Method and device for characterizing the quality of SEI film formation at solid electrolyte interface
By analyzing the voltage and capacity data of lithium-ion batteries during the charge and discharge process, the decomposed charge transfer capacity and impedance of the SEI film are calculated to directly characterize the quality of the SEI film formation and solve the problem of low efficiency in evaluating the quality of the SEI layer film formation in the existing technology. , improving battery cycle storage performance and service life.
Patent Information
- Application Number
- CN202410670667.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-05-28
AI Technical Summary
It is difficult to efficiently evaluate the film-forming quality of the SEI layer in lithium-ion batteries with existing technology, resulting in poor battery cycle storage performance and short service life.
By analyzing the voltage and capacity data of the battery during charging and discharging, the decomposed charge transfer capacity and decomposition impedance of the SEI film are calculated, and the SEI film formation quality is directly characterized by combining the film quality characterization value with the ratio of the SEI decomposed charge transfer capacity and impedance. , improve assessment efficiency and accuracy.
It achieves rapid and accurate evaluation of SEI film-forming quality, improves the cycle storage performance and service life of the battery, and reduces evaluation time and cost.
Smart Images

Figure CN118244140B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and specifically to a method and device for characterizing the quality of SEI (Solid Electrolyte Interface) film formation. Background Art
[0002] The negative electrode active material of lithium-ion batteries is often graphite. During the initial formation, graphite will undergo an irreversible side reaction with the electrolyte and form a SEI layer.
[0003] A SEI layer with good quality can effectively reduce the irreversible lithium consumption of the negative electrode during long-term cycle storage of the battery and increase the service life of the battery. Summary of the invention
[0004] The present application provides a method and device for characterizing the quality of SEI film formation, which improves the efficiency of SEI film formation quality assessment.
[0005] In the first aspect, the present application provides a method for characterizing the quality of SEI film formation, comprising: determining the amount of lithium depleted from graphite from the beginning of charging to the end of the delithiation voltage platform based on the voltage data and capacity data of a test battery during the charging process; obtaining the SEI decomposition charge transfer amount based on the delithiation amount and the total lithium insertion amount of the test battery; determining the SEI decomposition impedance based on the voltage data, capacity data and delithiation current; determining a film formation quality characterization value based on the SEI decomposition charge transfer amount and the SEI decomposition impedance, wherein the film formation quality characterization value is negatively correlated with the SEI decomposition charge transfer amount, and positively correlated with the SEI decomposition impedance.
[0006] In the technical solution of the embodiment of the present application, the charge transferred by SEI film decomposition and the SEI film decomposition impedance can be obtained according to the voltage and capacity data of the battery during the lithium insertion and delithiation process. Based on the fact that the film quality characterization value is negatively correlated with the SEI decomposition charge transferred and positively correlated with the SEI decomposition impedance, the film quality characterization value is obtained to improve the efficiency of SEI film quality assessment.
[0007] In some embodiments, based on the voltage data and capacity data of the test battery during the charging process, determining the amount of lithium depleted from the graphite from the start of charging to the end of the delithiation voltage platform includes: obtaining the rate of change of voltage change relative to the capacity change; based on the rate of change and the capacity data, obtaining a first curve of the rate of change versus capacity; and determining the capacity corresponding to the valley value of the rate of change in the first curve as the amount of lithium depletion.
[0008] In the technical solution of the embodiment of the present application, the amount of electricity released by graphite from full lithium insertion to deviation from the delithiation voltage platform can be determined based on the voltage and capacity data during the delithiation process, and then the amount of charge transferred by the decomposition of the SEI film can be obtained in combination with the amount of electricity of the graphite fully inserted with lithium, thereby improving the accuracy and efficiency of the determined amount of charge transferred by the decomposition of the SEI film, and thus improving the accuracy and efficiency of the SEI film quality assessment.
[0009] In some embodiments, determining the SEI decomposition impedance based on voltage data, capacity data and delithiation current includes: obtaining the rate of change of voltage change relative to capacity change; obtaining a second curve of the rate of change as a inverse of voltage based on the rate of change and voltage data; determining the peak value of the rate of change when the voltage in the second curve is greater than a threshold value; and obtaining the ratio of the peak value to the delithiation current as the SEI decomposition impedance.
[0010] In the technical solution of the embodiment of the present application, the decomposition resistance of SEI entering the electrodecomposition stage can be determined based on the voltage and capacity data during the delithiation process, and then the SEI decomposition impedance is obtained by normalizing the delithiation current, thereby improving the accuracy of the SEI decomposition impedance, which is beneficial to improving the accuracy of the SEI film quality assessment.
[0011] In some embodiments, determining the film quality characterization value according to the SEI decomposition charge transfer amount and the SEI decomposition impedance includes: determining a ratio of the SEI decomposition impedance to the SEI decomposition charge transfer amount as the film quality characterization value.
[0012] In the technical solution of the embodiment of the present application, the film quality characterization value can be determined by calculating the ratio of SEI decomposition impedance and SEI decomposition charge transfer quantity, which has low computational complexity and is conducive to improving the efficiency of determining the film quality characterization value.
[0013] In some embodiments, the characterization method further includes: performing a charging operation on the test battery, wherein a delithiation voltage range during the charging process exceeds a normal use range of the test battery.
[0014] In the technical solution of the embodiment of the present application, the graphite electrode can be fully delithiated by charging operations exceeding the normal use range of the test battery to reach the SEI film electrolysis stage, thereby improving the accuracy of the charge transferred by the SEI film decomposition, and thereby improving the accuracy of the SEI film quality assessment.
[0015] In some embodiments, the characterization method further includes: before performing the charging operation, performing a discharge operation on the test battery and obtaining a total lithium insertion amount.
[0016] In the technical solution of the embodiment of the present application, before performing the charging operation, the test battery can be formed through a discharge operation to produce a SEI film, and the accuracy of the data collected in the subsequent charging can be improved by leaving it in a static stable state; in addition, the amount of electricity fully embedded in the graphite based on the discharge operation is beneficial to improving the accuracy of the data used in the subsequent calculation of the amount of charge transferred by the decomposition of the SEI film.
[0017] In some embodiments, the charging operation includes: charging the test battery with a charging current to a normal operating voltage of the test battery; charging the test battery with a delithiation current to a first voltage, wherein the charging current is greater than the delithiation current, and the first voltage is greater than the normal operating voltage of the test battery.
[0018] In the technical solution of the embodiment of the present application, after the test battery is charged to the normal operating voltage with a larger charging current, it is then charged to a first voltage exceeding the normal operating voltage with a smaller delithiation current, thereby shortening the time required to charge to the first voltage and improving the charging efficiency.
[0019] In some embodiments, the charging operation includes: charging the test battery with a delithiation current to a first voltage, wherein the first voltage is greater than a normal operating voltage of the test battery.
[0020] In the technical solution of the embodiment of the present application, the test battery is charged by a constant lithium removal current, which simplifies the charging operation process; lithium removal with a small current helps to eliminate the influence of polarization factors on the measurement effect.
[0021] In some embodiments, the discharge operation includes: discharging the test battery with a first discharge current to a second voltage; discharging the test battery with a second discharge current to a third voltage; leaving the test battery to rest for a first time; discharging the test battery with a third discharge current to a fourth voltage, wherein the first discharge current>the second discharge current>the third discharge current.
[0022] In the technical solution of the embodiment of the present application, three constant current discharges are adopted, and the discharge current is gradually reduced to increase the full embedding degree of lithium ions in the graphite electrode, thereby improving the accuracy of the total lithium embedding amount obtained; in addition, it can improve the accuracy of the SEI decomposition charge transfer amount obtained subsequently, thereby improving the accuracy of the SEI film formation quality characterization.
[0023] In some embodiments, the characterization method further includes: making a test cell based on the graphite powder to be tested; and screening the graphite powder to be tested according to the film quality characterization value corresponding to the test cell.
[0024] In the technical solution of the embodiment of the present application, a test battery is manufactured based on graphite powder, and the SEI film formation quality is evaluated and the graphite powder is screened, thereby realizing rapid characterization of the SEI film formation quality of the graphite powder, and predicting the battery cycle and storage performance of the finished battery made from the graphite powder. The finished battery is manufactured based on the evaluated and screened graphite powder, which is beneficial to improving the battery cycle and storage performance of the finished battery.
[0025] In some embodiments, the characterization method further includes: allowing the manufactured test battery to stand at room temperature for a predetermined second period of time; and performing a discharge operation on the test battery that has been left standing.
[0026] In the technical solution of the embodiment of the present application, the electrolyte can fully infiltrate the electrodes and the diaphragm, thereby improving the accuracy of the data obtained in subsequent tests, and further improving the accuracy of the characterization of the film quality of the SEI film.
[0027] In some embodiments, the characterization method also includes: obtaining the proportion of graphite powder in graphite slurry during the process of making a test battery; obtaining a first mass of a graphite pole piece, which is generated after coating the graphite slurry on a copper foil current collector; obtaining a second mass of a copper foil current collector of the same size as the graphite pole piece; determining the mass of graphite in the graphite pole piece based on the mass difference between the first mass and the second mass, and the proportion of graphite powder in the graphite slurry; and determining the delithiation current based on the mass of graphite.
[0028] In the technical solution of the embodiment of the present application, the mass of the active material in the graphite electrode of the test battery can be obtained, and the corresponding delithiation current can be determined according to the mass of the active material, thereby improving the matching degree between the delithiation current and the test battery, improving the accuracy of the SEI decomposition impedance after data normalization, and then improving the accuracy of the SEI film quality characterization; in addition, based on the test results, the graphite powder used in the production of the test battery can be screened, which can improve the accuracy of the performance evaluation of the graphite powder and improve the quality of the finished battery.
[0029] In some embodiments, the characterization method further comprises: determining at least one discharge current during the discharge process according to the graphite mass. In the technical solution of the embodiment of the present application, the matching degree between the discharge current used during the discharge process and the test battery can be improved.
[0030] In some embodiments, the test battery includes a button battery. In the technical solution of the embodiment of the present application, a button battery is made as the test battery, and the manufacturing process of the button battery is relatively simple, which is conducive to shortening the time length of graphite powder evaluation and improving the efficiency of graphite powder screening.
[0031] In some embodiments, making a test battery includes: mixing graphite powder with conductive carbon and a binder in a predetermined mass percentage to obtain a graphite slurry; treating the surface of a copper foil current collector with anhydrous ethanol, hydrochloric acid, anhydrous ethanol, and pure water in sequence and performing a drying treatment, and coating the graphite slurry on the surface of the copper foil current collector after the drying treatment; drying and rolling the surface of the copper foil current collector after coating, and cutting it into a pole piece size to obtain a graphite electrode; after drying the graphite electrode, using it as a working electrode, lithium metal as a counter electrode, and using a lithium-ion battery separator to isolate the working electrode and the counter electrode, and obtaining a test battery through assembly.
[0032] In the technical solution of the embodiment of the present application, a simplified production process can be used to complete the production of the test battery, reduce the production cost of the test battery, and shorten the production time of the test battery, which is beneficial to improving the evaluation efficiency of the graphite powder.
[0033] In the second aspect, the present application provides a device for characterizing the quality of SEI film formation, including: an SEI decomposition charge transfer amount determination unit, configured to: determine the amount of lithium desorbed from graphite from the beginning of charging to the end of the delithiation voltage platform based on the voltage data and capacity data of the test battery during the charging process; obtain the SEI decomposition charge transfer amount based on the delithiation amount and the total lithium insertion amount of the test battery; an SEI decomposition impedance determination unit, configured to determine the SEI decomposition impedance based on the voltage data, capacity data and delithiation current; and a film formation quality characterization unit, configured to determine a film formation quality characterization value based on the SEI decomposition charge transfer amount and the SEI decomposition impedance, wherein the film formation quality characterization value is negatively correlated with the SEI decomposition charge transfer amount, and positively correlated with the SEI decomposition impedance.
[0034] In the technical solution of the embodiment of the present application, the charge transferred by SEI film decomposition and the SEI film decomposition impedance can be obtained according to the voltage and capacity data of the battery during the lithium insertion and delithiation process. Based on the fact that the film quality characterization value is negatively correlated with the SEI decomposition charge transferred and positively correlated with the SEI decomposition impedance, the film quality characterization value is obtained to improve the efficiency of SEI film quality assessment.
[0035] In a third aspect, the present application provides a device for characterizing the quality of SEI film formation, comprising: a memory; and a processor coupled to the memory, the processor being configured to execute the data processing portion of any one of the above-mentioned methods for characterizing the quality of SEI film formation based on instructions stored in the memory.
[0036] In the technical solution of the embodiment of the present application, the charge transferred by SEI film decomposition and the SEI film decomposition impedance can be obtained according to the voltage and capacity data of the battery during the lithium insertion and delithiation process. Based on the fact that the film quality characterization value is negatively correlated with the SEI decomposition charge transferred and positively correlated with the SEI decomposition impedance, the film quality characterization value is obtained to improve the efficiency of SEI film quality assessment.
[0037] In a fourth aspect, the present application provides a computer-readable storage medium having computer program instructions stored thereon, which, when executed by a processor, implement the content of the data processing part of any of the above-mentioned methods for characterizing the SEI film quality.
[0038] In the technical solution of the embodiment of the present application, by executing the instructions stored in the storage medium, the charge transferred by SEI film decomposition and the SEI film decomposition impedance can be obtained according to the voltage and capacity data of the battery during the lithium insertion and delithiation process. Based on the fact that the film quality characterization value is negatively correlated with the SEI decomposition charge transferred and positively correlated with the SEI decomposition impedance, the film quality characterization value is obtained to improve the efficiency of SEI film quality assessment.
[0039] In a fifth aspect, the present application provides a computer program product, including a computer program or instructions, which, when executed by a processor, implements the data processing part of any of the above-mentioned methods for characterizing the quality of SEI film formation.
[0040] In the technical solution of the embodiment of the present application, by using the computer program product, the charge transferred by SEI film decomposition and the SEI film decomposition impedance can be obtained according to the voltage and capacity data of the battery during the lithium insertion and delithiation process. Based on the fact that the film quality characterization value is negatively correlated with the SEI decomposition charge transferred and positively correlated with the SEI decomposition impedance, the film quality characterization value is obtained, thereby improving the efficiency of SEI film quality assessment.
[0041] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0043] Figure 1 A flow chart of a method for characterizing the quality of SEI film formation according to one or more embodiments of the present application;
[0044] Figure 2 Schematic diagrams of some embodiments of the first curve in the method for characterizing the SEI film quality of one or more embodiments of the present application;
[0045] Figure 3Schematic diagrams of some embodiments of the second curve in the method for characterizing the SEI film quality of one or more embodiments of the present application;
[0046] Figure 4 A flowchart of a method for characterizing SEI film quality according to another one or more embodiments of the present application;
[0047] Figure 5 A schematic diagram of a test cell in a method for characterizing the quality of SEI film formation according to one or more embodiments of the present application;
[0048] Figure 6 A box plot of SEI film quality of different graphites in the method for characterizing SEI film quality of one or more embodiments of the present application;
[0049] Figure 7 A life data diagram of finished batteries made of different graphites in the method for characterizing the SEI film quality of one or more embodiments of the present application;
[0050] Figure 8 A schematic diagram of a device for characterizing the quality of SEI film formation according to one or more embodiments of the present application;
[0051] Fig. 9 A schematic diagram of a device for characterizing the quality of SEI film formation according to another one or more embodiments of the present application;
[0052] Fig.10 A schematic diagram of a device for characterizing the quality of SEI film formation according to one or more embodiments of the present application. DETAILED DESCRIPTION
[0053] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0054] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0055] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0056] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0057] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0058] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0059] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0060] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0061] The formation of the SEI film consumes some lithium ions, which increases the irreversible capacity of the first charge and discharge and reduces the charge and discharge efficiency of the electrode material. In addition, the SEI film is insoluble in organic solvents and can exist stably in organic electrolyte solutions, and the solvent molecules cannot pass through the passivation film, which can effectively prevent the co-embedding of solvent molecules and avoid the damage to the electrode material caused by the co-embedding of solvent molecules, thereby improving the cycle performance and service life of the electrode. Therefore, the SEI film has an important influence on the performance of the electrode material. The evaluation of the film quality of the SEI film is one aspect of evaluating the performance of the battery. The stability of the SEI film can be characterized by the change of the battery cycle performance during the charge and discharge process by a cycle test. This characterization method requires a long test time and has a high time cost. In addition, the gas production volume and gas production rate during the formation of lithium-ion batteries can be measured, and the gas production volume and gas production rate can be comprehensively analyzed on the pressure bearing capacity design value of the battery structure, as well as the influence of the gas production volume and gas production rate on the battery film formation interface. The film quality can be characterized from the side. The test process of this method is complicated and reduces the efficiency of the film quality characterization.
[0062] Based on the above-mentioned SEI film quality characterization, this application proposes a SEI film quality characterization scheme. Specifically, by obtaining the voltage and capacity data of the battery during the lithium insertion and delithiation process, the charge transferred by the SEI film decomposition and the SEI film decomposition impedance are obtained. Based on the principle that the film quality characterization value is negatively correlated with the SEI decomposition charge transfer amount and positively correlated with the SEI decomposition impedance, the film quality characterization value is calculated.
[0063] The method and device for characterizing the SEI film quality of the present application can obtain the charge transferred by SEI film decomposition and the SEI film decomposition impedance through the electrical performance data obtained during the lithium removal and lithium insertion processes, and then calculate the film quality characterization value, directly characterize the SEI film quality from the perspective of electrical performance, and improve the efficiency of SEI film quality assessment.
[0064] The flowchart of the method for characterizing the SEI film quality of one or more embodiments of the present application is as follows: Figure 1 As shown, it includes steps S14 to S17. The charging process (lithium removal process) and discharging process (lithium insertion process) mentioned in this application refer to the operation in a single charge and discharge cycle. There is no need to perform multiple cycles of charge and discharge operations on the test battery, thereby reducing time cost.
[0065] In step S14, the amount of lithium removed from the graphite from the start of charging to the end of the lithium removal voltage platform is determined based on the voltage data and capacity data of the test battery during the charging process. The voltage data and capacity data of the above charging process are data generated in the same charging operation. During the charging process (lithium removal process), the voltage data and capacity changes of the test battery can be obtained by real-time data statistics.
[0066] In some embodiments, the voltage data and the capacity data are sorted in chronological order, and the change rate dV / dQ of the voltage V change relative to the capacity Q change is calculated. For example, the calculation is performed row by row in the order of charging time: (V t2 -V t1 ) / (Q2-Q1), and obtain the differential voltage data dV / dQ, where the above V t2 is the voltage value at time t2, Q2 is the charging capacity value at time t2; V t1 is the voltage value at time t1, Q1 is the charging capacity value at time t1, where time t1 is the previous moment before time t2 (such as the previous second).
[0067] In some embodiments, a differential voltage curve may be plotted with the charge capacity as the horizontal coordinate and the dV / dQ differential voltage value as the vertical coordinate to obtain a first curve, such as Figure 2 as shown in .
[0068] As the degree of lithium removal increases, the first curve shows phase transition peaks of LiC6, LiC12, LiC18, LiC24, etc., and a differential voltage valley appears after the last phase transition peak (such as Figure 2 The position indicated by the black dot in the middle), and then enters the SEI decomposition and charge transfer stage. The lithium removal capacity corresponding to the differential voltage valley value is recorded as Q plate , which is the amount of electricity released when graphite deviates from the lithium desorption voltage platform from full lithium insertion.
[0069] In the above charging process, the test battery is charged more fully, and the lithium removal voltage range during the charging process exceeds the normal use range of the test battery, so that the differential voltage valley value can be obtained based on the first curve, and the lithium removal amount of the graphite from the beginning of charging to the end of the lithium removal voltage platform is obtained. The normal use range of the above battery refers to the voltage range of the battery under normal operating conditions, such as the rated voltage (or nominal voltage) of the battery. If the lithium removal voltage range exceeds the normal use range of the test battery, that is, the lithium removal voltage is greater than the rated voltage of the test battery.
[0070] In step S15, the SEI decomposition charge transfer amount is obtained based on the lithium removal amount and the total lithium insertion amount of the test battery. plate The total amount of lithium intercalation bound to graphite Q DC , the SEI decomposition charge Q can be calculated SEI :
[0071] Q SEI =Q DC -Q plate (1)
[0072] In the above embodiment, the total lithium insertion amount Q of graphite is DC It can be obtained and recorded by testing the battery's pre-lithiation process. The less the SEI decomposition charge transfer, the better the electrical stability of the SEI layer.
[0073] In step S16, the SEI decomposition impedance is determined based on the voltage data, capacity data and lithium desorption current. The voltage data and capacity data used in this step are collected during the same charging process as the voltage data and capacity data used in the above step S14.
[0074] In some embodiments, the voltage data and the capacity data are sorted in chronological order, and the change rate dV / dQ of the voltage V change relative to the capacity Q change is calculated. For example, the calculation is performed row by row in the order of charging time: (V t2 -V t1 ) / (Q2-Q1), and obtain the differential voltage data dV / dQ, where the above V t2 is the voltage value at time t2, Q2 is the charging capacity value at time t2; V t1 is the voltage value at time t1, Q1 is the charging capacity value at time t1, where time t1 is the previous moment before time t2 (such as the previous second).
[0075] In some embodiments, a differential voltage curve may be plotted with voltage as the horizontal coordinate and dV / dQ differential voltage value as the vertical coordinate to obtain a second curve, such as Figure 3 as shown in .
[0076] The counter electrode of the graphite electrode in the test cell is lithium metal, and the full cell potential is the working electrode (graphite electrode) potential; but when the graphite potential rises to a certain level (≥0.5V), it will enter the SEI electrolysis stage. The highest point of the SEI decomposition peak (such as Figure 3 The peak intensity of the position indicated by the black dot in the middle is S1. The dimension of dV / dQ is as follows: dQ=Idt+tdI. If constant current lithium removal is adopted, tdI=0, so dQ=Idt, and its dimension is V / (A*s)=ohm / s. The higher the peak intensity, the greater the resistance of SEI electrolysis, and the better the film quality. Based on the method in this embodiment, the resistance of SEI electrolysis can be extracted by using the differential voltage curve, so that the film quality characterization value can reflect the resistance of SEI electrolysis, thereby improving the reliability of the film quality characterization value.
[0077] In some embodiments, the SEI decomposition impedance is calculated as follows:
[0078] S SEI =S1 / I (2)
[0079] Wherein, I is the delithiation current of graphite during the delithiation stage.
[0080] Based on the method in this embodiment, the fluctuation in the mass of each electrode is taken into account and the delithiation current is used for normalization, wherein the magnitude of the delithiation current is positively correlated with the active material loading in the electrode (graphite content in the graphite electrode), thereby achieving the normalization of the SEI decomposition impedance and improving the horizontal standard uniformity when testing different test batteries.
[0081] In step S17, a film quality characterization value is determined according to the SEI decomposition charge transfer amount and the SEI decomposition impedance, wherein the film quality characterization value is negatively correlated with the SEI decomposition charge transfer amount and positively correlated with the SEI decomposition impedance.
[0082] For example, the ratio of SEI decomposition impedance to SEI decomposition charge transfer quantity is determined as the film quality characterization value, that is, the film quality characterization value SEI is determined according to formula (3): quality .
[0083] SEI quality =S SEI / Q SEI (3)
[0084] The method for calculating the film quality characterization value in this embodiment has low computational complexity and is easy to implement, which is beneficial to improving the efficiency of determining the film quality characterization value.
[0085] As mentioned above, the less the SEI decomposition charge transfer, the better the electrical stability of the SEI layer; the greater the resistance of SEI electrical decomposition, the better the film quality. Using the relationship between SEI decomposition charge transfer, SEI decomposition impedance and film quality characterization value, the film quality characterization value is determined from the perspective of two electrical properties: SEI decomposition charge transfer and SEI decomposition impedance, which is conducive to improving the reliability and reference value of the film quality characterization value.
[0086] In the technical solution of the embodiment of the present application, the charge transferred by SEI film decomposition and the SEI film decomposition impedance can be obtained according to the voltage and capacity data of the battery during the lithium insertion and delithiation process. Based on the fact that the film quality characterization value is negatively correlated with the SEI decomposition charge transferred and positively correlated with the SEI decomposition impedance, the film quality characterization value is obtained to improve the efficiency of SEI film quality assessment.
[0087] In some embodiments, Figure 4 As shown, before executing step S14, step S13 may also be included: charging the test battery. The delithiation voltage range during the charging process exceeds the normal use range of the test battery, so that the graphite is fully delithiated during the charging operation to reach the SEI film electrolysis stage, and the voltage and capacity data of the SEI film decomposition stage can be obtained, thereby improving the success rate of obtaining the film quality characterization value and the reliability of the data.
[0088] In addition, the maximum value of the delithiation voltage should not be too large, and the value range can be determined according to the short-circuit voltage value of the test battery, such as the maximum value of the normal use voltage of the test battery < delithiation voltage < short-circuit voltage of the test battery, thereby avoiding short circuit of the test battery. Taking the maximum value of the normal use voltage as 0.2-0.3V as an example, the short-circuit voltage is, for example, 3V, and the delithiation voltage can be selected as 2V, so as to avoid short circuit while reaching the SEI membrane electrolysis stage.
[0089] The charging operation can adopt a two-stage charging operation, for example, charging the test battery with a charging current to the normal working voltage of the test battery, and then charging the test battery with a lithium removal current to a first voltage. The charging current is greater than the lithium removal current. After charging the test battery to the normal working voltage with a larger charging current, charging it with a smaller lithium removal current to a first voltage exceeding the normal working voltage shortens the time required to charge to the first voltage and improves the charging efficiency.
[0090] The entire charging operation process can use a constant current, and charge to the first voltage with a lithium removal current, which simplifies the charging operation process; lithium removal with a small current helps to eliminate the influence of polarization factors on the measurement effect.
[0091] In some embodiments, Figure 4 As shown, before executing step S13, step S12 may also be included: discharging the test battery and obtaining the total amount of lithium insertion. The total amount of lithium insertion obtained will be applied to the above step S15. The test battery is formed by the discharge operation to produce an SEI film, and the accuracy of the data collected in the subsequent charging is improved by standing in a stable state; in addition, the amount of electricity fully inserted with lithium in graphite is obtained based on the discharge operation, which is conducive to improving the accuracy of the data used in the subsequent calculation of the amount of charge transferred by the decomposition of the SEI film.
[0092] During the lithium insertion process, a multi-stage discharge can be used, and the discharge current of each stage is less than the current of the previous stage. For example, the test battery is discharged to a second voltage with a first discharge current; the test battery is discharged to a third voltage with a second discharge current; the test battery is left to stand for a first time; the test battery is discharged to a fourth voltage with a third discharge current, wherein the first discharge current> the second discharge current> the third discharge current. The second, third, and fourth voltages are voltage values approaching 0, for example, not greater than 0.005V. Using three constant current discharges and gradually reducing the discharge current can increase the full insertion degree of lithium ions in the graphite electrode, thereby improving the accuracy of the total lithium insertion amount obtained; in addition, it can improve the accuracy of the SEI decomposition charge transfer amount obtained subsequently, thereby improving the accuracy of the SEI film formation quality characterization.
[0093] The method for characterizing the SEI film quality of one or more embodiments of the present application also includes making a test battery based on the graphite powder to be tested, determining the SEI film quality characterization value of the graphite electrode of the test battery, and using the film quality characterization value to evaluate the corresponding graphite powder to screen the graphite powder. The SEI film quality characterization value of the test battery can be used as a basis for predicting the battery cycle and storage performance when the same graphite material is used to make a finished battery in the future.
[0094] Through the method in the above embodiment, the characterization of the quality of the graphite SEI layer is achieved from the powder level, the SEI film quality of the graphite powder can be quickly characterized, and the battery cycle and storage performance of the finished battery made from the graphite powder can be predicted; the finished battery is made based on the evaluated and screened graphite powder, which is beneficial to improving the battery cycle and storage performance of the finished battery.
[0095] The test battery can be a button cell, such as Figure 5 As shown in , the manufacturing process of this type of battery is relatively simple, with low cost and time consumption, which is conducive to reducing costs and improving efficiency.
[0096] In some embodiments, making a test battery includes: mixing graphite powder with conductive carbon and a binder according to a predetermined mass percentage to obtain a graphite slurry; using anhydrous ethanol, hydrochloric acid, anhydrous ethanol, and pure water to treat the surface of the copper foil current collector and perform a drying process in sequence, and coating the graphite slurry on the surface of the copper foil current collector after the drying process; drying and rolling the surface of the copper foil current collector after coating, and cutting it into the size of the pole piece to obtain a graphite electrode; after the graphite electrode is dried, it is used as a working electrode, lithium metal is used as a counter electrode, and a lithium-ion battery separator is used to isolate the working electrode and the counter electrode, and the test battery is obtained by assembly. Based on the method in this embodiment, a simplified manufacturing process can be used to complete the manufacturing of the test battery, reduce the manufacturing cost of the test battery, and shorten the manufacturing time of the test battery, which is conducive to improving the evaluation efficiency of the graphite powder.
[0097] In addition, in the process of making the test battery, the mass of graphite in the graphite pole piece of the test battery is recorded, and the delithiation current in the delithiation process is calculated and configured using the mass of graphite, so as to improve the accuracy of the SEI decomposition impedance after data normalization, thereby improving the accuracy of the SEI film quality characterization. In some embodiments, the proportion of graphite powder in the graphite slurry is obtained in the process of making the test battery; the first mass of the graphite pole piece is obtained, and the graphite pole piece is generated after the graphite slurry is coated on the copper foil current collector; the second mass of the copper foil current collector of the same size as the graphite pole piece is obtained; the mass of graphite in the graphite pole piece is determined according to the mass difference between the first mass and the second mass, and the proportion of graphite powder in the graphite slurry; the delithiation current is determined according to the mass of graphite. Based on the method in this embodiment, the mass of the active material in the graphite pole piece of the test battery can be obtained, and the corresponding delithiation current is determined according to the mass of the active material, thereby improving the matching degree between the delithiation current and the test battery, improving the accuracy of the SEI decomposition impedance after data normalization, and thereby improving the accuracy of the SEI film quality characterization.
[0098] like Figure 4 As shown, before executing step S12, step S11 is included, in which a test cell is made based on graphite powder. For graphite powders from different sources and batches, test cells can be made respectively, and corresponding film quality characterization values can be determined respectively to evaluate the quality of graphite powders from corresponding sources and batches.
[0099] like Figure 4 As shown, after step S17, step S18 may also be included, wherein graphite powders of corresponding sources and batches are screened according to the film quality characterization values to improve the qualified rate of finished batteries. In some embodiments, the film quality characterization values corresponding to graphite powders of different sources and batches may be compared horizontally to select appropriate graphite powders, thereby improving the reliability of raw material selection and facilitating the performance of finished batteries.
[0100] In the following Figure 4 Taking the SEI film quality characterization method of one or more embodiments of the present application as an example, combined with the specific parameters in the feasible embodiments, a method for characterizing the SEI film quality of graphite powder is provided to quickly characterize the SEI film quality of the graphite powder and accurately predict the quality of the cycle / storage performance of the finished battery produced by the graphite powder. The parameters in the embodiments are examples of feasible solutions and do not constitute an improper limitation on the present application.
[0101] In step S11, a test battery is made based on the graphite powder to be tested. The test battery made is a simple battery. Take the manufacture of button batteries as an example. Figure 5As shown in FIG. 5 , the button cell includes a negative electrode shell 501, a working electrode 502, a separator, a counter electrode 504, and a positive electrode shell 505. The preparation of the test cell may include stirring, coating, drying, rolling, slicing, baking, and assembling the cell.
[0102] ① Stirring: Graphite powder, conductive carbon, and binder are mixed in a certain mass percentage. The parameters can be selected as 91.6:1.8:6.6. The specific values can fluctuate within a certain range. N-methylpyrrolidone (NMP) is used as a stirring solvent. After stirring, graphite slurry is obtained. The mass percentage of active substances in the graphite slurry is recorded as S (loading value), and the calculation method is shown in formula (4).
[0103] S=m1 / (m1+m2+m3) (4)
[0104] In this formula, m1 is the weight of graphite powder, m2 is the weight of conductive carbon, and m3 is the weight of binder.
[0105] ② Coating: Cut the copper foil current collector of the target size (thickness 5~20 microns, length and width can be adjusted according to the actual size of the oven), use anhydrous ethanol (remove the oil layer on the surface of the copper foil), dilute hydrochloric acid (concentration ≤0.1M, remove the oxide layer on the surface of the copper foil), anhydrous ethanol (remove the residual dilute hydrochloric acid), and pure water (remove the residual dilute hydrochloric acid and anhydrous ethanol) in turn. After completing the surface treatment, move it to a vacuum drying oven for drying (30~35℃, indoor or too high temperature can easily cause oxidation of the copper foil surface, time ≥2h); use an applicator to evenly spread graphite slurry on the surface of the copper foil current collector, the slurry thickness is 150~250 microns. The above target size can be determined according to the size of the vacuum drying oven and the high temperature oven so that the copper foil current collector can be placed in the subsequent equipment.
[0106] ③ Drying: Transfer the copper foil current collector coated with slurry to a high temperature box with a temperature ≥ 60°C and a time ≥ 1h to dry the excess N-methylpyrrolidone solvent in the electrode.
[0107] ④ Roller pressing: Use a roller press to compact the dried electrode with a roller pressing pressure of 0.2~0.5 tons.
[0108] ⑤ Slicing: Use a punching machine to cut the electrode sheet. The diameter of the cut electrode sheet is 14 mm. Weigh the mass of each electrode sheet and record it as M1. Take the copper foil current collector punched from the same batch and weigh it, record it as M2. Calculate the mass m of the active material (graphite) in the cut electrode sheet according to formula (5):
[0109] m = (M1-M2) × S (5)
[0110] In some embodiments, the mass of each pole piece is recorded separately, and each battery and its test results are calculated after the battery is assembled.
[0111] ⑥Baking: After cutting, place the electrode into a vacuum high temperature oven for drying to remove moisture from the electrode (parameters: temperature, ≥110°C, time, ≥12h, vacuum degree, ≤0.1 atmosphere).
[0112] ⑦ Assembled battery: Graphite pole piece is used as working electrode (diameter 14mm), lithium metal is used as counter electrode (diameter 16 or 18mm), and lithium-ion battery diaphragm (diameter 18 or 20mm) is used to isolate the working electrode and counter electrode; the diameter principle is as follows: diaphragm diameter ≥ counter electrode diameter + 2mm ≥ working electrode + 2mm.
[0113] According to Figure 5 The structure in the figure completes the assembly of a simple button cell. The amount of lithium-ion battery electrolyte used is 150~200 microliters. You can choose to add a spring + gasket or foam nickel or other fillers between the counter electrode and the positive electrode shell.
[0114] Based on the above operations, the test battery is made using the graphite material to be tested. When there are multiple types of graphite materials, test batteries are made respectively, and the active mass m in each graphite pole piece is recorded.
[0115] In steps S12 and S13, the test battery is tested. The test equipment is a device with charging and discharging functions, but is not limited to a charging and discharging machine, an electrochemical workstation, and the like.
[0116] The test process is divided into two stages: lithium removal (discharge) and lithium insertion (charge). The counter electrode is lithium metal, which has a lower electrode potential and serves as the negative electrode; the working electrode is a graphite electrode, which has a higher electrode potential and serves as the positive electrode.
[0117] In the above step S11, after the battery is assembled, it is left to stand at room temperature for ≥12 hours to allow the electrolyte to fully infiltrate the electrodes and the separator.
[0118] In step S12 , a discharge operation (graphite lithium insertion operation) is performed on the test battery and the total lithium insertion amount is obtained.
[0119] In the graphite lithium insertion stage, the following process is adopted:
[0120] 1) Rest 3h
[0121] 2) 0.05C DC 0.005V
[0122] 3) 0.025C DC 0.005V
[0123] 4) Rest 5min
[0124] 5) 0.01mA DC 0.005V
[0125] In the above process, the theoretical gram capacity of graphite is C (generally 340~360mAh / g), and the charge and discharge current of aC is a×C×m, where x is the coefficient and m is the mass of active material in the graphite electrode of the test battery, as shown in the above formula (2). For example, if the mass of active material is 0.009g and the theoretical gram capacity is 340mAh / g, the current at a rate of 0.1C is 0.306mA.
[0126] The current in step 2 is 0.05×C×m, and the current in step 3 is 0.025×C×m. Taking a button cell as an example, in step 2, the current is about 0.1mA, and in step 3, the current is about 0.05~0.1mA.
[0127] The voltage of 0.005 V in the above steps 2, 3, and 4 is a relatively small voltage close to 0, which can be set between 0 and 0.005 V to fully embed lithium into the graphite.
[0128] In step S13, a charging operation (graphite delithiation operation) is performed on the test battery, wherein the delithiation voltage range during the charging process exceeds the normal use range of the test battery.
[0129] In the graphite delithiation stage, the following process is adopted:
[0130] 1) Rest 10 minutes
[0131] 2) 0.1C CC 2.0V
[0132] As mentioned above, the delithiation current in step 2 of this process is 0.1C, that is, 0.1×C×m. In some embodiments, a smaller current, such as 0.05C or less, can be used to delithiate to 2.0V to obtain a better delithiation effect. In some embodiments, 0.1C can be set as the upper limit of the constant current delithiation current to achieve a balance between the delithiation time and effect.
[0133] Taking button cells as an example, the conventional delithiation process is to delithiate to a voltage of 0.2-0.3V. Considering that short circuits are likely to occur above 3V, delithiation is selected to be between 2.0-3.0V.
[0134] In some embodiments, the lithium removal value may be firstly reduced to 0.26V at a constant current of 0.1C, and then reduced to 2.0V at a smaller constant current (eg, between 0.1C and 0.05C) to shorten the duration of the lithium removal process.
[0135] In steps S14 to S17, the film quality characterization value is calculated using the method in the above embodiment, which will not be repeated here.
[0136] In step S18, the graphite powder is selected according to the SEI film quality characterization value of the test battery. quality The higher the value, the better the quality of SEI film formation. The corresponding finished battery has a lower degree of SEI damage during the cycle and storage process, and the irreversible active lithium consumption caused by the graphite electrode (irreversible lithium consumption caused by the repair process due to the destruction of SEI), and the better its cycle storage life.
[0137] The box plot of the film quality characterization value obtained by measuring eight groups of graphite powders in this scheme is as follows: Figure 6 shown. Figure 6 In the graph, the horizontal axis is eight kinds of graphite powders, and the vertical axis is the film quality characterization value. Graphite H>Graphite G>Graphite C>Graphite F≈Graphite A≈Graphite D≈Graphite E>Graphite B.
[0138] After using these eight groups of graphite powder to make finished batteries, the life data of the batteries were tested at 45°C according to the following process, and the following were obtained: Figure 7 Battery performance shown.
[0139] 1) Rest 10 minutes
[0140] 2) 1C CC 3.65V
[0141] 3) Rest 10 minutes
[0142] 4) 1C CC 2.0V
[0143] 5) Repeat steps 1 to 4 until the value decays to 60%
[0144] Figure 7 The horizontal axis in the middle is the number of cycles, and the vertical axis is the performance retention ratio. The upper right corner of the figure is the legend area. Different line types correspond to finished batteries made with graphite AH as raw materials. The legend area shows the corresponding relationship between the legend and the graphite raw materials of the finished battery. Figure 7 The figure shows the change of the performance retention ratio of the finished battery made of graphite AH with the number of cycles. It can be seen that the relationship between the life of the finished battery is similar to the relationship between the film quality characterization value, that is, graphite H>graphite G>graphite C>graphite F≈graphite A≈graphite D≈graphite E>graphite B.
[0145] From the above comparison, it can be seen that the method for characterizing the quality of SEI film formation provided in this application can effectively predict the life of the battery after the finished battery is made of graphite powder with high accuracy; the quality of the graphite SEI layer is characterized from the powder level, and the battery cycle and storage performance of the finished battery made of graphite powder are predicted. The finished battery is made based on the evaluated and screened graphite powder, which is beneficial to improve the battery cycle and storage performance of the finished battery.
[0146] A schematic diagram of a device for characterizing the SEI film quality according to one or more embodiments of the present application is shown in FIG. Figure 8 The device for characterizing the SEI film quality can perform data processing based on the voltage, capacity and other data obtained during the battery test to obtain a film quality characterization value.
[0147] The SEI decomposition charge transfer amount determination unit 81 can determine the amount of lithium removed from the graphite from the start of charging to the end of the lithium removal voltage platform according to the voltage data and capacity data of the test battery during the charging process, and then obtain the SEI decomposition charge transfer amount according to the lithium removal amount and the total lithium insertion amount of the test battery. In some embodiments, the SEI decomposition charge transfer amount determination unit 81 can execute the method in any of the above steps S14 and S15.
[0148] The SEI decomposition impedance determination unit 82 can determine the SEI decomposition impedance according to the voltage data, the capacity data and the delithiation current. In some embodiments, the SEI decomposition impedance determination unit 82 can execute the method in any of the embodiments of step S16 above.
[0149] The film quality characterization unit 83 can determine the film quality characterization value according to the SEI decomposition charge transfer amount and the SEI decomposition impedance, wherein the film quality characterization value is negatively correlated with the SEI decomposition charge transfer amount and positively correlated with the SEI decomposition impedance. In some embodiments, the SEI decomposition impedance determination unit 83 can execute the method in any embodiment of step S17 above.
[0150] In the technical solution of the embodiment of the present application, the charge transferred by SEI film decomposition and the SEI film decomposition impedance can be obtained according to the voltage and capacity data of the battery during the lithium insertion and delithiation process. Based on the fact that the film quality characterization value is negatively correlated with the SEI decomposition charge transferred and positively correlated with the SEI decomposition impedance, the film quality characterization value is obtained to improve the efficiency of SEI film quality assessment.
[0151] The structural schematic diagram of an embodiment of the device for characterizing the SEI film quality of the present application is as follows: Fig. 9As shown. The device for characterizing the quality of SEI film formation includes a memory 901 and a processor 902. Wherein: the memory 901 can be a disk, a flash memory or any other non-volatile storage medium. The memory is used to store the instructions in the corresponding embodiment of the method for characterizing the quality of SEI film formation described above. The processor 902 is coupled to the memory 901 and can be implemented as one or more integrated circuits, such as a microprocessor or a microcontroller. The processor 902 is used to execute the instructions stored in the memory, which can improve the efficiency of SEI film formation quality assessment.
[0152] In one embodiment, it is also possible to Fig.10 As shown, the SEI film quality characterization device 1000 includes a memory 901 and a processor 902. The processor 902 is coupled to the memory 901 via a BUS bus 1003. The SEI film quality characterization device 1000 can also be connected to an external storage device 1005 via a storage interface 1004 to call external data, and can also be connected to a network or another computer system (not shown) via a network interface 1006. No detailed description will be given here.
[0153] In this embodiment, the efficiency of SEI film quality assessment can be improved by storing data instructions in a memory and processing the instructions through a processor.
[0154] In another embodiment, a computer-readable storage medium stores computer program instructions, which, when executed by a processor, implement the steps of the method in the corresponding embodiment of the method for characterizing the quality of SEI film formation. It should be understood by those skilled in the art that the embodiments of the present disclosure may be provided as methods, devices, or computer program products. Therefore, the present disclosure may take the form of a complete hardware embodiment, a complete software embodiment, or an embodiment combining software and hardware. Moreover, the present disclosure may take the form of a computer program product implemented on one or more computer-usable non-transient storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.
[0155] The above description of various embodiments tends to emphasize the differences between the various embodiments. The same or similar aspects can be referenced to each other, and for the sake of brevity, they will not be repeated herein.
[0156] The present disclosure is described with reference to flowcharts and / or block diagrams of methods, devices (systems) and computer program products according to embodiments of the present disclosure. It should be understood that each process and / or block in the flowchart and / or block diagram and the combination of processes and / or blocks in the flowchart and / or block diagram can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, a special-purpose computer, an embedded processor or other programmable data processing device to produce a machine, so that the instructions executed by the processor of the computer or other programmable data processing device generate instructions for implementing the processes in the flowchart and / or block diagram. Figure 1 A process or multiple processes and / or boxes Figure 1 A device that provides the functions specified in a block or multiple blocks.
[0157] These computer program instructions may also be stored in a computer-readable memory capable of directing a computer or other programmable data processing device to operate in a specific manner, so that the instructions stored in the computer-readable memory produce an article of manufacture comprising an instruction device, which implements the process Figure 1 A process or multiple processes and / or boxes Figure 1 A function specified in one or more boxes.
[0158] These computer program instructions can also be loaded onto a computer or other programmable data processing device so that a series of operating steps are executed on the computer or other programmable device to produce a computer-implemented process, thereby providing instructions for implementing the process. Figure 1 A process or multiple processes and / or boxes Figure 1 The steps for the functions specified in one or more boxes.
[0159] So far, the present disclosure has been described in detail. In order to avoid obscuring the concept of the present disclosure, some details known in the art are not described. Based on the above description, those skilled in the art can fully understand how to implement the technical solution disclosed here.
[0160] The method and apparatus of the present disclosure may be implemented in many ways. For example, the method and apparatus of the present disclosure may be implemented by software, hardware, firmware, or any combination of software, hardware, and firmware. The above order of steps for the method is for illustration only, and the steps of the method of the present disclosure are not limited to the order specifically described above, unless otherwise specifically stated. In addition, in some embodiments, the present disclosure may also be implemented as a program recorded in a recording medium, which includes machine-readable instructions for implementing the method according to the present disclosure. Therefore, the present disclosure also covers a recording medium storing a program for executing the method according to the present disclosure.
[0161] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A method for characterizing the quality of SEI film formation at a solid electrolyte interface, comprising: According to the voltage data and capacity data of the test battery during the charging process, the amount of lithium removed from the graphite from the start of charging to the end of the lithium removal voltage platform is determined; Obtaining the SEI decomposition charge transfer amount according to the lithium removal amount and the total lithium insertion amount of the test battery; Determining the SEI decomposition impedance according to the voltage data, the capacity data and the lithium desorption current, including: obtaining the rate of change of voltage change relative to the capacity change; obtaining a second curve of the rate of change as a inverse of voltage according to the rate of change and the voltage data; determining the peak value of the rate of change when the voltage in the second curve is greater than a threshold value; obtaining a ratio of the peak value to the lithium desorption current as the SEI decomposition impedance; A film quality characterization value is determined according to the SEI decomposition charge transfer amount and the SEI decomposition impedance, wherein the film quality characterization value is negatively correlated with the SEI decomposition charge transfer amount and positively correlated with the SEI decomposition impedance.
2. The characterization method according to claim 1, wherein: Determining the amount of lithium removed from the graphite from the start of charging to the end of the lithium removal voltage platform according to the voltage data and capacity data of the test battery during the charging process includes: Get the rate of change of voltage change relative to capacity change; According to the change rate and the capacity data, obtaining a first curve of the change rate versus capacity; The capacity corresponding to the valley value of the change rate in the first curve is determined as the delithiation amount.
3. The characterization method according to claim 1 or 2, wherein: Determining the film quality characterization value according to the SEI decomposition charge transfer amount and the SEI decomposition impedance includes: The ratio of the SEI decomposition impedance to the SEI decomposition charge transfer amount is determined as the film quality characterization value.
4. The characterization method according to claim 1, further comprising: A charging operation is performed on the test battery, wherein a delithiation voltage range during the charging process exceeds a normal use range of the test battery.
5. The characterization method according to claim 4, further comprising: Before performing the charging operation, a discharging operation is performed on the test battery and the total lithium insertion amount is obtained.
6. The characterization method according to claim 4, wherein: The charging operation includes: The test battery is charged to a first voltage with the delithiation current, wherein the first voltage is greater than a normal operating voltage of the test battery.
7. The characterization method according to claim 4, wherein: The charging operation includes: Charging the test battery with a charging current to a normal operating voltage of the test battery; The test battery is charged to a first voltage with the delithiation current, wherein the charging current is greater than the delithiation current, and the first voltage is greater than a normal operating voltage of the test battery.
8. The characterization method according to claim 5, wherein: The discharging operation includes: discharging the test battery to a second voltage at a first discharge current; discharging the test battery to a third voltage at a second discharge current; allowing the test battery to rest for a first period of time; discharging the test battery at a third discharge current to a fourth voltage, Among them, the first discharge current>the second discharge current>the third discharge current.
9. The characterization method according to claim 1, further comprising: Based on the graphite powder to be tested, manufacturing the test battery; The graphite powder to be tested is screened according to the film quality characterization value corresponding to the test battery.
10. The characterization method according to claim 9, further comprising: Allowing the manufactured test battery to stand at room temperature for a predetermined second period of time; A discharge operation is performed on the test battery after the standing still.
11. The characterization method according to claim 9, further comprising: Obtaining the proportion of the graphite powder in the graphite slurry during the process of manufacturing the test battery; Obtaining a first mass of a graphite pole piece, the graphite pole piece being produced after coating the graphite slurry on a copper foil current collector; Obtaining a second mass of the copper foil current collector having the same size as the graphite pole piece; Determining the mass of graphite in the graphite pole piece according to the mass difference between the first mass and the second mass, and the proportion of the graphite powder in the graphite slurry; The delithiation current is determined according to the graphite mass.
12. The characterization method according to claim 11, further comprising: At least one discharge current in the discharge process is determined according to the graphite mass.
13. The characterization method according to claim 1, wherein: The test battery includes a button cell.
14. The characterization method according to claim 9 or 13, wherein: Making the test battery includes: Mixing graphite powder, conductive carbon and a binder according to a predetermined mass percentage to obtain graphite slurry; sequentially treating the surface of the copper foil current collector with anhydrous ethanol, hydrochloric acid, anhydrous ethanol, and pure water and performing a drying process, and coating the graphite slurry on the surface of the copper foil current collector after the drying process; Drying and rolling the surface of the copper foil current collector after coating, and cutting it into the size of a pole piece to obtain a graphite electrode; After the graphite electrode is dried, it is used as a working electrode, lithium metal is used as a counter electrode, and a lithium-ion battery separator is used to isolate the working electrode and the counter electrode, and the test battery is obtained by assembly.
15. A device for characterizing the quality of SEI film formation at a solid electrolyte interface, comprising: The SEI decomposition charge transfer amount determination unit is configured to: determine the amount of lithium removed from the graphite from the start of charging to the end of the lithium removal voltage platform according to the voltage data and capacity data of the test battery during the charging process; and obtain the SEI decomposition charge transfer amount according to the lithium removal amount and the total lithium insertion amount of the test battery; The SEI decomposition impedance determination unit is configured to determine the SEI decomposition impedance according to the voltage data, the capacity data and the lithium desorption current, including: obtaining a change rate of voltage change relative to capacity change; obtaining a second curve of the change rate as a inverse of voltage according to the change rate and the voltage data; determining a peak value of the change rate when the voltage in the second curve is greater than a threshold value; obtaining a ratio of the peak value to the lithium desorption current as the SEI decomposition impedance; The film quality characterization unit is configured to determine a film quality characterization value according to the SEI decomposition charge transfer amount and the SEI decomposition impedance, wherein the film quality characterization value is negatively correlated with the SEI decomposition charge transfer amount and positively correlated with the SEI decomposition impedance.
16. A device for characterizing the quality of SEI film formation at a solid electrolyte interface, comprising: Memory; as well as A processor coupled to the memory, the processor being configured to execute the method according to any one of claims 1 to 3 based on instructions stored in the memory.
17. A computer-readable storage medium having computer program instructions stored thereon, wherein the instructions, when executed by a processor, implement the method according to any one of claims 1 to 3.
18. A computer program product, comprising a computer program or instructions, wherein when the computer program or instructions are executed by a processor, the method according to any one of claims 1 to 3 is implemented.
Citation Information
Patent Citations
Impedance monitoring method representing film-forming process of SEI film
CN109461980A
Lithium separation detection method and device for lithium battery
CN112703125A
Hard carbon negative electrode material, negative electrode plate and battery
CN115911368A
Battery lithium precipitation detection method and device and storage medium
CN116754971A
Method for determining SEI film performance of lithium ion battery
CN116773601A
Cited By
Control method for lithium-ion battery formation and lithium-ion battery formation system