A high-nitrogen low-nickel alloy steel and smelting method thereof

The medium-frequency induction furnace and ultrasonic oscillation technology are used to smelt high-nitrogen and low-nickel alloy steel under normal pressure, which solves the complexity and cost problems of high-pressure smelting, achieves uniform distribution of nitrogen and improves material properties.

CN118256828BActive Publication Date: 2024-10-22烟台哈尔滨工程大学研究院
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410408180.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-07
Publication Date
2024-10-22
Estimated Expiration
2044-04-07

AI Technical Summary

Technical Problem

The existing smelting technology for high-nitrogen steel requires high-pressure equipment and is complex to operate, which increases production costs and safety risks. It is difficult to achieve uniformity of nitrogen distribution and has limited industrial application.

Method used

A medium-frequency induction furnace is used for atmospheric smelting, an ultrasonic oscillation device is used to promote the solid solution of nitrogen atoms into the iron lattice, and simple raw materials and processes are combined to achieve the preparation of high-nitrogen and low-nickel alloy steel.

Benefits of technology

It achieves a substantial increase in nitrogen under normal pressure, reduces solidification defects such as pores, segregation, shrinkage, etc., simplifies the process, reduces costs, is suitable for industrial production, and improves the corrosion resistance and strength of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118256828B_ABST
    Figure CN118256828B_ABST
Patent Text Reader

Abstract

A high-nitrogen low-nickel alloy steel and a smelting method thereof belong to the field of alloy steel smelting. In order to reduce the difficulty of preparing the high-nitrogen low-nickel alloy steel and improve the corrosion resistance of the material, the nitrogen content in the material composition of the present invention is 0.6-1.4wt%, the chromium content is 16.0-24.0wt%, the manganese content is 5.0-17.0wt%, the nickel content is 0.5-4.5wt%, the silicon content is 0.2-0.5wt%, the molybdenum content is 1.5-3.5wt%, the niobium content is 0.05-0.3wt%, the titanium content is 0.01-0.25wt%, the cobalt content is ≤0.1wt%, the zinc content is 0.01-0.1wt%, the lead content is 0.01-0.1wt%, the vanadium content is 0.05-0.35wt%, the copper content is ≤0.1wt%, the carbon content is ≤0.05wt%, the sulfur content is ≤0.008wt%, the phosphorus content is ≤0.02wt%, and the balance is iron.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of alloy steel smelting, and specifically relates to a high-nitrogen low-nickel alloy steel and a smelting method thereof. Background Art

[0002] At present, the smelting of high nitrogen steel mainly adopts pressurized nitrogen addition methods, such as ladle nitrogen purge method, pressurized induction melting and pressurized electric slag furnace to complete the nitrogen addition in steel. However, the existing technical solutions have the following shortcomings: 1. High-pressure equipment is required, the equipment investment is large, and the operation is complicated, which limits its industrial development and application. 2. The pressure smelting method must use super-balanced high pressure, add nitride alloy powder, use prefabricated nitrogen alloyed consumable electrodes, and pressurized solidification is required to suppress the precipitation of nitrogen bubbles, thereby increasing the production cost and the complexity of the refining chamber, and reducing the safety of production and the uniformity of nitrogen distribution.

[0003] The invention patent with application number 201510433958.4 and invention name "A method for smelting high nitrogen stainless steel under nitrogen atmospheric pressure" discloses a preparation method for smelting high nitrogen austenitic stainless steel in a vacuum induction furnace by filling nitrogen into the induction furnace and quickly adding nitrides at the end of smelting. However, the induction furnace melting chamber used in this method needs to be evacuated to a vacuum degree of less than 220Pa, and the smelting is carried out under negative pressure nitrogen protection during the high temperature stage, and the preparation method is complicated.

[0004] The invention patent with application number 202111301480.1 and invention name "A high-strength, low-yield ratio, high-corrosion-resistant high-nitrogen steel for marine engineering and its preparation method" discloses the following preparation method: (1) weighing of raw materials; (2) remelting and smelting after ingot preparation; (3) solid solution and forging treatment; (4) hot rolling and post-rolling treatment. However, this method uses an induction furnace crucible with a pressure of 80,000 Pa, which is about 8 atmospheres, and the induction furnace crucible is a small laboratory equipment rather than a normal production equipment. This method is difficult to apply to industrial production. Summary of the invention

[0005] The problem to be solved by the present invention is to reduce the cost of preparing high-nitrogen, low-nickel alloy steel, the difficulty of smelting, and to greatly improve the plasticity and corrosion resistance of the material while ensuring that the high-nitrogen, low-nickel stainless steel has sufficiently high strength, so as to obtain a stainless steel with excellent comprehensive performance, and to propose a high-nitrogen, low-nickel alloy steel and a smelting method thereof.

[0006] To achieve the above object, the present invention is implemented through the following technical solutions:

[0007] A high-nitrogen low-nickel alloy steel, wherein the material composition of the high-nitrogen low-nickel alloy steel is 0.6-1.4wt% nitrogen, 16.0-24.0wt% chromium, 5.0-17.0wt% manganese, 0.5-4.5wt% nickel, 0.2-0.5wt% silicon, 1.5-3.5wt% molybdenum, 0.05-0.3wt% niobium, 0.01-0.25wt% titanium, ≤0.1wt% cobalt, 0.01-0.1wt% zinc, 0.01-0.1wt% lead, 0.01-0.1wt% vanadium, 0.05-0.35wt% copper, ≤0.1wt% carbon, ≤0.05wt% sulfur, ≤0.008wt% phosphorus, and the balance is iron.

[0008] Furthermore, the material composition of the high-nitrogen low-nickel alloy steel includes 0.7wt% nitrogen, 16.5wt% chromium, 8.1wt% manganese, 3.8wt% nickel, 0.35wt% silicon, 2.3wt% molybdenum, 0.12wt% niobium, 0.035wt% titanium, 0.04wt% cobalt, 0.02wt% zinc, 0.04wt% lead, 0.075wt% vanadium, 0.02wt% copper, 0.03wt% carbon, 0.006wt% sulfur, 0.006wt% phosphorus, and the balance is iron.

[0009] Furthermore, the material composition of the high-nitrogen low-nickel alloy steel includes 0.63wt% nitrogen, 18.7wt% chromium, 11.6wt% manganese, 4.2wt% nickel, 0.32wt% silicon, 2.12wt% molybdenum, 0.12wt% niobium, 0.05wt% titanium, 0.05wt% cobalt, 0.035wt% zinc, 0.03wt% lead, 0.2wt% vanadium, 0.04wt% copper, 0.03wt% carbon, 0.005wt% sulfur, 0.004wt% phosphorus, and the remainder is iron.

[0010] Furthermore, the smelting raw materials of the high-nitrogen low-nickel alloy steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide.

[0011] A smelting method of high-nitrogen low-nickel alloy steel comprises the following steps:

[0012] Step 1, according to the elemental composition of high-nitrogen low-nickel alloy steel, raw materials for smelting steel are prepared, wherein the raw materials for smelting steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide, and are set aside;

[0013] Step 2, putting the industrial pure iron weighed in step 1 into a medium frequency induction furnace, applying power and heating until the industrial pure iron is converted into molten iron, adding molybdenum-iron alloy, nickel-iron alloy and chromium-iron alloy, and continuing to heat until all the raw materials are melted to obtain molten liquid A;

[0014] Step 3, in a medium frequency induction furnace, cooling the molten liquid A obtained in step 2 to a certain temperature, adding pure metal manganese, niobium alloy, and cobalt alloy, and after all are melted, heating to a certain temperature, adding high nitrogen ferrochrome alloy to carry out nitrogen alloying treatment, and after the high nitrogen ferrochrome alloy is completely melted, obtaining molten liquid B;

[0015] Step 4, in a medium frequency induction furnace, cooling the molten liquid B obtained in step 3 to a certain temperature, then adding calcium oxide for desulfurization treatment, and then heating it to a certain temperature and then adding CaF2, and refining it under ultrasonic oscillation conditions to obtain molten liquid C;

[0016] Step 5, slagging the molten liquid C obtained in step 4, and then transferring it to a ladle containing rare earth cerium and yttrium oxide at the bottom for modification to obtain a modified molten liquid D;

[0017] Step 6: pouring the modified molten liquid D obtained in step 5 under mechanical oscillation conditions to obtain high-nitrogen, low-nickel alloy steel.

[0018] Furthermore, in step 2, the medium frequency induction furnace is first powered on and heated to 1500-1540°C. After 60-100wt% of the industrial pure iron is converted into molten iron, the temperature is raised to 1560-1600°C until all the raw materials are melted. The frequency of the medium frequency induction furnace is 100-1000Hz.

[0019] Furthermore, in step 3, the melt A is cooled to 1520-1540° C., and slag removal is performed 3-7 times during the melting process of pure metallic manganese until the liquid surface is clean; and then the temperature is raised to 1550-1610° C. again.

[0020] Furthermore, in step 4, the molten liquid B is cooled to 1520-1600°C, and the desulfurization treatment time is 0.5-3h; then the temperature is raised to 1570-1650°C for refining treatment, and the ultrasonic oscillator installed outside the medium frequency induction furnace is turned on, the frequency of the ultrasonic oscillator is 40-100kHz, the ultrasonic oscillation time is 0.5-1h, and the refining treatment time is 0.5-3h.

[0021] Furthermore, in step 5, the slag removal method is to perform slag removal under ultrasonic conditions, and the number of slag removal times is 1-3 times; then the time for the modification treatment is 1-2 minutes, and the total mass of rare earth cerium and yttrium oxide added to the ladle is 0.05-0.3wt% of the mass of the molten liquid C.

[0022] Furthermore, in step 6, the molten liquid D after the modification treatment is poured after the liquid surface is calm. During the pouring, a mechanical oscillation is set outside the membrane shell, and the swing amplitude of the mechanical oscillation is 30-100 mm.

[0023] Beneficial effects of the present invention:

[0024] The smelting method of a high-nitrogen low-nickel alloy steel described in the present invention adopts simple raw materials, and can achieve a significant nitrogen increase effect in stainless steel by normal pressure smelting without nitrogen protective gas. An ultrasonic oscillation device is added to the medium frequency induction smelting furnace, and the high-intensity sound wave energy generated by the high-frequency sound wave of the ultrasonic wave is used to dissolve the nitrogen atoms decomposed by the high-nitrogen ferrochrome into the iron lattice faster, so that the obtained austenite nucleus is more uniform and complete, and the crystal growth is accelerated, and a better solid solution strengthening effect is produced. Under normal pressure smelting conditions, a significant nitrogen increase effect in stainless steel can be achieved without nitrogen protective gas. In addition, the ultrasonic effect can also reduce solidification defects such as pores, segregation, shrinkage and the like.

[0025] The smelting method of the high-nitrogen and low-nickel alloy steel of the present invention adopts a conventional atmospheric pressure induction melting equipment, has a simple preparation process, is easy to operate, and is convenient for industrial production. The raw materials are widely available, have high nitrogen and low nickel components, reduce the price of stainless steel, and have good economic benefits.

[0026] The high-nitrogen, low-nickel alloy steel disclosed in the present invention has excellent corrosion resistance and good strength and plasticity. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a comparison curve of the self-corrosion potential of a high-nitrogen, low-nickel alloy steel prepared according to a specific embodiment of the present invention. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the specific embodiments described are only part of the embodiments of the present invention, rather than all of the specific embodiments. The components of the specific embodiments of the present invention described and shown in the drawings herein can be arranged and designed in various different configurations, and the present invention can also have other embodiments.

[0029] Therefore, the following detailed description of the specific embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents the selected specific embodiments of the present invention. Based on the specific embodiments of the present invention, all other specific embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.

[0030] In order to further understand the content, features and effects of the present invention, the following specific implementation methods are given as examples, and the attached Figure 1 The detailed instructions are as follows: Specific implementation method one:

[0032] A high-nitrogen, low-nickel alloy steel, wherein the material composition of the high-nitrogen, low-nickel alloy steel is 0.81wt% nitrogen, 16.5wt% chromium, 8.1wt% manganese, 3.8wt% nickel, 0.35wt% silicon, 2.3wt% molybdenum, 0.12wt% niobium, 0.035wt% titanium, 0.04wt% cobalt, 0.02wt% zinc, 0.04wt% lead, 0.075wt% vanadium, 0.02wt% copper, 0.03wt% carbon, 0.006wt% sulfur, 0.006wt% phosphorus, and the balance is iron.

[0033] Furthermore, the smelting raw materials of the high-nitrogen low-nickel alloy steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide.

[0034] A smelting method of a high-nitrogen low-nickel alloy steel described in this embodiment comprises the following steps:

[0035] Step 1, according to the elemental composition of the high-nitrogen low-nickel alloy steel of this embodiment, raw materials for smelting steel are prepared, wherein the raw materials for smelting steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide, and are set aside;

[0036] Step 2, putting the industrial pure iron weighed in step 1 into a medium frequency induction furnace, applying power and heating until the industrial pure iron is converted into molten iron, adding molybdenum-iron alloy, nickel-iron alloy and chromium-iron alloy, and continuing to heat until all the raw materials are melted to obtain molten liquid A;

[0037] Furthermore, in step 2, the medium frequency induction furnace is first powered on and heated to 1500° C., and when 60wt% of the industrial pure iron is converted into molten iron, the temperature is raised to 1560° C. until all the raw materials are melted, and the frequency of the medium frequency induction furnace is 1000 Hz;

[0038] Step 3, in a medium frequency induction furnace, cooling the molten liquid A obtained in step 2 to a certain temperature, adding pure metal manganese, niobium alloy, and cobalt alloy, and after all are melted, heating to a certain temperature, adding high nitrogen ferrochrome alloy to carry out nitrogen alloying treatment, and after the high nitrogen ferrochrome alloy is completely melted, obtaining molten liquid B;

[0039] Furthermore, in step 3, the melt A is cooled to 1520° C., and slag is removed four times during the melting process of pure metallic manganese until the liquid surface is clean; then the temperature is raised to 1560° C. again, and an ultrasonic oscillator installed outside the medium frequency induction furnace is turned on during the nitrogen alloying treatment, wherein the frequency of the ultrasonic oscillator is 60 kHz, and the ultrasonic oscillation time is 0.5 h;

[0040] Step 4, in a medium frequency induction furnace, cooling the molten liquid B obtained in step 3 to a certain temperature, then adding calcium oxide for desulfurization treatment, and then heating it to a certain temperature and then adding CaF2, and refining it under ultrasonic oscillation conditions to obtain molten liquid C;

[0041] Furthermore, in step 4, the melt B is cooled to 1540°C and the desulfurization treatment time is 0.5h; then the temperature is raised to 1580°C for refining treatment, and the ultrasonic oscillator installed outside the medium frequency induction furnace is turned on, the frequency of the ultrasonic oscillator is 60kHz, the ultrasonic oscillation time is 0.5h, and the refining treatment time is 0.5h;

[0042] Step 5, slagging the molten liquid C obtained in step 4, and then transferring it to a ladle containing rare earth cerium and yttrium oxide at the bottom for modification to obtain a modified molten liquid D;

[0043] Furthermore, in step 5, the slag removal method is to perform slag removal under ultrasonic conditions, and the number of slag removal is 2 times; then the time for the modification treatment is 2 minutes, and the total mass of rare earth cerium and yttrium oxide added to the ladle is 0.1wt% of the mass of the melt C;

[0044] Step 6, pouring the modified molten liquid D obtained in step 5 under the condition of mechanical oscillation to obtain high-nitrogen low-nickel alloy steel;

[0045] Furthermore, in step 6, the molten liquid D after the modification treatment is poured after the liquid surface is calm. During the pouring, a mechanical oscillation is arranged outside the membrane shell, and the swing amplitude of the mechanical oscillation is 50 mm.

[0046] The smelting method of a high-nitrogen, low-nickel alloy steel described in this embodiment adopts simple raw materials and can achieve a significant nitrogen increase effect in stainless steel by smelting at normal pressure without the need for nitrogen protective gas. An ultrasonic oscillation device is added to the medium-frequency induction smelting furnace, and the ultrasonic effect is used to promote the uniform distribution of nitrogen in the steel, thereby reducing solidification defects such as pores, segregation, shrinkage and the like.

[0047] A high-nitrogen, low-nickel alloy steel prepared by the smelting method of a high-nitrogen, low-nickel alloy steel described in this embodiment, after testing, it is found that the material composition of the high-nitrogen, low-nickel alloy steel has a nitrogen content of 0.81wt%, a chromium content of 16.5wt%, a manganese content of 8.1wt%, a nickel content of 3.8wt%, a silicon content of 0.35wt%, a molybdenum content of 2.3wt%, a niobium content of 0.12wt%, a titanium content of 0.035wt%, a cobalt content of 0.04wt%, a zinc content of 0.02wt%, a lead content of 0.04wt%, a vanadium content of 0.075wt%, a copper content of 0.02wt%, a carbon content of 0.03wt%, a sulfur content of 0.006wt%, a phosphorus content of 0.006wt%, and the remainder is iron.

[0048] A high nitrogen low nickel alloy steel prepared by the smelting method of a high nitrogen low nickel alloy steel described in this embodiment and 316L stainless steel pipe are respectively prepared to prepare 3 mechanical property test samples, wherein the high nitrogen low nickel alloy steel is a sample after solid solution treatment after smelting, and the tensile property test is carried out according to GB / T228 and GB / T229 to obtain the tensile strength and elongation after fracture of the two materials. The test results are shown in Table 1:

[0049] Table 1 Mechanical properties of materials prepared in this embodiment and 316L stainless steel

[0050] ;

[0051] Three test samples were prepared using the high nitrogen low nickel alloy steel and 316L stainless steel pipe described in this embodiment, and the self-corrosion potential test was carried out in natural seawater in Weihai for 28 days. The test equipment was a digital multimeter and the reference electrode was a saturated calomel electrode. The self-corrosion potential test results of the high nitrogen low nickel alloy steel and 316L stainless steel samples are shown in Figure 1 and Table 2:

[0052] Table 2 Self-corrosion potential test results of the material of this embodiment and 316L stainless steel

[0053] ;

[0054] from Figure 1 It can be seen from the data in Table 2 that the self-corrosion potential of the high nitrogen low nickel alloy steel described in this embodiment is higher than that of 316L stainless steel, indicating that the hydrogen evolution corrosion tendency of the high nitrogen low nickel alloy steel described in this embodiment is lower than that of 316L stainless steel.

[0055] The corrosion rate results of the indoor full immersion corrosion test of the high nitrogen low nickel alloy steel sample and the 316L sample in the natural seawater of Weihai are shown in Table 3:

[0056] Table 3 Results of indoor full immersion corrosion test on materials and 316L stainless steel in this embodiment

[0057] ;

[0058] ;

[0059] Table 3 shows the results of the indoor full immersion corrosion test of the high nitrogen low nickel alloy steel and 316L stainless steel described in this embodiment. The corrosion rate of the high nitrogen low nickel stainless steel is lower than that of the 316L stainless steel, indicating that the corrosion resistance of the high nitrogen low nickel stainless steel is better than that of the 316L stainless steel. Specific implementation method 2:

[0061] A high-nitrogen, low-nickel alloy steel, wherein the material composition of the high-nitrogen, low-nickel alloy steel is 1.23wt% nitrogen, 18.7wt% chromium, 11.6wt% manganese, 4.2wt% nickel, 0.32wt% silicon, 2.12wt% molybdenum, 0.12wt% niobium, 0.05wt% titanium, 0.05wt% cobalt, 0.035wt% zinc, 0.03wt% lead, 0.2wt% vanadium, 0.04wt% copper, 0.03wt% carbon, 0.005wt% sulfur, 0.004wt% phosphorus, and the remainder is iron.

[0062] Furthermore, the smelting raw materials of the high-nitrogen low-nickel alloy steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide.

[0063] A smelting method of a high-nitrogen low-nickel alloy steel described in this embodiment comprises the following steps:

[0064] Step 1, according to the elemental composition of the high-nitrogen low-nickel alloy steel of this embodiment, raw materials for smelting steel are prepared, wherein the raw materials for smelting steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide, and are set aside;

[0065] Step 2, putting the industrial pure iron weighed in step 1 into a medium frequency induction furnace, applying power and heating until the industrial pure iron is converted into molten iron, adding molybdenum-iron alloy, nickel-iron alloy and chromium-iron alloy, and continuing to heat until all the raw materials are melted to obtain molten liquid A;

[0066] Furthermore, in step 2, the medium frequency induction furnace is first powered on and heated to 1520° C., and when 70wt% of the industrial pure iron is converted into molten iron, the temperature is raised to 1560° C. until all the raw materials are melted, and the frequency of the medium frequency induction furnace is 1000 Hz;

[0067] Step 3, in a medium frequency induction furnace, cooling the molten liquid A obtained in step 2 to a certain temperature, adding pure metal manganese, niobium alloy, and cobalt alloy, and after all are melted, heating to a certain temperature, adding high nitrogen ferrochrome alloy to carry out nitrogen alloying treatment, and after the high nitrogen ferrochrome alloy is completely melted, obtaining molten liquid B;

[0068] Furthermore, in step 3, the melt A is cooled to 1530° C., and slag is removed four times during the melting process of pure metallic manganese until the liquid surface is clean; then the temperature is raised to 1560° C. again, and an ultrasonic oscillator installed outside the medium frequency induction furnace is turned on during the nitrogen alloying treatment, the frequency of the ultrasonic oscillator is 200 kHz, and the ultrasonic oscillation time is 0.5 h;

[0069] Step 4, in a medium frequency induction furnace, cooling the molten liquid B obtained in step 3 to a certain temperature, then adding calcium oxide for desulfurization treatment, and then heating it to a certain temperature and then adding CaF2, and refining it under ultrasonic oscillation conditions to obtain molten liquid C;

[0070] Furthermore, in step 4, the melt B is cooled to 1540°C and the desulfurization treatment time is 0.5h; then the temperature is raised to 1580°C for refining treatment, and the ultrasonic oscillator installed outside the medium frequency induction furnace is turned on, the frequency of the ultrasonic oscillator is 60kHz, the ultrasonic oscillation time is 0.5h, and the refining treatment time is 0.5h;

[0071] Step 5, slagging the molten liquid C obtained in step 4, and then transferring it to a ladle containing rare earth cerium and yttrium oxide at the bottom for modification to obtain a modified molten liquid D;

[0072] Furthermore, in step 5, the slag removal method is to perform slag removal under ultrasonic conditions for 3 times; then the modification time is 2 minutes, and the total mass of rare earth cerium and yttrium oxide added to the ladle is 0.1wt% of the mass of the melt C;

[0073] Step 6, pouring the modified molten liquid D obtained in step 5 under the condition of mechanical oscillation to obtain high-nitrogen low-nickel alloy steel;

[0074] Furthermore, in step 6, the molten liquid D after the modification treatment is poured after the liquid surface is calm. During the pouring, a mechanical oscillation is arranged outside the membrane shell, and the swing amplitude of the mechanical oscillation is 50 mm.

[0075] The smelting method of a high-nitrogen low-nickel alloy steel described in this embodiment uses simple raw materials, adds an ultrasonic oscillation device to a medium-frequency induction smelting furnace, and uses the high-intensity sound wave energy generated by the high-frequency sound waves of the ultrasonic wave to dissolve the nitrogen atoms decomposed from the high-nitrogen ferrochrome into the iron lattice faster, so that the obtained austenite nuclei are more uniform and complete, accelerate crystal growth, and produce a better solid solution strengthening effect. Under normal pressure smelting conditions, a significant nitrogen increase effect can be achieved in stainless steel without nitrogen protective gas. In addition, the ultrasonic effect can also reduce solidification defects such as pores, segregation, shrinkage and other defects.

[0076] A high-nitrogen, low-nickel alloy steel is prepared by the smelting method of a high-nitrogen, low-nickel alloy steel described in this embodiment. After testing, the material composition of the high-nitrogen, low-nickel alloy steel is found to be 1.23wt% nitrogen, 18.7wt% chromium, 11.6wt% manganese, 4.2wt% nickel, 0.32wt% silicon, 2.12wt% molybdenum, 0.12wt% niobium, 0.05wt% titanium, 0.05wt% cobalt, 0.035wt% zinc, 0.03wt% lead, 0.2wt% vanadium, 0.04wt% copper, 0.03wt% carbon, 0.005wt% sulfur, 0.004wt% phosphorus, and the remainder is iron. Specific implementation method three:

[0078] A high-nitrogen, low-nickel alloy steel, wherein the material composition of the high-nitrogen, low-nickel alloy steel is 0.74wt% nitrogen, 18.2wt% chromium, 8.5wt% manganese, 4.3wt% nickel, 0.43wt% silicon, 3.24wt% molybdenum, 0.2wt% niobium, 0.16wt% titanium, 0.05wt% cobalt, 0.04wt% zinc, 0.03wt% lead, 0.06wt% vanadium, 0.04wt% copper, 0.03wt% carbon, 0.006wt% sulfur, 0.005wt% phosphorus, and the balance is iron.

[0079] Furthermore, the smelting raw materials of the high-nitrogen low-nickel alloy steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide.

[0080] A smelting method of a high-nitrogen low-nickel alloy steel described in this embodiment comprises the following steps:

[0081] Step 1, according to the elemental composition of the high-nitrogen low-nickel alloy steel of this embodiment, raw materials for smelting steel are prepared, wherein the raw materials for smelting steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide, and are set aside;

[0082] Step 2, putting the industrial pure iron weighed in step 1 into a medium frequency induction furnace, applying power and heating until the industrial pure iron is converted into molten iron, adding molybdenum-iron alloy, nickel-iron alloy and chromium-iron alloy, and continuing to heat until all the raw materials are melted to obtain molten liquid A;

[0083] Furthermore, in step 2, the medium frequency induction furnace is first powered on and heated to 1530° C., and when 80 wt% of the industrial pure iron is converted into molten iron, the temperature is raised to 1570° C. until all the raw materials are melted, and the frequency of the medium frequency induction furnace is 100 Hz;

[0084] Step 3, in a medium frequency induction furnace, cooling the molten liquid A obtained in step 2 to a certain temperature, adding pure metal manganese, niobium alloy, and cobalt alloy, and after all are melted, heating to a certain temperature, adding high nitrogen ferrochrome alloy to carry out nitrogen alloying treatment, and after the high nitrogen ferrochrome alloy is completely melted, obtaining molten liquid B;

[0085] Furthermore, in step 3, the melt A is cooled to 1520° C., and slag is removed 5 times during the melting process of pure metallic manganese until the liquid surface is clean; then the temperature is raised to 1570° C. again, and an ultrasonic oscillator installed outside the medium frequency induction furnace is turned on during the nitrogen alloying treatment, wherein the frequency of the ultrasonic oscillator is 70 kHz, and the ultrasonic oscillation time is 0.6 h;

[0086] Step 4, in a medium frequency induction furnace, cooling the molten liquid B obtained in step 3 to a certain temperature, then adding calcium oxide for desulfurization treatment, and then heating it to a certain temperature and then adding CaF2, and refining it under ultrasonic oscillation conditions to obtain molten liquid C;

[0087] Furthermore, in step 4, the melt B is cooled to 1550°C, and the desulfurization treatment time is 0.6h; then the temperature is raised to 1580°C for refining treatment, and the ultrasonic oscillator installed outside the medium frequency induction furnace is turned on, the frequency of the ultrasonic oscillator is 70kHz, the ultrasonic oscillation time is 0.5h, and the refining treatment time is 0.5h;

[0088] Step 5, slagging the molten liquid C obtained in step 4, and then transferring it to a ladle containing rare earth cerium and yttrium oxide at the bottom for modification to obtain a modified molten liquid D;

[0089] Furthermore, in step 5, the slag removal method is to perform slag removal under ultrasonic conditions, and the number of slag removals is 3 times; then the modification time is 2 minutes, and the total mass of rare earth cerium and yttrium oxide added to the ladle is 0.05wt% of the mass of the melt C;

[0090] Step 6, pouring the modified molten liquid D obtained in step 5 under the condition of mechanical oscillation to obtain high-nitrogen low-nickel alloy steel;

[0091] Furthermore, in step 6, the molten liquid D after the modification treatment is poured after the liquid surface is calm. During the pouring, a mechanical oscillation is arranged outside the membrane shell, and the swing amplitude of the mechanical oscillation is 40 mm.

[0092] The smelting method of a high-nitrogen, low-nickel alloy steel described in this embodiment adopts simple raw materials and can achieve a significant nitrogen increase effect in stainless steel by smelting at normal pressure without the need for nitrogen protective gas. An ultrasonic oscillation device is added to the medium-frequency induction smelting furnace, and the ultrasonic effect is used to promote the uniform distribution of nitrogen in the steel, thereby reducing solidification defects such as pores, segregation, shrinkage and the like.

[0093] A high-nitrogen, low-nickel alloy steel is prepared by the smelting method of a high-nitrogen, low-nickel alloy steel described in this embodiment. After testing, the material components of the high-nitrogen, low-nickel alloy steel are 0.74wt% nitrogen, 18.2wt% chromium, 8.5wt% manganese, 4.3wt% nickel, 0.43wt% silicon, 3.24wt% molybdenum, 0.2wt% niobium, 0.16wt% titanium, 0.05wt% cobalt, 0.04wt% zinc, 0.03wt% lead, 0.06wt% vanadium, 0.04wt% copper, 0.03wt% carbon, 0.006wt% sulfur, 0.005wt% phosphorus, and the remainder is iron. Specific implementation method four:

[0095] A high-nitrogen low-nickel alloy steel, wherein the material composition of the high-nitrogen low-nickel alloy steel is 0.97wt% nitrogen, 17.4wt% chromium, 13.5wt% manganese, 4.5wt% nickel, 0.32wt% silicon, 2.15wt% molybdenum, 0.25wt% niobium, 0.23wt% titanium, 0.06wt% cobalt, 0.08wt% zinc, 0.08wt% lead, 0.06wt% vanadium, 0.03wt% copper, 0.03wt% carbon, 0.006wt% sulfur, 0.03wt% phosphorus, and the balance is iron.

[0096] Furthermore, the smelting raw materials of the high-nitrogen low-nickel alloy steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide.

[0097] A smelting method of a high-nitrogen low-nickel alloy steel described in this embodiment comprises the following steps:

[0098] Step 1, according to the elemental composition of the high-nitrogen low-nickel alloy steel of this embodiment, raw materials for smelting steel are prepared, wherein the raw materials for smelting steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide, and are set aside;

[0099] Step 2, putting the industrial pure iron weighed in step 1 into a medium frequency induction furnace, applying power and heating until the industrial pure iron is converted into molten iron, adding molybdenum-iron alloy, nickel-iron alloy and chromium-iron alloy, and continuing to heat until all the raw materials are melted to obtain molten liquid A;

[0100] Furthermore, in step 2, the medium frequency induction furnace is first powered on and heated to 1540° C., and when 90wt% of the industrial pure iron is converted into molten iron, the temperature is raised to 1590° C. until all the raw materials are melted, and the frequency of the medium frequency induction furnace is 1000 Hz;

[0101] Step 3, in a medium frequency induction furnace, cooling the molten liquid A obtained in step 2 to a certain temperature, adding pure metal manganese, niobium alloy, and cobalt alloy, and after all are melted, heating to a certain temperature, adding high nitrogen ferrochrome alloy to carry out nitrogen alloying treatment, and after the high nitrogen ferrochrome alloy is completely melted, obtaining molten liquid B;

[0102] Furthermore, in step 3, the melt A is cooled to 1540° C., and slag is removed 7 times during the melting process of pure metallic manganese until the liquid surface is clean; then the temperature is raised to 1610° C. again, and an ultrasonic oscillator installed outside the medium frequency induction furnace is turned on during the nitrogen alloying treatment, the frequency of the ultrasonic oscillator is 80 kHz, and the ultrasonic oscillation time is 1 hour;

[0103] Step 4, in a medium frequency induction furnace, cooling the molten liquid B obtained in step 3 to a certain temperature, then adding calcium oxide for desulfurization treatment, and then heating it to a certain temperature and then adding CaF2, and refining it under ultrasonic oscillation conditions to obtain molten liquid C;

[0104] Furthermore, in step 4, the melt B is cooled to 1600°C and the desulfurization treatment time is 2 hours; then the temperature is raised to 1650°C for refining treatment, and the ultrasonic oscillator installed outside the medium frequency induction furnace is turned on, the frequency of the ultrasonic oscillator is 80kHz, the ultrasonic oscillation time is 0.5 hours, and the refining treatment time is 2 hours;

[0105] Step 5, slagging the molten liquid C obtained in step 4, and then transferring it to a ladle containing rare earth cerium and yttrium oxide at the bottom for modification to obtain a modified molten liquid D;

[0106] Furthermore, in step 5, the slag removal method is to perform slag removal under ultrasonic conditions for 3 times; then the modification time is 2 minutes, and the total mass of rare earth cerium and yttrium oxide added to the ladle is 0.2wt% of the mass of the melt C;

[0107] Step 6, pouring the modified molten liquid D obtained in step 5 under the condition of mechanical oscillation to obtain high-nitrogen low-nickel alloy steel;

[0108] Furthermore, in step 6, the molten liquid D after the modification treatment is poured after the liquid surface is calm. During the pouring, a mechanical oscillation is set outside the membrane shell, and the swing amplitude of the mechanical oscillation is 100 mm.

[0109] The smelting method of a high-nitrogen, low-nickel alloy steel described in this embodiment adopts simple raw materials and can achieve a significant nitrogen increase effect in stainless steel by smelting at normal pressure without the need for nitrogen protective gas. An ultrasonic oscillation device is added to the medium-frequency induction smelting furnace, and the ultrasonic effect is used to promote the uniform distribution of nitrogen in the steel, thereby reducing solidification defects such as pores, segregation, shrinkage and the like.

[0110] A high-nitrogen, low-nickel alloy steel is prepared by the smelting method of a high-nitrogen, low-nickel alloy steel described in this embodiment. After testing, the material composition of the high-nitrogen, low-nickel alloy steel is 0.97wt% nitrogen, 17.4wt% chromium, 13.5wt% manganese, 4.5wt% nickel, 0.32wt% silicon, 2.15wt% molybdenum, 0.25wt% niobium, 0.23wt% titanium, 0.06wt% cobalt, 0.08wt% zinc, 0.08wt% lead, 0.06wt% vanadium, 0.03wt% copper, 0.03wt% carbon, 0.006wt% sulfur, 0.03wt% phosphorus, and the remainder is iron. Specific implementation method five:

[0112] The difference between this embodiment and specific embodiment one is that the material composition of the high-nitrogen low-nickel alloy steel described in this embodiment is 0.7wt% nitrogen, 16.5wt% chromium, 8.1wt% manganese, 3.8wt% nickel, 0.35wt% silicon, 2.3wt% molybdenum, 0.12wt% niobium, 0.035wt% titanium, 0.04wt% cobalt, 0.02wt% zinc, 0.04wt% lead, 0.075wt% vanadium, 0.02wt% copper, 0.03wt% carbon, 0.006wt% sulfur, 0.006wt% phosphorus, and the remainder is iron. Specific implementation method six:

[0114] The difference between this embodiment and specific embodiment one is that the material composition of the high-nitrogen low-nickel alloy steel described in this embodiment has a nitrogen content of 0.63wt%, a chromium content of 18.7wt%, a manganese content of 11.6wt%, a nickel content of 4.2wt%, a silicon content of 0.32wt%, a molybdenum content of 2.12wt%, a niobium content of 0.12wt%, a titanium content of 0.05wt%, a cobalt content of 0.05wt%, a zinc content of 0.035wt%, a lead content of 0.03wt%, a vanadium content of 0.2wt%, a copper content of 0.04wt%, a carbon content of 0.03wt%, a sulfur content of 0.005wt%, a phosphorus content of 0.004wt%, and the remainder is iron.

[0115] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0116] Although the present application has been described above with reference to specific embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, as long as there is no structural conflict, the various features in the specific embodiments disclosed in the present application may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A smelting method for high-nitrogen low-nickel alloy steel, wherein the material composition of the high-nitrogen low-nickel alloy steel is 0.6-1.4wt% nitrogen, 16.0-24.0wt% chromium, 5.0-17.0wt% manganese, 0.5-4.5wt% nickel, 0.2-0.5wt% silicon, 1.5-3.5wt% molybdenum, 0.05-0.3wt% niobium, 0.01-0.25wt% titanium, ≤0.1wt% cobalt, 0.01-0.1wt% zinc, 0.01-0.1wt% lead, 0.01-0.1wt% vanadium, ≤0.1wt% copper, ≤0.05wt% carbon, ≤0.008wt% sulfur, ≤0.02wt% phosphorus, and the remainder is iron, characterized in that: The steps include: Step 1, according to the elemental composition of high-nitrogen low-nickel alloy steel, raw materials for smelting steel are prepared, wherein the raw materials for smelting steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide, and are set aside; Step 2, putting the industrial pure iron weighed in step 1 into a medium frequency induction furnace, applying power and heating until the industrial pure iron is converted into molten iron, adding molybdenum-iron alloy, nickel-iron alloy and chromium-iron alloy, and continuing to heat until all the raw materials are melted to obtain molten liquid A; Step 3, in a medium frequency induction furnace, cooling the molten liquid A obtained in step 2 to a certain temperature, adding pure metal manganese, niobium alloy, and cobalt alloy, and after all are melted, heating to a certain temperature, adding high nitrogen ferrochrome alloy to carry out nitrogen alloying treatment, and after the high nitrogen ferrochrome alloy is completely melted, obtaining molten liquid B; In step 3, the melt A is cooled to 1520-1540° C., and slag is removed 3-7 times during the melting process of pure metallic manganese until the liquid surface is clean; then the temperature is raised to 1550-1610° C. again, and an ultrasonic oscillator installed outside the medium frequency induction furnace is turned on during the nitrogen alloying treatment, wherein the frequency of the ultrasonic oscillator is 40-100 kHz, and the ultrasonic oscillation time is 0.5-1 h; Step 4, in a medium frequency induction furnace, cooling the molten liquid B obtained in step 3 to a certain temperature, then adding calcium oxide for desulfurization treatment, and then heating it to a certain temperature and then adding CaF2, and refining it under ultrasonic oscillation conditions to obtain molten liquid C; In step 4, the melt B is cooled to 1520-1600°C, and the desulfurization treatment time is 0.5-3h; then the temperature is raised to 1570-1650°C for refining treatment, and an ultrasonic oscillator installed outside the medium frequency induction furnace is turned on. The frequency of the ultrasonic oscillator is 40-100kHz, the ultrasonic oscillation time is 0.5-1h, and the refining treatment time is 0.5-3h; Step 5, slagging the molten liquid C obtained in step 4, and then transferring it to a ladle containing rare earth cerium and yttrium oxide at the bottom for modification to obtain a modified molten liquid D; Step 6: pouring the modified molten liquid D obtained in step 5 under mechanical oscillation conditions to obtain high-nitrogen, low-nickel alloy steel.

2. The smelting method of a high-nitrogen low-nickel alloy steel according to claim 1, characterized in that: In step 2, the medium frequency induction furnace is first powered on and heated to 1500-1540°C. After 60-100wt% of the industrial pure iron is converted into molten iron, the temperature is raised to 1560-1600°C until all the raw materials are melted. The frequency of the medium frequency induction furnace is 100-1000Hz.

3. The smelting method of a high-nitrogen low-nickel alloy steel according to claim 2, characterized in that: In step 5, the slag removal method is to perform slag removal under ultrasonic conditions, and the number of slag removal times is 1-3 times; then the time for the modification treatment is 1-2 minutes, and the total mass of rare earth cerium and yttrium oxide added to the ladle is 0.05-0.3wt% of the mass of the molten liquid C.

4. The smelting method of a high-nitrogen low-nickel alloy steel according to claim 3, characterized in that: In step 6, the melt D after the modification treatment is poured after the liquid level is calm. During the pouring, a mechanical oscillation is set outside the membrane shell, and the swing amplitude of the mechanical oscillation is 30 to 100 mm.

5. The smelting method of a high-nitrogen low-nickel alloy steel according to claim 4, characterized in that: The material composition of the high-nitrogen low-nickel alloy steel includes 0.7wt% nitrogen, 16.5wt% chromium, 8.1wt% manganese, 3.8wt% nickel, 0.35wt% silicon, 2.3wt% molybdenum, 0.12wt% niobium, 0.035wt% titanium, 0.04wt% cobalt, 0.02wt% zinc, 0.04wt% lead, 0.075wt% vanadium, 0.02wt% copper, 0.03wt% carbon, 0.006wt% sulfur, 0.006wt% phosphorus, and the balance is iron.

6. The smelting method of a high-nitrogen low-nickel alloy steel according to claim 5, characterized in that: The material composition of the high-nitrogen low-nickel alloy steel includes 0.63wt% nitrogen, 18.7wt% chromium, 11.6wt% manganese, 4.2wt% nickel, 0.32wt% silicon, 2.12wt% molybdenum, 0.12wt% niobium, 0.05wt% titanium, 0.05wt% cobalt, 0.035wt% zinc, 0.03wt% lead, 0.2wt% vanadium, 0.04wt% copper, 0.03wt% carbon, 0.005wt% sulfur, 0.004wt% phosphorus, and the balance is iron.

7. The smelting method of a high-nitrogen low-nickel alloy steel according to claim 6, characterized in that: The smelting raw materials of the high-nitrogen low-nickel alloy steel include industrial pure iron, pure metallic manganese, ferromolybdenum alloy, ferronickel alloy, ferrochrome alloy, high-nitrogen ferrochrome alloy, niobium alloy, cobalt alloy, calcium oxide, CaF2, rare earth cerium, and yttrium oxide.

Citation Information

Patent Citations

  • Method for smelting high-nitrogen stainless steel under nitrogen normal pressure

    CN104988279A

  • High-strength low-yield-ratio high-corrosion-resistance maritime work high-nitrogen steel and preparation method thereof

    CN114032461A

  • Stainless steel, stainless steel wire for bridge pull sling as well as preparation methods and application thereof

    CN102534424A

  • Seamless thin-wall high-nitrogen steel pipe and preparation method thereof

    CN117947247A

  • Steel sheet having superior formability and shape accuracy, and method for manufacturing the same

    KR1020030032437A