A silicone rubber protective coating, its preparation method and application
By adding straw cellulose aerogel powder to the silicone rubber coating, a silicone rubber protective coating with better hydrophobic properties was prepared, which solved the problem of insufficient hydrophobic properties of silicone rubber in the prior art and achieved better waterproof and wear-resistant effects.
Patent Information
- Application Number
- CN202410357486.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-27
AI Technical Summary
The hydrophobic properties of existing silicone rubber need further improvement, especially in areas requiring self-cleaning and waterproofing properties.
Straw cellulose aerogel powder is added to a silicone rubber coating. The aerogel powder is prepared by a specific treatment method and then mixed with other raw materials to form a silicone rubber protective coating.
It significantly improves the hydrophobicity of the silicone rubber coating and enhances its abrasion resistance and adhesion.
Smart Images

Figure BDA0004761825820000071
Abstract
Description
Technical Field
[0001] This invention relates to the field of silicone rubber coating technology, and in particular to a silicone rubber protective coating, its preparation method, and its application. Background Technology
[0002] Silicone rubber protective coatings are widely used for corrosion protection, waterproofing, and heat insulation of base surfaces, and therefore have a wide range of applications in daily life, especially in the construction, automotive, and medical device industries.
[0003] Superhydrophobic silicone rubber offers several advantages, including better self-cleaning, waterproofing, and stain resistance. This type of superhydrophobic silicone rubber coating holds significant promise for applications on surfaces that are difficult to clean and require routine waterproofing and thermal insulation. However, further improvements are needed to enhance the hydrophobic properties of silicone rubber. Summary of the Invention
[0004] In view of this, the present invention proposes a protective coating for silicone rubber, its preparation method and application, aiming to improve the hydrophobic properties of silicone rubber by improving the raw materials and preparation process of silicone rubber.
[0005] The technical solution of the present invention is implemented as follows: The present invention provides a silicone rubber protective coating, the raw materials of which, by weight, include: 90-100 parts of silicone rubber base, 1-5 parts of aerogel powder, 5-10 parts of filler, 0.01-0.03 parts of catalyst, 5-10 parts of crosslinking agent and 0.001 parts of inhibitor, wherein the aerogel powder is straw cellulose aerogel powder.
[0006] In some embodiments, the preparation method of aerogel powder includes: degreasing straw fragments, then heating and soaking the degreased straw in hydrogen peroxide solution, then soaking it in acetic acid solution, then soaking it in alkaline solution, rinsing it with water to the center to obtain straw cellulose, making the obtained straw cellulose into a hydrochloric acid suspension, aging the solution for a period of time, filtering it to obtain hydrogel, freeze-drying the hydrogel and pulverizing it to obtain aerogel powder.
[0007] In some embodiments, the detailed preparation method of aerogel powder is as follows: straw fragments are immersed in ethanol, heated to 75°C, and refluxed at a constant temperature for 4 hours. After filtration and drying, the dried straw fragments are soaked in 8% hydrogen peroxide solution and heated to 50°C, kept at this temperature and stirred for 6 hours. Then, they are rinsed with deionized water. Next, the straw fragments are soaked in acetic acid solution with a pH of 4, heated to 70°C, and kept at this temperature for 3 hours. Then, they are soaked in sodium hydroxide solution with a pH of 12 for 10 hours. After rinsing with deionized water until neutral, straw cellulose is obtained. A 1% (w / w) straw cellulose suspension is prepared by adding water, and hydrochloric acid is added to adjust the pH to 4. The suspension is then stirred for 3 hours, filtered, and a hydrogel is obtained. The hydrogel is freeze-dried to obtain an aerogel, which is then pulverized to obtain aerogel powder.
[0008] In some embodiments, the steps for preparing aerogel powder described above, after preparing a hydrochloric acid suspension of straw cellulose, further include adding a silane coupling agent to the suspension and then performing an aging treatment.
[0009] In some embodiments, the silane coupling agent added to the suspension is n-octyltriethoxysilane.
[0010] In some embodiments, the average particle size of the aerogel powder is 200-500 nm.
[0011] In some embodiments, the silicone rubber base is phenylene ether silicone rubber, and the annual strength of the silicone rubber base is 5000-8000 mPa·s.
[0012] In some implementations, the filler is silica.
[0013] In some implementations, the catalyst is a platinum catalyst.
[0014] In some embodiments, the crosslinking agent is methylphenyl hydrogen-containing silicone oil.
[0015] In some implementations, the inhibitor is 1-butynylcyclohexanol.
[0016] Secondly, the present invention also provides a method for preparing the above-mentioned silicone rubber protective coating, comprising the following steps: mixing and stirring each raw material according to the weight parts, degassing to obtain a silicone rubber protective coating, applying the protective coating to the surface of a substrate, heating to 80°C, and vulcanizing for 2 hours to obtain a silicone rubber protective coating.
[0017] Thirdly, the present invention also provides an application of the above-mentioned silicone rubber protective coating, which can be used as a self-cleaning water conveyance protective coating.
[0018] The present invention has the following advantages over the prior art:
[0019] This invention significantly improves the hydrophobic properties of silicone rubber coatings by adding aerogel powder with superhydrophobic properties to the coating material. The aerogel powder used in this application is prepared from straw cellulose, which not only enables the rational utilization of straw resources, but also provides better waterproof performance than conventional cellulose aerogel powder when applied to silicone rubber coatings. Detailed Implementation
[0020] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the embodiments of this invention pertain. If any definition stated in this section is contrary to or otherwise inconsistent with a definition stated in a patent, patent application, published patent application, or other publication incorporated herein by reference, the definitions listed here shall prevail over those incorporated herein by reference.
[0022] Unless otherwise specified, the methods used in the following embodiments are conventional methods. Unless otherwise specified, the materials, reagents, and instruments used are conventional materials, reagents, and instruments in the art, and can be obtained commercially by those skilled in the art.
[0023] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1 to 5” is disclosed, the described range should be interpreted as including ranges “1 to 4”, “1 to 3”, “1 to 2”, “1 to 2 and 4 to 5”, “1 to 3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range. In this specification and claims, range definitions may be combined and / or interchanged, unless otherwise stated, these ranges include all subranges contained therein.
[0024] Example 1.
[0025] This embodiment prepares a silicone rubber protective coating. The coating raw materials include: 90g of phenylene ether silicone rubber (viscosity 5000mPa·s), 1g of straw cellulose aerogel powder (average particle size 300nm), 5g of silica, 0.01g of platinum catalyst, 5g of methylphenyl hydrogen silicone oil, and 0.001g of 1-butynylcyclohexanol.
[0026] Preparation of straw cellulose aerogel powder:
[0027] Fragments of straw were immersed in ethanol, heated to 75°C, and refluxed for 4 hours. After filtration and drying, the dried straw fragments were soaked in 8% hydrogen peroxide solution and heated to 50°C for 6 hours. Then, they were rinsed with deionized water. The straw fragments were then soaked in acetic acid solution with a pH of 4 and heated to 70°C for 3 hours. After that, they were soaked in sodium hydroxide solution with a pH of 12 for 10 hours. After rinsing with deionized water until neutral, straw cellulose was obtained. Water was added to the straw cellulose to prepare a 1% (w / w) straw cellulose suspension. Hydrochloric acid was added to adjust the pH to 4, and the suspension was stirred for 3 hours. After filtration, hydrogel was obtained. The hydrogel was freeze-dried to obtain aerogel. The aerogel was pulverized to an average particle size of 300 nm to obtain aerogel powder.
[0028] Preparation of silicone rubber protective coating:
[0029] After mixing and stirring the raw materials according to the above proportions, the mixture is degassed to obtain a silicone rubber protective coating.
[0030] Example 2
[0031] Based on Example 1, keeping other conditions unchanged, the coating raw materials include: 95g of phenylene ether silicone rubber (viscosity 5000mPa·s), 3g of straw cellulose aerogel powder (average particle size 300nm), 8g of silica, 0.02g of platinum catalyst, 7g of methylphenyl hydrogen silicone oil, and 0.001g of 1-butynylcyclohexanol.
[0032] Example 3
[0033] Based on Example 1, keeping other conditions unchanged, the coating raw materials include: 100g of phenylene ether silicone rubber (viscosity 5000mPa·s), 5g of straw cellulose aerogel powder (average particle size 300nm), 10g of silica, 0.03g of platinum catalyst, 10g of methylphenyl hydrogen silicone oil, and 0.001g of 1-butynylcyclohexanol.
[0034] Example 4
[0035] Based on Example 1, keeping other conditions unchanged, the viscosity of the phenylene ether silicone rubber is 7000 mPa·s.
[0036] Example 5
[0037] Based on Example 1, keeping other conditions unchanged, the viscosity of the phenylene ether silicone rubber is 8000 mPa·s.
[0038] Example 6
[0039] Based on Example 1, keeping other conditions unchanged, wherein the average particle size of the aerogel powder is 200 nm.
[0040] Example 7
[0041] Based on Example 1, keeping other conditions unchanged, wherein the average particle size of the aerogel powder is 500 nm.
[0042] Example 8
[0043] Based on Example 1, keeping other conditions unchanged, in the preparation process of straw cellulose aerogel powder, after preparing a straw cellulose suspension with a mass concentration of 1%, n-octyltriethoxysilane is added, and the mass concentration of n-octyltriethoxysilane in the suspension is 0.1%.
[0044] Example 9
[0045] Based on Example 1, keeping other conditions unchanged, in the preparation process of straw cellulose aerogel powder, after preparing a straw cellulose suspension with a mass concentration of 1%, methyltrimethoxysilane is added, the mass concentration of methyltrimethoxysilane in the suspension is 0.1%, and then hydrochloric acid is added to adjust the pH.
[0046] Comparative Example 1
[0047] Based on Example 1, keeping other conditions unchanged, the aerogel powder used is cellulose aerogel powder. The preparation method of the cellulose aerogel powder includes:
[0048] A straw cellulose suspension with a mass concentration of 1% was prepared by adding water to vitamin B1. Hydrochloric acid was added to adjust the pH to 4, and the mixture was stirred for 3 hours. After filtration, a hydrogel was obtained. The hydrogel was freeze-dried to obtain an aerogel. The aerogel was then pulverized to an average particle size of 300 nm to obtain aerogel powder.
[0049] Comparative Example 2
[0050] Based on Example 1, keeping other conditions unchanged, the aerogel powder was replaced with the same mass of silica.
[0051] Comparative Example 3
[0052] Based on Example 1, keeping other conditions unchanged, the average particle size of the aerogel powder is 150 nm.
[0053] Comparative Example 4
[0054] Based on Example 1, keeping other conditions unchanged, the average particle size of the aerogel powder is 550 nm.
[0055] The silicone rubber protective coatings prepared in the above examples and comparative examples were coated and then heated to 80°C for 2 hours to obtain silicone rubber protective coatings. The hydrophobicity, abrasion resistance, and adhesion of the protective coatings were tested, and the results are shown in the table below:
[0056]
[0057] The above abrasion resistance test method is in accordance with GB / T 1689-2014 Determination of Abrasion Resistance of Vulcanized Rubber. The abrasion test is carried out using an Akron abrasion tester to obtain the wear mass (unit: g). The adhesion test is carried out using a tensile tester.
[0058] As can be seen from the experimental data of the above embodiments and comparative examples, the silicone rubber protective coating of the present invention can not only greatly enhance the hydrophobic properties, but also improve the wear resistance and adhesion to a certain extent, and has good application prospects.
[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A silicone rubber protective coating, characterized in that, The raw materials for the protective coating, by weight, include: 90 parts silicone rubber base, 1 part straw cellulose aerogel powder with an average particle size of 300 nm, 5 parts silica, 0.01 parts platinum catalyst, 5 parts methylphenyl hydrogen-containing silicone oil, and 0.001 parts inhibitor. The preparation method of the straw cellulose aerogel powder includes: immersing straw fragments in ethanol, heating to 75°C until it flows out for 4 hours, filtering and drying; immersing the dried straw fragments in an 8% hydrogen peroxide solution and heating to 50°C for 6 hours, then rinsing with deionized water; immersing the rinsed straw fragments in acetic acid solution with a pH of 4. The solution was heated to 70°C and kept at that temperature for 3 hours. Then, it was soaked in a sodium hydroxide solution with a pH of 12 for 10 hours and rinsed with deionized water until neutral to obtain straw cellulose. Water was added to the straw cellulose to prepare a straw cellulose suspension with a mass concentration of 1%. Octyltriethoxysilane was added to the straw cellulose suspension to make the mass concentration of octyltriethoxysilane in the straw cellulose suspension 0.1%. Hydrochloric acid was added to adjust the pH to 4, and the mixture was stirred for 3 hours. The mixture was filtered to obtain a hydrogel. The hydrogel was freeze-dried and pulverized to obtain straw cellulose aerogel powder with an average particle size of 300 nm.
2. A method for preparing the silicone rubber protective coating according to claim 1, characterized in that, The process includes the following steps: mixing and stirring phenyl ether silicone rubber, straw cellulose aerogel powder, silica, platinum catalyst, methyl phenyl hydrogen silicone oil and inhibitor evenly, and then degassing to obtain a silicone rubber protective coating. The protective coating is then applied to the surface of a substrate, heated to 80°C, and vulcanized for 2 hours to obtain a silicone rubber protective coating layer.
Citation Information
Patent Citations
Novel low-thermal-conductivity thermal-insulation coating adhesive and preparation method thereof
CN106700925A
Flexible thermal protection coating, flexible thermal protection coating layer for ethylene propylene rubber, and preparation method of flexible thermal protection coating layer
CN113667399A