A method for repairing blind grooves on the surface of a workpiece

By embedding a filler plate of the same material in the blind groove and performing plasma spraying, the problem of repairing blind grooves with large depths was solved, the surface of the workpiece was restored and the shape was controlled, and the repair effect and bonding strength were improved.

CN118253931BActive Publication Date: 2026-11-10GUIZHOU LIYANG INT MFG
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410435033.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-11
Publication Date
2026-11-10
Estimated Expiration
2044-04-11

AI Technical Summary

Technical Problem

Existing technologies are difficult to effectively repair blind groove defects with large depths on the surface of parts, and it is difficult to control the shape and size of the workpiece during the repair process, which affects the repair effect and bonding strength.

Method used

By embedding a filler plate of the same material as the workpiece in the blind groove, and forming a filler coating in the blind groove using plasma spraying, combined with cutting and sandblasting, the coating is made flush with the workpiece surface and has a strong bond.

Benefits of technology

It enhances the load-bearing capacity of the blind groove location, restores the original appearance of the workpiece surface, extends the service life, avoids resource waste, and improves the repair effect and bonding strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118253931B_ABST
    Figure CN118253931B_ABST
Patent Text Reader

Abstract

This invention provides a method for repairing blind grooves on the surface of a workpiece, comprising the following steps: cleaning the workpiece and the blind groove; performing sandblasting treatment on the blind groove; measuring the diameter of the blind groove; machining the blind groove to expand it into a rectangle; preparing a filler plate and bonding it into the blind groove; plasma spraying a filler coating into the blind groove; machining the filler coating to make it flush with the surface of the workpiece. By embedding a filler plate of the same material as the workpiece into the blind groove, the defective area of ​​the workpiece is reconnected into a whole through the filler plate, enhancing the load-bearing capacity of that location. This effectively compensates for the blind groove defects on the workpiece surface. Furthermore, plasma spraying covers the damaged groove defects on the workpiece surface, restoring the workpiece surface to its original appearance. Strict control of the shape and size of the workpiece during the repair process restores its performance, extends its service life, and avoids resource waste caused by workpiece scrapping.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of maintenance technology, and in particular relates to a method for repairing blind grooves on the surface of a workpiece. Background Technology

[0002] With the development of mechanical manufacturing technology, people have used various manufacturing methods to produce a large number of mechanical parts. These products vary in performance, shape and material. If the products are bumped or damaged during production and use, pits or grooves will be generated on the product surface, affecting the normal use of the flattening. If the product is scrapped, it will result in a large waste of resources because the damaged part is small. Therefore, when some parts have local defects, technical measures can be taken to repair them so that the products can maintain normal performance as much as possible and extend their service life.

[0003] In the prior art, patent document with publication number "CN101403086" discloses a method for repairing a lubricating pump housing bushing using plasma spraying of a Cu-Al coating. This method repairs the narrow arc-shaped boss end face of the lubricating pump housing bushing using plasma spraying. The steps include cleaning, sandblasting, protection, and spraying the coating material onto the narrow arc-shaped boss end face of the lubricating pump housing bushing using plasma spraying equipment. Using this patented technology, the coating adhesion strength reaches 41.07 MPa, indicating relatively stable hardness and good coating adhesion performance, which helps reduce material waste. However, this repair method is generally only suitable for minor surface defects. When the surface damage groove is deep, the adhesion strength between the plasma coating and the substrate is limited, and controlling the shape and dimensions of the workpiece during the repair process is difficult, affecting the repair and restoration effect. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a method for repairing blind grooves on the surface of a workpiece.

[0005] The present invention is achieved through the following technical solutions.

[0006] This invention provides a method for repairing blind grooves on the surface of a workpiece, comprising the following steps:

[0007] Step 1: Provide a workpiece with blind grooves on its surface, and clean the workpiece and the blind grooves;

[0008] Step 2: Sandblasting treatment of the blind channel;

[0009] Step 3: Measure the length a, width b, and depth δ of the blind groove. If δ ≤ 3mm, proceed to Step 6; if δ > 3mm, proceed to Step 4.

[0010] Step 4: Perform cutting machining on the blind groove on the workpiece surface to expand the shape of the blind groove into a rectangle, and expand the shape and size of the blind groove to: length × width × depth = (a + Δp) × (b + Δp) × (δ + Δp);

[0011] Step 5: Prepare the landfill plate, the external dimensions of which are: length × width × thickness = (a + Δp) × (b + Δp) × h, and then bond the landfill plate to the blind groove;

[0012] Step 6: Using hydrogen as fuel, oxygen as combustion-supporting gas, and argon as powder carrier gas, plasma spraying is performed on the blind groove, so that the sprayed powder is sprayed out from the spray gun and a filling coating with a thickness of s is obtained in the blind groove.

[0013] Step 7: Perform cutting processing on the embedded coating so that the surface of the embedded coating is flush with the surface of the workpiece.

[0014] In steps three through six, if δ ≤ 3 mm, then s - δ ≥ 1 mm; if δ > 3 mm, then s + h - δ - Δp ≥ 1 mm; 1 mm ≤ Δp ≤ 2 mm; 1 mm ≤ h ≤ 3 mm.

[0015] The cleaning of the workpiece and blind groove mentioned in step one refers to cleaning the workpiece and blind groove with acetone or anhydrous ethanol.

[0016] The repair method for the blind groove on the workpiece surface also includes the following steps: before performing step two, high-temperature resistant tape is used to adhere to the surface of the workpiece as a protection.

[0017] The process parameters for sandblasting treatment of the blind groove in step two are as follows: white corundum sand with a fine particle size of 36# to 180# is used as the sandblasting raw material, the sandblasting pressure is 0.1MPa to 0.3MPa, the impact angle of the sandblasting relative to the surface of the blind groove is 35° to 65°, and the distance between the sandblasting outlet and the surface of the blind groove is 140mm to 150mm.

[0018] In step five, bonding the landfill plate to the blind groove means using AB glue to bond the landfill plate to the bottom surface of the blind groove as a whole.

[0019] In step six, the process parameters for plasma spraying the blind groove are as follows: gas flow rate is 10L / min, powder carrier gas flow rate is 55L / min, the angle between the spray gun outlet and the bottom surface of the blind groove is 35° to 90°, the distance between the spray gun outlet and the bottom surface of the blind groove is 160mm, the spray gun moving speed is less than 8mm / s, and the temperature of the sprayed powder is less than 200℃.

[0020] In step seven, machining the landfill coating means using a milling machine to mill the landfill coating or using a lathe to turn the landfill coating.

[0021] The workpiece, the filler plate, and the spray powder are all made of the same material.

[0022] The workpiece is made of aluminum.

[0023] The beneficial effects of this invention are as follows: By embedding a filler plate of the same material as the workpiece into the blind groove, the defective part of the workpiece is reconnected into a whole through the filler plate, which enhances the load-bearing capacity of the location and can effectively compensate for the blind groove defect on the surface of the workpiece. Furthermore, the damaged groove defect on the surface of the workpiece is covered by plasma spraying, so that the surface of the workpiece is restored to its original appearance. In addition, the shape and size of the workpiece are strictly controlled during the repair process, restoring the performance of the workpiece, extending the service life of the workpiece, avoiding the waste of resources caused by the scrapping of the workpiece, and laying the foundation for improving the economic benefits of the enterprise. Attached Figure Description

[0024] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation

[0025] The technical solution of the present invention is further described below, but the scope of protection is not limited to what is described.

[0026] like Figure 1 As shown, the present invention provides a method for repairing blind grooves on the surface of a workpiece, comprising the following steps:

[0027] Step 1: Provide a workpiece with blind grooves on its surface; clean the workpiece and the blind grooves.

[0028] Step 2: Sandblasting treatment of the blind channel;

[0029] Step 3: Measure the length a, width b, and depth δ of the blind groove. If δ ≤ 3mm, proceed to Step 6; if δ > 3mm, proceed to Step 4.

[0030] Step 4: Perform cutting machining on the blind groove on the workpiece surface to expand the shape of the blind groove into a rectangle, and expand the shape and size of the blind groove to: length × width × depth = (a + Δp) × (b + Δp) × (δ + Δp);

[0031] Step 5: Prepare the landfill plate. The external dimensions of the landfill plate are: length × width × thickness = (a + Δp) × (b + Δp) × h, and then bond the landfill plate to the blind trench.

[0032] Step 6: Using hydrogen as fuel, oxygen as combustion-supporting gas, and argon as powder carrier gas, plasma spraying is performed on the blind groove, so that the sprayed powder is sprayed out from the spray gun and a filling coating with a thickness of s is obtained in the blind groove.

[0033] Step 7: Machining the embedded coating to make its surface flush with the workpiece surface.

[0034] By employing the technical solution of this invention, a filler plate of the same material as the workpiece is embedded into the blind groove. The filler plate reconnects the defective parts of the workpiece into a whole, enhancing the load-bearing capacity of that location. This effectively compensates for the blind groove defects on the workpiece surface. Furthermore, plasma spraying is used to cover the damaged groove defects on the workpiece surface, restoring the workpiece surface to its original appearance. During the repair process, the shape and size of the workpiece are strictly controlled, restoring its performance and extending its service life. This avoids resource waste caused by workpiece scrapping and lays the foundation for improving the economic benefits of enterprises.

[0035] Specifically, in steps three to six, if δ≤3mm, then s-δ≥1mm; if δ>3mm, then s+h-δ-Δp≥1mm; 1mm≤Δp≤2mm; 1mm≤h≤3mm. Using the technical solution of this invention, the blind groove is expanded to a regular shape and size by cutting before plasma spraying. The sandblasting treatment of the blind groove in step two typically only reduces its shape and size by 150 micrometers, and its impact on subsequent processes is negligible. On the one hand, this facilitates control of the plasma spray coating thickness, resulting in a uniform and dense plasma spray coating; on the other hand, it increases the bonding area between the filling coating and the groove surface, which is beneficial for improving the bonding strength of the filling coating and also helps restore the original appearance of the workpiece surface.

[0036] In addition, cleaning the workpiece and blind groove in step one refers to cleaning the workpiece and blind groove with acetone or anhydrous ethanol. This avoids the negative impact of foreign matter or impurities on the spraying process or the bonding process between the paint and the workpiece, and improves the bonding strength between the paint and the workpiece.

[0037] In addition, the repair method for blind grooves on the workpiece surface also includes the following steps: Before step two, high-temperature resistant tape is applied to the surface of the workpiece as a protective measure. The process parameters for sandblasting treatment of the blind groove in step two are as follows: white corundum alumina particles with a fine particle size of 36# to 180# are used as the sandblasting raw material, the sandblasting pressure is 0.1MPa to 0.3MPa, the impact angle of the sandblasting relative to the surface of the blind groove is 35° to 65°, and the distance between the sandblasting outlet and the surface of the blind groove is 140mm to 150mm.

[0038] Specifically, in step five, bonding the landfill plate to the blind trench means using AB glue to bond the landfill plate to the bottom surface of the blind trench as a single unit. In step six, the process parameters for plasma spraying the blind trench are as follows: gas flow rate is 10L / min, powder carrier gas flow rate is 55L / min, the angle between the spray gun outlet and the bottom surface of the blind trench is 35° to 90°, the distance between the spray gun outlet and the bottom surface of the blind trench is 160mm, the spray gun moving speed is less than 8mm / s, and the temperature of the sprayed powder is less than 200℃.

[0039] Furthermore, in step seven, machining the landfill coating refers to milling the landfill coating using a milling machine or turning it using a lathe. The workpiece, landfill plate, and sprayed powder are all made of the same material. The workpiece is made of aluminum.

Claims

1. A method for repairing blind grooves on the surface of a workpiece, characterized in that: Includes the following steps: Step 1: Provide a workpiece with blind grooves on its surface, and clean the workpiece and the blind grooves; Step 2: Sandblasting treatment of the blind channel; Step 3: Measure the length of the blind groove. Width dimension is The depth dimension is , and if Then proceed to step six, if Then proceed to step four; Step 4: Machin the blind groove on the workpiece surface to expand its shape into a rectangle, and expand its dimensions to: length × width × depth = ; Step 5: Prepare the landfill plate, the external dimensions of which are: length × width × thickness = The landfill plate is then bonded to the blind groove. Step Six: Using hydrogen as the fuel gas, oxygen as the combustion-supporting gas, and argon as the powder carrier gas, plasma spraying is performed on the blind groove, causing the sprayed powder to be ejected from the spray gun and achieving a thickness of [thickness value missing] within the blind groove. Landfill coating; Step 7: Machining the filling coating to make the surface of the filling coating flush with the surface of the workpiece; In steps three through six, if ,but ,like ,but , , ; The workpiece and blind groove are cleaned with acetone or anhydrous ethanol. Before proceeding to step two, high-temperature resistant tape is used to adhere to the surface of the workpiece as a protective measure. In step five, bonding the landfill plate to the blind trench means using AB glue to bond the landfill plate to the bottom surface of the blind trench as a whole. The workpiece, the filler plate, and the spray powder are all made of the same material.

2. The method for repairing blind grooves on the surface of a workpiece as described in claim 1, characterized in that: The process parameters for sandblasting treatment of the blind groove in step two are as follows: white corundum sand with a fine particle size of 36# to 180# is used as the sandblasting raw material, the sandblasting pressure is 0.1MPa to 0.3MPa, the impact angle of the sandblasting relative to the surface of the blind groove is 35° to 65°, and the distance between the sandblasting outlet and the surface of the blind groove is 140mm to 150mm.

3. The method for repairing blind grooves on the surface of a workpiece as described in claim 1, characterized in that: In step six, the process parameters for plasma spraying the blind groove are as follows: gas flow rate is 10L / min, powder carrier gas flow rate is 55L / min, the angle between the spray gun outlet and the bottom surface of the blind groove is 35° to 90°, the distance between the spray gun outlet and the bottom surface of the blind groove is 160mm, the spray gun moving speed is less than 8mm / s, and the temperature of the sprayed powder is less than 200℃.

4. The method for repairing blind grooves on the surface of a workpiece as described in claim 1, characterized in that: In step seven, machining the landfill coating means using a milling machine to mill the landfill coating or using a lathe to turn the landfill coating.

5. The method for repairing blind grooves on the surface of a workpiece as described in claim 1, characterized in that: The workpiece is made of aluminum.

Citation Information

Patent Citations

  • Method for repairing defect on surface of workpiece

    CN104625391A

  • Method for repairing dimension of GH4169 part through plasma spraying of NiCrFeMo coating

    CN105420661A