 40 min, 45 min, 50 min, 55 min, etc.). Then, perform solid-liquid separation to obtain the antimony-precipitated liquid and antimony slag. The acid solution is a hydrochloric acid solution with a concentration of 2-4 mol / L (e.g., 2.2 mol / L, 2.5 mol / L, 2.8 mol / L, 3 mol / L, 3.2 mol / L, 3.5 mol / L, 3.8 mol / L, etc.); the stirring speed is 140-180 rpm (e.g., 145 rpm, 150 rpm, 160 rpm, 165 rpm, 170 rpm, 175 rpm, etc.).

[0061] The method of the present invention will be further explained below through specific embodiments. Embodiments 1-3 of the present invention were carried out in the laboratory, and Embodiments 4-7 were completed using the system disclosed in the present invention.

[0062] Example 1

[0063] A method for the comprehensive recovery of lead anode mud includes the following steps:

[0064] (1) Take 100g of lead anode mud into a 1000ml three-necked flask, add 310ml of 3mol / L hydrochloric acid solution, 55ml of 50% sodium chlorate solution and 47ml of sodium chloride solution to the three-necked flask in sequence, raise the temperature to 70℃, turn on the stirrer, the stirring speed is 180rpm, the stirring time is 50min, after the reaction is completed, the solid and liquid are separated, the pre-impregnated residue is washed once with water to produce a first washing liquid, and the pre-impregnated residue is further processed.

[0065] (2) The first washing solution and the pre-soaking solution were added together into a new three-necked flask, production water was added, the pH value was controlled at 2.3, the stirring was turned on, the stirring speed was 150 rpm, the stirring time was 30 min, the temperature was 40℃, the reaction was completed, the solid and liquid were separated, the antimony bismuth precipitate was washed twice with water to produce a second washing solution, and the antimony bismuth precipitate was further processed.

[0066] (3) Add the second washing solution and the solution after antimony and bismuth precipitation together to a new three-necked flask, heat to 30°C, start stirring, stir at 140 rpm for 30 min, add sodium hydroxide to adjust the acid concentration of the solution (referring to H+). + (Concentration, the same below) 12g / L, add iron powder, the amount of iron powder is 1.2 times the amount of copper in the solution. After the reaction is complete, the solid and liquid are separated, the copper slag is further processed, and the liquid after replacement is poured into the wastewater discharge system.

[0067] (4) The antimony-bismuth slag from step (2) is added to a new three-necked flask. The mass ratio of production water to antimony-bismuth slag is 1:1. Stirring is started at 80 rpm for 20 min. Then, 6 mol / L sodium hydroxide solution is added. The amount of sodium hydroxide added is 0.8 times the amount of antimony in the solution. The stirring speed is increased to 180 rpm for 40 min. After the reaction is completed, the solid and liquid are separated, and the bismuth slag is further processed.

[0068] (5) The neutralized liquid from step (4) is added to a new three-necked flask, heated to 30°C, stirred at 140 rpm, and 3 mol / L hydrochloric acid solution is added to adjust the pH to 2.1. The stirring time is 30 min. After the reaction is complete, the solid and liquid are separated, the antimony slag is further processed, and the antimony precipitated liquid is poured into the wastewater treatment system.

[0069] Experimental results showed that the copper-antimony-bismuth leaching rate in this embodiment was 98.2%, and the recovery rate was 99.1%.

[0070] Example 2

[0071] (1) Take 100g of lead anode mud into a 1000ml three-necked flask, add 410ml of 3mol / L hydrochloric acid solution, 61ml of 50% sodium chlorate solution and 66ml of sodium chloride solution to the three-necked flask in sequence, raise the temperature to 75℃, turn on the stirrer, the stirring speed is 200rpm, the stirring time is 50min, after the reaction is completed, the solid and liquid are separated, the pre-impregnated residue is washed once with water to produce a first washing liquid, and the pre-impregnated residue is further processed.

[0072] (2) The first washing solution and the pre-soaking solution are added together into a new three-necked flask, production water is added, the pH value is controlled at 2.3, the stirring is turned on, the stirring speed is 150 rpm, the stirring time is 45 min, the temperature is 48℃, the reaction is completed, the solid and liquid are separated, the antimony bismuth precipitate is washed twice with water to produce a second washing solution, and the antimony bismuth precipitate is further processed.

[0073] (3) The second washing solution and the antimony-bismuth precipitation solution were added together into a new three-necked flask, heated to 39°C, stirred at 160 rpm for 45 min, sodium hydroxide was added to adjust the acid concentration of the solution to 15 g / L, iron powder was added, the amount of iron powder was 1.32 times the amount of copper in the solution, after the reaction was completed, the solid and liquid were separated, the copper slag was further processed, and the replacement liquid was poured into the wastewater discharge system.

[0074] (4) The antimony-bismuth slag from step (2) is added to a new three-necked flask. The mass ratio of production water to antimony-bismuth slag is 1:1. Stirring is started at 90 rpm for 30 min. Then, 6 mol / L sodium hydroxide solution is added. The amount of sodium hydroxide added is 1.34 times the amount of antimony in the solution. The stirring speed is increased to 195 rpm for 56 min. After the reaction is completed, the solid and liquid are separated, and the bismuth slag is further processed.

[0075] (5) The neutralized liquid from step (4) is added to a new three-necked flask, heated to 46°C, stirred at 167 rpm, 3 mol / L hydrochloric acid solution is added, the pH value is adjusted to 2.2, and the stirring time is 47 min. After the reaction is complete, the solid and liquid are separated, the antimony slag is further processed, and the antimony precipitated liquid is poured into the wastewater treatment system.

[0076] Experimental results showed that the copper-antimony-bismuth leaching rate in this embodiment was 98.5%, and the recovery rate was 99.3%.

[0077] Example 3

[0078] (1) Take 100g of lead anode mud into a 1000ml three-necked flask, add 435ml of 3mol / L hydrochloric acid solution, 82ml of 50% sodium chlorate solution and 85ml of sodium chloride solution to the three-necked flask in sequence, raise the temperature to 85℃, turn on the stirrer, the stirring speed is 220rpm, the stirring time is 120min, after the reaction is completed, the solid and liquid are separated, the pre-impregnated residue is washed once with water to produce a first washing liquid, and the pre-impregnated residue is further processed.

[0079] (2) The first washing solution and the pre-soaking solution were added together into a new three-necked flask, production water was added, the pH value was controlled at 2.4, the stirring was turned on, the stirring speed was 180 rpm, the stirring time was 58 min, the temperature was 56℃, the reaction was completed, the solid and liquid were separated, the antimony bismuth precipitate was washed twice with water to produce a second washing solution, and the antimony bismuth precipitate was further processed.

[0080] (3) The second washing solution and the antimony-bismuth precipitation solution were added together into a new three-necked flask, heated to 49°C, stirred at 178 rpm for 58 min, sodium hydroxide was added to adjust the acid concentration of the solution to 18 g / L, iron powder was added, the amount of iron powder was 1.47 times the amount of copper in the solution, after the reaction was completed, the solid and liquid were separated, the copper slag was further processed, and the replacement liquid was poured into the wastewater discharge system.

[0081] (4) The antimony bismuth slag from step (2) is added to a new three-necked flask. The mass ratio of production water to antimony bismuth slag is 1:1. Stirring is started at 137 rpm for 39 min. Then, 6 mol / L sodium hydroxide solution is added. The amount of sodium hydroxide added is 1.35 times the amount of antimony in the solution. The stirring speed is increased to 220 rpm for 75 min. After the reaction is completed, the solid and liquid are separated, and the bismuth slag is further processed.

[0082] (5) The neutralized liquid from step (4) is added to a new three-necked flask, heated to 58°C, stirred at 175 rpm, 3 mol / L hydrochloric acid solution is added, the pH value is adjusted to 2.4, and the stirring time is 55 min. After the reaction is complete, the solid and liquid are separated, the antimony slag is further processed, and the antimony precipitated liquid is poured into the wastewater treatment system.

[0083] Experimental results showed that the copper-antimony-bismuth leaching rate in this embodiment was 99%, and the recovery rate was 99.6%.

[0084] Example 4

[0085] A method for the comprehensive recovery of lead anode mud includes the following steps:

[0086] (1) Place the lead anode mud in a pre-immersion kettle 1, add hydrochloric acid solution, oxidant and sodium salt to the pre-immersion kettle 1, heat the pre-immersion kettle 1 to 65-85℃ and start stirring, the stirring speed is 180-220rpm, the stirring time is 50-120min, after the reaction is completed, the solid and liquid are separated, the material in the pre-immersion kettle 1 is pumped into the first filter press 3 through the first centrifugal pump 2 for filtration, to obtain pre-immersion residue and pre-immersion liquid, the pre-immersion residue enters the pre-immersion residue receiving hopper 4, and the pre-immersion liquid enters the antimony and bismuth precipitation reactor 5. The concentration of hydrochloric acid is 3mol / L, the sodium salt is a saturated sodium chloride solution, the oxidant is a 50% sodium chlorate solution, the liquid-solid ratio is 3-5:1; the mass ratio of hydrochloric acid:sodium chlorate:sodium chloride solution is 1:0.13-0.3:0.15-0.25.

[0087] (2) After the pre-impregnation liquid is pumped into the antimony-bismuth precipitation reactor 5, production water is added, the pH value is controlled, the stirring is turned on, the stirring speed is 140-180 rpm, the stirring time is 30-60 min, the temperature is 40-60℃, after the reaction is completed, the slurry is pumped into the second filter press 7 through the second centrifugal pump 6 for filter washing, the antimony-bismuth precipitation liquid and the first washing liquid are pumped into the copper replacement reactor 9, and the antimony-bismuth slag enters the antimony-bismuth slurry tank 8, wherein the reaction pH value is controlled <2.5.

[0088] (3) The antimony-bismuth precipitation solution and the first washing solution are pumped into the copper displacement reactor 9, heated to 30-50℃, and alkali is added to adjust the acid concentration. Stirring is started at 140-180 rpm for 30-60 min. The displacement agent is added. After the reaction is complete, solid-liquid separation is performed through the copper displacement filter tank 10. The filter residue is further processed, and the filtrate is sent to the wastewater treatment system through the third centrifugal pump 16. The alkali is sodium hydroxide, potassium hydroxide, or sodium carbonate. Sodium hydroxide is used in this process. The acid concentration is adjusted to 10 g / L-18 g / L. The displacement agent is iron powder. The iron powder is sieved through a 100-mesh sieve, and the amount of iron powder added is 1.2-1.5 times the amount of copper in the solution.

[0089] (4) Antimony-bismuth slag is added to slurry tank 8, production water is added, and stirring is started at a speed of 80-120 rpm for 20-40 min. Then, the material is pumped into neutralization tank 11 through the fourth centrifugal pump 17. A strong alkali solution is added to neutralization tank 11, and stirring is started at a speed of 180-220 rpm for 40-80 min. After the reaction is completed, bismuth slag is produced by solid-liquid separation through neutralization filter tank 12. The bismuth slag is further processed, and the filtrate is pumped into antimony settling tank 13 through the fifth centrifugal pump 18. The mass ratio of production water to antimony-bismuth slag is 1:1, the strong alkali is a 6 mol / L sodium hydroxide solution, and the amount of sodium hydroxide added is 0.8-1.4 times the amount of antimony.

[0090] (5) After the filtrate is pumped into the antimony precipitation vessel 13, the temperature is raised to 30-60℃, stirring is started at a speed of 140-180 rpm, a strong acid is added, the pH value is controlled, and the stirring time is 30-60 min. After the reaction is complete, solid-liquid separation is performed through the antimony precipitation filter tank 14. The filter residue is further processed, and the filtrate is sent to the waste liquid treatment system through the sixth centrifugal pump 15. The strong acid is a 3 mol / L hydrochloric acid solution, and the pH value is controlled at 2.0-2.5.

[0091] Experimental testing showed that the copper-antimony-bismuth leaching rate in this embodiment was over 98%, and the recovery rate was over 99%.

[0092] Example 5

[0093] A method for the comprehensive recovery of lead anode mud includes the following steps:

[0094] (1) Pre-impregnation: Hydrochloric acid solution, oxidant and sodium salt solution are added to lead anode mud, and the mixture is stirred at 68°C for 60 min. Then the solid and liquid are separated to obtain the pre-impregnation solution. The concentration of the hydrochloric acid is 2.8 mol / L. The oxidant is a sodium chlorate solution with a mass concentration of 48%. The sodium salt solution is a saturated sodium chloride solution. The mass ratio of the hydrochloric acid solution, oxidant and sodium salt solution is 1:0.13:0.18. The liquid-solid ratio of the pre-impregnation reaction system is controlled at 3.5:1. The stirring speed is 190 rpm.

[0095] (2) Antimony-bismuth precipitation: Adjust the pre-impregnation solution to pH=1-2, stir and react at 45℃ for 35min, and then separate the solid and liquid to obtain antimony-bismuth precipitation liquid and antimony-bismuth residue; the method of adjusting the pH of the pre-impregnation solution is to add water to it; the stirring speed is 150rpm.

[0096] (3) Copper replacement: Adjust the temperature of the antimony-bismuth precipitated liquid to 35℃, add alkali to adjust the acid concentration to 12g / L, add replacement agent, stir and react for 35min, and then separate the solid and liquid to obtain copper-replaced liquid and copper slag; the alkali is sodium hydroxide; the replacement agent is iron powder with a particle size of 50 mesh; the amount of replacement agent added is 1.2 times the copper content in the antimony-bismuth precipitated liquid; the stirring speed is 145rpm.

[0097] (4) Slurrying: Water is added to the antimony bismuth slag and stirred to slurry to obtain a slurry; the mass ratio of water to antimony bismuth slag is 1:1; the stirring speed is 80 rpm; the stirring time is 20 min.

[0098] (5) Neutralization: Add an alkaline solution to the slurry, stir and react for 40 min, then separate the solid and liquid to obtain bismuth slag and antimony-containing liquid; the alkaline solution is a sodium hydroxide solution with a concentration of 5 mol / L, and the amount of sodium hydroxide added is 0.8 times the amount of antimony in the slurry; the stirring speed is 180 rpm.

[0099] (6) Antimony precipitation: Add acid solution to the antimony-containing liquid to adjust the pH to 2.0, stir the reaction at 30℃ for 30 min, and then perform solid-liquid separation to obtain the antimony-precipitated liquid and antimony slag. The acid solution is a 2 mol / L hydrochloric acid solution; the stirring speed is 140 rpm.

[0100] Experimental results showed that the copper-antimony-bismuth leaching rate in this embodiment was 99.3%, and the recovery rate was 99.6%.

[0101] Example 6

[0102] A method for the comprehensive recovery of lead anode mud includes the following steps:

[0103] (1) Pre-impregnation: Hydrochloric acid solution, oxidant and sodium salt solution are added to lead anode mud, and the mixture is stirred at 72°C for 85 min. Then the solid and liquid are separated to obtain the pre-impregnation solution. The concentration of the hydrochloric acid is 3.2 mol / L. The oxidant is a sodium chlorate solution with a mass concentration of 50%. The sodium salt solution is a saturated sodium chloride solution. The mass ratio of the hydrochloric acid solution, oxidant and sodium salt solution is 1:0.25:0.2. The liquid-solid ratio of the pre-impregnation reaction system is controlled at 4:1. The stirring speed is 200 rpm.

[0104] (2) Antimony-bismuth precipitation: Adjust the pre-impregnation solution to pH < (1.5-2.2), stir the reaction at 50℃ for 45 min, and then separate the solid and liquid to obtain the antimony-bismuth precipitation liquid and antimony-bismuth slag; the method of adjusting the pH of the pre-impregnation solution is to add water to it; the stirring speed is 160 rpm.

[0105] (3) Copper replacement: Adjust the temperature of the antimony-bismuth precipitated liquid to 40℃, add alkali to adjust the acid concentration to 15g / L, add replacement agent, stir and react for 45min, and then separate the solid and liquid to obtain copper replacement liquid and copper slag; the alkali is potassium hydroxide; the replacement agent is iron powder with a particle size of 150 mesh; the amount of replacement agent added is 1.3 times the copper content in the antimony-bismuth precipitated liquid; the stirring speed is 160rpm.

[0106] (4) Slurrying: Water is added to the antimony bismuth slag and stirred to slurry to obtain a slurry; the mass ratio of water to antimony bismuth slag is 1.3:1; the stirring speed is 100 rpm; and the stirring time is 30 min.

[0107] (5) Neutralization: Add an alkaline solution to the slurry, stir and react for 60 min, then separate the solid and liquid to obtain bismuth slag and antimony-containing liquid; the alkaline solution is a sodium hydroxide solution with a concentration of 6 mol / L, and the amount of sodium hydroxide added is 1.2 times the amount of antimony in the slurry; the stirring speed is 200 rpm.

[0108] (6) Antimony precipitation: Add an acid solution to the antimony-containing liquid to adjust the pH to 2.1-2.3, stir the reaction at 45℃ for 45 min, and then perform solid-liquid separation to obtain the antimony-precipitated liquid and antimony slag. The acid solution is a 3 mol / L hydrochloric acid solution; the stirring speed is 160 rpm.

[0109] Experimental results showed that the copper-antimony-bismuth leaching rate in this embodiment was 98.7%, and the recovery rate was 99.4%.

[0110] Example 7

[0111] A method for the comprehensive recovery of lead anode mud includes the following steps:

[0112] (1) Pre-impregnation: Hydrochloric acid solution, oxidant and sodium salt solution are added to lead anode mud, and the mixture is stirred at 85°C for 120 min. Then the solid and liquid are separated to obtain the pre-impregnation solution. The concentration of the hydrochloric acid is 4 mol / L. The oxidant is a sodium chlorate solution with a mass concentration of 55%. The sodium salt solution is a saturated sodium chloride solution. The mass ratio of the hydrochloric acid solution, oxidant and sodium salt solution is 1:-0.3:0.25. The liquid-solid ratio of the pre-impregnation reaction system is controlled at 5:1. The stirring speed is 220 rpm.

[0113] (2) Antimony-bismuth precipitation: Adjust the pre-impregnation solution to pH < (2.4-2.5), stir the reaction at 60℃ for 60 min, and then separate the solid and liquid to obtain the antimony-bismuth precipitation liquid and antimony-bismuth slag; the method of adjusting the pH of the pre-impregnation solution is to add water to it; the stirring speed is 180 rpm.

[0114] (3) Copper replacement: Adjust the temperature of the antimony-bismuth precipitated liquid to 50℃, add alkali to adjust the acid concentration to 18g / L, add replacement agent, stir and react for 60min, and then separate the solid and liquid to obtain copper-replaced liquid and copper slag; the alkali is sodium hydroxide, potassium hydroxide and sodium carbonate; the replacement agent is iron powder with a particle size of 200 mesh; the amount of replacement agent added is 1.5 times the copper content in the antimony-bismuth precipitated liquid; the stirring speed is 180rpm.

[0115] (4) Slurrying: Water is added to the antimony bismuth slag and stirred to slurry to obtain a slurry; the mass ratio of water to antimony bismuth slag is 1.5:1; the stirring speed is 120 rpm; and the stirring time is 40 min.

[0116] (5) Neutralization: Add an alkaline solution to the slurry, stir and react for 80 min, then separate the solid and liquid to obtain bismuth slag and antimony-containing liquid; the alkaline solution is a sodium hydroxide solution with a concentration of 7 mol / L, and the amount of sodium hydroxide added is 1.4 times the amount of antimony in the slurry; the stirring speed is 220 rpm.

[0117] (6) Antimony precipitation: Add an acid solution to the antimony-containing liquid to adjust the pH to 2.5, stir the reaction at 60°C for 60 min, and then perform solid-liquid separation to obtain the antimony-precipitated liquid and antimony slag. The acid solution is a 4 mol / L hydrochloric acid solution; the stirring speed is 180 rpm.

[0118] Experimental results showed that the copper-antimony-bismuth leaching rate in this embodiment was 98.8%, and the recovery rate was 99.3%.

[0119] Reference Appendix Figure 2In another aspect, this invention also discloses a comprehensive lead anode mud recovery system, including a copper recovery system and an antimony-bismuth recovery system. The copper recovery system includes a first receiving hopper 4 and a pre-impregnation tank 1, a first filter press 3, an antimony-bismuth precipitation tank 5, a second filter press 7, a copper replacement tank 9, and a copper replacement filter tank 10, all equipped with inlets and outlets. The pre-impregnation tank 1, the first filter press 3, the antimony-bismuth precipitation tank 5, the second filter press 7, the copper replacement tank 9, and the copper replacement filter tank 10 are connected sequentially by pipelines. The first filter press 3 is also equipped with... The first filter press 3 has a first slag outlet, and the second filter press 7 also has a second slag outlet; the first receiving hopper 4 is connected to the first slag outlet of the first filter press 3; the antimony-bismuth recovery system includes an antimony-bismuth slurry tank 8, a neutralization kettle 11, a neutralization filter tank 12, an antimony precipitation kettle 13, and an antimony precipitation filter tank 14 connected in sequence by pipes, and the antimony-bismuth slurry tank 8 is connected to the second slag outlet of the second filter press 7; the pre-impregnation kettle 1, the antimony-bismuth precipitation kettle 5, the copper replacement kettle 9, the neutralization kettle 11, and the antimony precipitation kettle 13 are all equipped with stirring devices.

[0120] In one embodiment of the present invention, the hopper 4 opening of the first hopper 4 is located below the first slag outlet of the first filter press 3; the slurry tank 8 opening is located below the second slag outlet of the second filter press 7.

[0121] In one embodiment of the present invention, the outlet of the copper replacement filter tank 10 is connected to a first outlet pipe; the antimony precipitation filter tank 14 is connected to a second outlet pipe; the copper recovery system further includes a first centrifugal pump 2 disposed on a pipe between the pre-leaching tank 1 and the first filter press 3, a second centrifugal pump 6 disposed on a pipe between the antimony and bismuth precipitation tank 5 and the second filter press 7, and a third centrifugal pump 16 disposed on the first outlet pipe; the antimony and bismuth recovery system further includes a fourth centrifugal pump 17 disposed on a pipe between the antimony and bismuth slurry tank 8 and the neutralization tank 11, a fifth centrifugal pump 18 disposed between the neutralization filter tank 12 and the antimony precipitation tank 13, and a sixth centrifugal pump 15 disposed on the second outlet pipe.

[0122] In one embodiment of the present invention, the pre-impregnation kettle 1, the antimony-bismuth precipitation reactor, the copper replacement kettle 9, and / or the antimony-bismuth slurry tank 8 are all made of bisphenol A fiberglass; the pre-impregnation slag hopper, the copper replacement filter tank 10, the neutralization filter tank 12, and the antimony precipitation filter tank 14 are all made of steel-lined PO material; the first filter press 3 and the second filter press 7 are both water-washed diaphragm filter presses; the neutralization kettle 11 and the antimony precipitation kettle 13 are both glass-lined jacketed reactors; the first centrifugal pump 2, the second centrifugal pump 6, the third centrifugal pump 16, the fourth centrifugal pump 17, the fifth centrifugal pump 18, and the sixth centrifugal pump 15 are all engineering plastic pumps; and all pipelines are bisphenol A fiberglass pipelines.

[0123] The method for comprehensive recovery of lead anode mud disclosed in this invention is preferably carried out using the system disclosed in this invention.

[0124] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for the comprehensive recovery of lead anode mud, characterized in that, Includes the following steps: (1) Pre-soaking: Add hydrochloric acid solution, oxidant and sodium salt solution to lead anode mud, stir and react at 65-85℃ for 50-120 min, then separate solid and liquid to obtain pre-soaking solution; the concentration of hydrochloric acid is 2.5-4 mol / L; the oxidant is sodium chlorate solution with a mass concentration of 45-55%; The sodium salt solution is a saturated sodium chloride solution; The mass ratio of the hydrochloric acid solution, oxidant, and sodium salt solution is 1:(0.13-0.3):(0.15-0.25); the liquid-solid mass ratio of the pre-impregnation reaction system is controlled to be (3-5):1; the stirring speed is 180-220 rpm. (2) Antimony-bismuth precipitation: Adjust the pre-impregnation solution to pH < 2.5, stir and react at 40-60℃ for 30-60 min, then separate the solid and liquid to obtain antimony-bismuth precipitation liquid and antimony-bismuth residue; the method of adjusting the pH of the pre-impregnation solution is to add water to it; the stirring speed is 140-180 rpm; (3) Copper replacement: Adjust the temperature of the solution after antimony and bismuth precipitation to 30-50℃, and add alkali to adjust the H. + The concentration is brought to 10-18 g / L, and a displacement agent is added. The displacement agent is iron powder with a particle size of 50-200 mesh. The amount of displacement agent added is 1.2-1.5 times the mass content of copper in the antimony-bismuth precipitated liquid. The mixture is stirred and reacted for 30-60 min. Then, the solid and liquid are separated to obtain copper-substituted liquid and copper slag. (4) Slurrying: Water is added to the antimony bismuth slag and stirred to form a slurry; (5) Neutralization: Add an alkaline solution to the slurry, wherein the alkaline solution is a sodium hydroxide solution with a concentration of 5-7 mol / L, and the amount of sodium hydroxide added is 0.8-1.4 times the mass content of antimony in the slurry. Stir the reaction for 40-80 min, and then separate the solid and liquid to obtain bismuth slag and antimony-containing liquid. (6) Antimony precipitation: Add acid solution to antimony-containing liquid, adjust pH to 2.0-2.5, stir reaction at 30-60℃ for 30-60 min, and then perform solid-liquid separation to obtain antimony-precipitated liquid and antimony slag.

2. The method for comprehensive recovery of lead anode mud according to claim 1, characterized in that, In step (3) The stirring speed is 140-180 rpm.

3. The method for comprehensive recovery of lead anode mud according to claim 1, characterized in that, In step (4) The mass ratio of water to antimony-bismuth slag is (1-1.5):1; The stirring speed is 80-120 rpm; the stirring time is 20-40 min.

4. The method for comprehensive recovery of lead anode mud according to claim 1, characterized in that, In step (5) The stirring speed is 180-220 rpm.

5. The method for comprehensive recovery of lead anode mud according to claim 1, characterized in that, In step (6) The acid solution is a hydrochloric acid solution with a concentration of 2-4 mol / L; The stirring speed is 140-180 rpm.

6. A system for comprehensively recovering lead anode mud according to any one of claims 1-5, characterized in that, Including copper recovery systems and antimony-bismuth recovery systems, The copper recovery system includes a first receiving hopper and a pre-leaching kettle, a first filter press, an antimony and bismuth precipitation kettle, a second filter press, a copper replacement kettle, and a copper replacement filter tank, all equipped with inlets and outlets. The pre-leaching kettle, the first filter press, the antimony and bismuth precipitation kettle, the second filter press, the copper replacement kettle, and the copper replacement filter tank are connected sequentially by pipelines. The first filter press is also equipped with a first slag outlet, and the second filter press is also equipped with a second slag outlet. The first receiving hopper is connected to the first slag outlet of the first filter press. The antimony-bismuth recovery system includes an antimony-bismuth slurry tank, a neutralization kettle, a neutralization filter tank, an antimony precipitation kettle, and an antimony precipitation filter tank connected in sequence by pipelines. The antimony-bismuth slurry tank is connected to the second slag outlet of the second filter press. The pre-impregnation kettle, antimony and bismuth precipitation kettle, copper replacement kettle, neutralization kettle, and antimony precipitation kettle are all equipped with stirring devices.

7. A system for the comprehensive recovery of lead anode mud according to claim 6, characterized in that, The hopper opening of the first receiving hopper is located below the first slag outlet of the first filter press; the slurry tank opening of the antimony-bismuth slurry tank is located below the second slag outlet of the second filter press.

8. A system for the comprehensive recovery of lead anode mud according to claim 6, characterized in that, The copper replacement filter tank has a first outlet pipe connected to its outlet; the antimony precipitation filter tank has a second outlet pipe connected to its outlet; the copper recovery system also includes a first centrifugal pump installed on the pipeline between the pre-leaching tank and the first filter press, a second centrifugal pump installed on the pipeline between the antimony and bismuth precipitation tank and the second filter press, and a third centrifugal pump installed on the first outlet pipe; the antimony and bismuth recovery system also includes a fourth centrifugal pump installed on the pipeline between the antimony and bismuth slurry tank and the neutralization tank, a fifth centrifugal pump installed between the neutralization filter tank and the antimony precipitation tank, and a sixth centrifugal pump installed on the second outlet pipe.

9. A system for the comprehensive recovery of lead anode mud according to claim 8, characterized in that, The pre-impregnation kettle, the antimony-bismuth precipitation reactor, the copper replacement kettle, and the antimony-bismuth slurry tank are all made of bisphenol A fiberglass. The pre-impregnation slag hopper, copper replacement filter tank, neutralization filter tank, and antimony precipitation filter tank are all made of steel lined with PO material. Both the first and second filter presses are water-washed diaphragm filter presses; Both the neutralization vessel and the antimony precipitation vessel are glass-lined jacketed reactors. The first, second, third, fourth, fifth, and sixth centrifugal pumps mentioned above are all engineering plastic pumps; All the pipes mentioned are bisphenol A fiberglass pipes.

Citation Information

Patent Citations

  • Method for enriching gold and silver by floating anode mud and recycling antimony and bismuth

    CN102041387A

  • Method for recycling valuable metals from lead anode slime

    CN102925703A

  • Silver anode slime treatment method and treatment system

    CN116676483A

  • System for comprehensively recovering lead anode slime

    CN222411748U