Hydrogel Evaporators with Hierarchical Gradient Structures, Their Preparation Methods and Applications

By designing a hydrogel evaporator with a hierarchical gradient structure, and utilizing nanocellulose and carbon nanotube materials, the problems of salt ion transfer and environmental pollution are solved, achieving efficient water evaporation and salt exchange, which is suitable for seawater desalination and wastewater treatment.

CN118286984BActive Publication Date: 2026-11-10DONGHUA UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410560116.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-08
Publication Date
2026-11-10
Estimated Expiration
2044-05-08

AI Technical Summary

Technical Problem

Existing solar evaporators have difficulty effectively limiting the transfer of salt ions when evaporating brine, which leads to salt crystallization and precipitation on the evaporator surface. Furthermore, traditional evaporator materials may be harmful to the environment, and the evaporation efficiency is low.

Method used

A hydrogel evaporator with a hierarchical gradient structure is used, with a three-dimensional porous network structure with different pore sizes in the upper and lower layers, and a secondary pore structure with macropores and micropores in the lower layer. It is prepared by freeze-thaw cycle method, using nanocellulose and carbon nanotubes as the main materials to enhance capillary action and hydrophilicity.

Benefits of technology

It effectively limits the transfer of salt ions, reduces salt accumulation, improves water transport rate and evaporation efficiency, is environmentally friendly and easy to operate, and is suitable for seawater desalination and wastewater treatment in printing and dyeing plants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118286984B_ABST
    Figure CN118286984B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of interfacial photothermal conversion technology, and discloses a hydrogel evaporator with a hierarchical gradient structure, its preparation method, and its application. The hydrogel evaporator has a composite layer structure, including adjacent upper and lower layers, both of which have a three-dimensional porous network structure. The preparation method is as follows: a uniform dispersion I containing nanocellulose, polyvinyl alcohol, polyethylene glycol, and deionized water is poured into a template and frozen. Then, a uniform dispersion II containing nanocellulose, polyvinyl alcohol, deionized water, and carbon nanotubes is poured into the template and frozen. The mixture is then thawed, and the above freeze-thaw process is repeated. After washing to remove polyethylene glycol, the product is obtained. The application involves using the hydrogel evaporator for seawater desalination or wastewater treatment in dyeing and printing plants. The hydrogel evaporator of this invention can provide a higher water transport rate and can effectively limit the transfer of salt ions during the evaporation of brine, reduce salt accumulation, and improve evaporation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of interfacial photothermal conversion technology, and specifically relates to a hydrogel evaporator with a hierarchical gradient structure, its preparation method, and its application. Background Technology

[0002] With continuous social development and progress, and the ongoing growth of the global population, water resource consumption and scarcity have become increasingly important issues of concern. Approximately 40% of the world's population faces a severe water crisis due to inadequate water resource management, and it is projected that by 2050, nearly 50 countries worldwide will face severe freshwater shortages. On the one hand, the Earth's freshwater resources are being continuously consumed, leading to severe water shortages in many countries and regions; on the other hand, industrial emissions, agricultural fertilizers, and wastewater discharges are causing serious pollution of water bodies, resulting in a decreasing supply of usable freshwater resources. Traditional methods for seawater desalination and industrial wastewater treatment include distillation (multi-stage flash distillation, multi-effect distillation), reverse osmosis, and membrane filtration, among others. These methods suffer from drawbacks such as high energy consumption, high cost, difficult equipment maintenance, and environmental harm.

[0003] Solar energy, as an inexhaustible energy source, has given rise to solar interface photo-steam conversion technology, which can effectively solve the aforementioned problems. Solar interface photo-steam conversion technology is one of the core technologies of solar evaporators. This technology uses photothermal materials to absorb sunlight and convert it into heat energy to treat seawater and wastewater, transforming them into pure water. It is considered an effective method to solve the freshwater shortage problem. In the manufacture of solar evaporators, materials with good photothermal properties, such as carbon-based materials, semiconductor nanoparticles, and plasma nanoparticles, are typically used to thermally localize solar radiation, thereby ensuring that solar radiation can be efficiently converted into heat energy. During the evaporation process, appropriate thermal management strategies are crucial for suppressing heat loss and improving the evaporator's evaporation efficiency. Simultaneously, the evaporator should have good water transport capacity, delivering water from the bottom to the evaporation interface.

[0004] Existing solar evaporators are mostly based on aerogel systems and composite membrane materials. Among them, solar evaporators with a graded gradient structure are favored for their efficient heat management and water delivery capabilities.

[0005] For example, patent application CN116474667A discloses a graphene composite aerogel, its preparation method and application. This patent constructs and regulates a gradient pore structure to create a capillary pressure difference in the radial direction of the evaporator. The brine spontaneously forms a concentration gradient in the radial direction and eventually crystallizes at the edge. Therefore, it can process high-concentration brine for a long time and maintain a stable and efficient evaporation rate. Ultimately, it can efficiently and stably collect fresh water / salt at the same time and achieve zero liquid discharge.

[0006] For example, patent application CN115746383B discloses a composite membrane material, its preparation method, and a solar evaporator. The composite membrane material comprises a water transport layer and a light-absorbing layer from bottom to top. The light-absorbing layer is attached to one side of the water transport layer. The water transport layer has a first pore structure, and the light-absorbing layer has a second pore structure. The first and second pore structures are interconnected, and the pore size of the first pore structure is larger than that of the second pore structure. The first pore structure of the water transport layer and the second pore structure of the light-absorbing layer form a gradient-decreasing hierarchical pore structure, exhibiting strong capillary action, which is beneficial for improving the water transport capacity of the composite membrane material. The second pore structure of the light-absorbing layer, acting as a water channel, increases the contact area between seawater and the light-absorbing layer, enhancing heat exchange and improving the energy utilization rate of photothermal conversion. Furthermore, the second pore structure of the light-absorbing layer can also serve as a salt ion exchange channel in seawater, allowing the high concentration of salt after water evaporation to be rapidly diluted within the pores of the second pore structure, alleviating the salt crystallization problem at the evaporation interface.

[0007] However, the aerogel system in patent application CN116474667A is difficult to effectively restrict the transfer of salt ions when evaporating brine, which makes it easy for salt to crystallize and precipitate on the surface of the evaporator and accumulate on the evaporation interface; although the composite membrane material in patent application CN115746383B can alleviate the salt crystallization problem at the evaporation interface to a certain extent, its effect is still relatively limited. Summary of the Invention

[0008] The purpose of this invention is to solve the problems existing in the prior art and to provide a hydrogel evaporator with a hierarchical gradient structure, its preparation method and application.

[0009] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0010] A hydrogel evaporator with a hierarchical gradient structure has a composite layer structure, including an adjacent upper layer and a lower layer, both of which have a three-dimensional porous network structure; the pore size of all pores in the upper layer ranges from 1 to 20 μm, and the average pore size of the upper layer is 4 to 6 μm; in the lower layer, a portion of the pores have a pore size range of 1 to 20 μm, another portion have a pore size range of 70 to 90 μm, and the average pore size of the lower layer is 14 to 17 μm, and all the pores in the lower layer are interconnected.

[0011] The hydrogel evaporator of the present invention has a smaller average pore size in the upper layer and a larger average pore size in the lower layer. The hierarchical gradient structure between the upper and lower layers enhances capillary action, achieving a faster water transport rate, so that water can be transported to the interface of the evaporator for evaporation in a timely manner.

[0012] While existing evaporators possess a graded gradient structure, they differ from the graded gradient structure of this invention. Existing technologies have relatively uniform pore sizes in both the upper and lower layers, whereas this invention features a relatively uniform upper pore size but a non-uniform lower layer with a two-stage pore structure. This results in the evaporator of this invention, with its graded gradient structure, being more effective than existing graded gradient evaporators in limiting salt ion transfer and reducing salt accumulation during brine evaporation. This is because the lower layer of this invention has two stages of pores (small pores with a pore size range of 1–20 μm + pores with a pore size range of…). The structure has macropores (70-90 μm). The macropores allow brine to flow freely through, while the micropores restrict the transfer of salt ions. When brine enters the macropores, the salt ions diffuse within the channels. Then, when brine flows through the micropores, the salt ions cannot or have difficulty passing through due to the smaller channel size. This causes salt reflux, which promptly returns the brine to the water body and prevents salt from crystallizing and precipitating on the surface of the evaporator, thus reducing salt accumulation. At the same time, because all the pores in the lower layer are interpenetrating and interconnected, brine and salt can flow and exchange effectively within the structure, thereby improving the salt exchange efficiency.

[0013] Furthermore, existing evaporators with graded gradient structures are mostly aerogel systems, while the evaporator with graded gradient structures of the present invention is a hydrogel system. Hydrogel systems have excellent hydrophilicity, which can provide a faster water transport rate and fully pump water to the evaporation interface for evaporation, greatly improving evaporation efficiency. This is a significant advantage compared to aerogel systems or other membrane materials.

[0014] As a preferred technical solution:

[0015] As described above, a hydrogel evaporator with a hierarchical gradient structure has an upper and lower three-dimensional porous network framework constructed from nanocellulose and polyvinyl alcohol. The nanocellulose contains a large number of hydroxyl groups, which enhances the hydrophilicity and mechanical properties of the hydrogel. At the same time, the significant increase in hydroxyl groups changes the state distribution of water in the hydrogel, increasing the proportion of "intermediate water," reducing the enthalpy of vaporization of water in the hydrogel, and increasing the evaporation rate and energy utilization efficiency of the evaporator, thus solving the problem of low evaporation rate in the prior art. The upper layer contains 0.5-1 wt% carbon nanotubes. Due to their broad light absorption spectrum, the different pore sizes of the upper and lower layers of the hydrogel evaporator of this invention also enhance capillary action, improve water transport rate, and enhance its salt resistance, making it effectively applicable to seawater desalination and wastewater treatment in dyeing and printing plants.

[0016] As described above, a hydrogel evaporator with a hierarchical gradient structure is prepared by TEMPO oxidation of nanocellulose, the length of which is 0.5-1.5 μm, and the carbon nanotubes are carboxylated multi-walled carbon nanotubes.

[0017] As described above, a hydrogel evaporator with a graded gradient structure has an upper layer with a porosity of 65-70% and a lower layer with a porosity of 75-85%.

[0018] As described above, a hydrogel evaporator with a graded gradient structure has an upper layer thickness of 3-4 mm and a lower layer thickness of 9-10 mm.

[0019] As described above, a hydrogel evaporator with a graded gradient structure exhibits an absorbance of 96.8%–97.1% in the 250–2500 nm spectral range, and under one solar load (1 kW / m²), [the absorbance is achieved]. 2 The evaporation rate of deionized water is 2.42–2.52 kg / m³. -2 h -1 During the continuous evaporation of brine (10wt% NaCl solution) for 8 hours, there was virtually no significant salt accumulation on the surface of the hydrogel evaporator.

[0020] The present invention also provides a method for preparing a hydrogel evaporator with a graded gradient structure as described in any of the preceding claims. A uniform dispersion I containing nanocellulose, polyvinyl alcohol, polyethylene glycol (molecular weight 6000), and deionized water is poured into a template and frozen. A uniform dispersion II containing nanocellulose, polyvinyl alcohol, deionized water, and carbon nanotubes is then poured into the template. A sandpaper sheet (36 mesh) of the same size as the template is placed on the surface of the uniform dispersion II and frozen. The mixture is then thawed. This freezing-thawing process is repeated. After washing to remove polyethylene glycol (soaking in deionized water for 12 hours, repeated 2-3 times), a hydrogel evaporator with a graded gradient structure is obtained.

[0021] Freeze-thaw cycle (FCR) is a method for preparing hydrogels. It forms strong hydrogen bonds between polymer chains through repeated freezing and thawing processes. This method helps to form a uniform three-dimensional network structure of hydrogels, thereby improving the performance and stability of hydrogels.

[0022] In uniform dispersion I, the content of nanocellulose is 0.25-0.35 wt%, the content of polyvinyl alcohol is 5-7 wt%, and the content of polyethylene glycol is 2-3 wt%. Polyvinyl glycol acts as a pore-forming agent to construct macropores, while nanocellulose and polyvinyl alcohol are used to construct micropores.

[0023] In the uniform dispersion II, the content of nanocellulose is 0.3-0.4 wt%, the content of polyvinyl alcohol is 6-8 wt%, and the content of carbon nanotubes is 0.5-1 wt%.

[0024] The freezing-thawing process is repeated 3 to 5 times, with each freezing time ranging from 14 to 16 hours and each thawing time ranging from 6 to 8 hours.

[0025] The present invention can control the above parameters to adjust the pore size and porosity of the upper and lower layers of a hydrogel evaporator with a hierarchical gradient structure.

[0026] The raw materials used in the preparation of the hydrogel evaporator with a hierarchical gradient structure in this invention (such as polyvinyl alcohol, polyethylene glycol, carbon nanotubes, nanocellulose, etc.) are all non-toxic or low-toxic environmentally friendly substances, and are green, biodegradable and biocompatible, which solves the problem that existing technologies will harm the environment due to the addition of a lot of toxic reagents.

[0027] As a preferred technical solution:

[0028] As described above, the preparation process of uniform dispersion I is as follows: nanocellulose and polyvinyl alcohol are added to deionized water and heated and stirred. Then, polyethylene glycol is added and stirred until completely dissolved and uniformly dispersed in the solution. After cooling to room temperature, ultrasonic dispersion is performed to obtain uniform dispersion I.

[0029] As described above, the preparation process of uniform dispersion II is as follows: nanocellulose and polyvinyl alcohol are added to deionized water and heated and stirred. Then, carbon nanotube dispersion is added to it, and heating, stirring and ultrasonic dispersion are performed in sequence to obtain uniform dispersion II.

[0030] As described above, all freezing temperatures are within the range of -20 to -40°C.

[0031] An application of a hydrogel evaporator with a graded gradient structure as described in the preceding item, for seawater desalination or wastewater treatment in printing and dyeing plants.

[0032] Beneficial effects:

[0033] (1) The hydrogel evaporator with a graded gradient structure of the present invention has a smaller average pore size in the upper layer and a larger average pore size in the lower layer. The graded gradient structure of the upper and lower layers enhances the capillary effect and achieves a faster water transport rate, so that water can be transported to the interface of the evaporator in a timely manner for evaporation.

[0034] (2) The lower layer of the hydrogel evaporator with a graded gradient structure of the present invention has a unique secondary pore structure, which can effectively limit the transfer of salt ions during the evaporation of brine, reduce the accumulation of salt, and achieve a good salt rejection effect.

[0035] (3) The evaporator with a graded gradient structure of the present invention is a hydrogel system. The hydrogel system has excellent hydrophilicity, which can provide a faster water transport rate and fully pump water to the evaporation interface for evaporation, thus greatly improving the evaporation efficiency.

[0036] (4) The present invention uses the freeze-thaw cycle method to prepare a hydrogel evaporator with a graded gradient structure. Simply pour the prepared uniform dispersion into the mold and freeze it, then thaw it as a whole, and repeat the above freeze-thaw process. After washing to remove the polyethylene glycol, the hydrogel evaporator with a graded gradient structure can be obtained. The operation is simple.

[0037] (5) The raw materials such as nanocellulose and polyethylene glycol used in this invention are non-toxic, biodegradable, cheap and readily available, have no harm to the environment, are green and environmentally friendly, and have low cost.

[0038] (6) The hydrogel evaporator with a graded gradient structure of the present invention has excellent purification performance for seawater and dye wastewater. Attached Figure Description

[0039] Figure 1 The flowchart shows the preparation of a hydrogel evaporator with a hierarchical gradient structure according to the present invention; in the figure, CNT is carbon nanotube, PEG is polyethylene glycol, CNF is cellulose nanofiber, and PVA is polyvinyl alcohol.

[0040] Figure 2 This is a photograph of the hydrogel evaporator with a graded gradient structure prepared in Example 1 of the present invention.

[0041] Figure 3 The images shown are scanning electron microscope (SEM) images of the hydrogel evaporator with a hierarchical gradient structure prepared in Example 1 of the present invention; wherein, a is an SEM image of the upper layer of the hydrogel evaporator with a hierarchical gradient structure, and b is an SEM image of the lower layer of the hydrogel evaporator with a hierarchical gradient structure.

[0042] Figure 4 The solar absorption spectra of the hydrogel evaporators with hierarchical gradient structures prepared in Examples 1, 2, and 4 of this invention are shown.

[0043] Figure 5 The figures show the evaporation rates of the hydrogel evaporators with graded gradient structures prepared in Examples 1-6 of this invention; in the figures, pure water refers to pure water without the use of a hydrogel evaporator under one sun (1kW / m²). 2 ) evaporation rate;

[0044] Figure 6 The figure shows a comparison of the evaporation rates of the hydrogel evaporator with a graded gradient structure prepared in Example 2 of the present invention and the hydrogel evaporator without a graded conventional pore structure prepared in Comparative Example 2. As can be seen from the figure, the evaporation rate of the hydrogel evaporator with the graded gradient pore structure is significantly improved.

[0045] Figure 7 Figure a shows the salt rejection effect of the hydrogel evaporator with a graded gradient structure prepared in Example 3 of the present invention and the hydrogel evaporator without a graded conventional pore structure prepared in Comparative Example 2; Figure b shows the salt rejection effect of the hydrogel evaporator with a graded gradient structure prepared in Example 3 of the present invention.

[0046] Figure 8 This is a graph showing the evaporation rate of the hydrogel evaporator with a graded gradient structure prepared in Example 4 of the present invention at different salt concentrations.

[0047] Figure 9 A comparison of the concentrations of various ions after seawater desalination using the hydrogel evaporator with a graded gradient structure prepared in Example 6 of this invention.

[0048] Figure 10 The figures show the UV absorption spectra of the hydrogel evaporator with a graded gradient structure prepared in Example 6 of this invention before and after treatment with two dye solutions. In the figures, 1 and 2 are the UV absorption spectra of Rhodamine B (RhB) dye solution before and after purification using the hydrogel evaporator with a graded gradient structure prepared in Example 6, and 3 and 4 are the UV absorption spectra of methylene blue (MB) dye solution before and after purification using the hydrogel evaporator with a graded gradient structure prepared in Example 6. Detailed Implementation

[0049] The present invention will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0050] The test methods for the relevant performance indicators in the following embodiments and comparative examples are as follows:

[0051] Light absorption rate: First, the hydrogel samples prepared in each example were used to control the sample size to cylinders with a thickness of 12-14 mm and a diameter of 33-35 mm using templates such as cell culture plates. Then, the transmittance (T) and reflectance (R) of the samples in the spectral range of 250-2500 nm were tested using an integrating sphere spectrometer UV3600 from Shimadzu Corporation of Japan in the integrating sphere mode. The slit width was 2 cm and the scanning speed was medium. The light absorption rate A was evaluated according to the formula A = 1 - TR.

[0052] Evaporation rate: An incident light source (simulated light source from Beijing CCCC Jinyuan Technology Co., Ltd.) was used, and the light intensity of the light source was adjusted using a light intensity meter (manufacturer: Soleb Optoelectronics Technology Co., Ltd., model PM100D) to achieve a light intensity of 1 kW / m² at the evaporation interface of the hydrogel evaporator. 2 Add 230 mL of deionized water or NaCl solutions of different concentrations (3.5 wt%, 7 wt%, 10 wt%, or 15 wt%) to a 250 mL beaker. Wrap the beaker with polystyrene foam (PS foam) to prevent localized heat dissipation. Then, place a hydrogel evaporator with a diameter of 22-25 mm and a thickness of 12-14 mm as the sample on the water surface. The entire beaker containing the solution and the hydrogel evaporator is then placed directly below a simulated light source. Photovaporization is carried out at 25°C and 60% relative humidity for 60 minutes. During this period, the real-time weight change of the solution is monitored using an electronic balance (model ME204), and the surface temperature of the hydrogel sample is recorded using an infrared thermal imaging camera (model T630sc) and a thermocouple (model HH506RA). The water evaporation rate (i.e., the rate of change under small time and small mass changes) v of the photothermal hydrogel sample can be calculated by the following formula:

[0053] v = dm / (S×dt);

[0054] In the formula, d represents a small change, m is the mass of liquid lost during photoevaporation (kg), t is the illumination time (h), and S is the surface area of ​​the hydrogel evaporator (m²). 2 ).

[0055] Seawater desalination: The concentrations of relevant ions in raw seawater and desalinated water were detected using a Prodigy-ICP spectrometer from Teledyne Leeman, USA.

[0056] Dye liquor purification: Using a Shimadzu UV2600 UV-Vis-NIR spectrometer, samples of dye liquor before and after treatment were poured into cuvettes and placed in the instrument for testing. The absorbance of the samples in the spectral range of 400-800 nm was measured.

[0057] Example 1

[0058] A method for preparing a hydrogel evaporator with a hierarchical gradient structure, such as Figure 1 As shown, the specific steps are as follows:

[0059] (1) Preparation of raw materials;

[0060] Nanocellulose: prepared by TEMPO oxidation, with a length of 0.5–1.5 μm;

[0061] Polyvinyl alcohol: Manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., CAS number is 9002-89-5, product specification is: 1750±50 type;

[0062] Deionized water;

[0063] Polyethylene glycol: molecular weight 6000;

[0064] Carbon nanotubes: Carboxylated multi-walled carbon nanotubes, manufactured by Shanghai Maclean Biochemical Technology Co., Ltd., CAS number 308068-56-6, product number C835711;

[0065] Sandpaper: 36 mesh;

[0066] (2) Prepare a uniform dispersion I;

[0067] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Polyethylene glycol was then added and stirring was continued for 1 hour until completely dissolved. The mixture was then cooled to 25°C and ultrasonically dispersed for 30 minutes to obtain a uniform dispersion I. The contents of nanocellulose were 0.25 wt%, polyvinyl alcohol was 5 wt%, and polyethylene glycol was 2 wt%.

[0068] (3) Preparation of carbon nanotube dispersion;

[0069] Carbon nanotubes were added to deionized water and dispersed using a high-speed homogenizer at 10,000 rpm for 20 minutes to achieve uniform dispersion, resulting in a carbon nanotube dispersion with a carbon nanotube content of 0.5 wt%.

[0070] (4) Prepare uniform dispersion II;

[0071] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Then, the carbon nanotube dispersion obtained in step (3) was added to it, and the mixture was heated and stirred until uniformly dispersed. After cooling to 25°C, it was ultrasonically treated for 30 minutes to obtain uniform dispersion II. The content of nanocellulose was 0.3 wt%, the content of polyvinyl alcohol was 6 wt%, and the content of carbon nanotubes was 0.5 wt%.

[0072] (5) Prepare a hydrogel evaporator with a hierarchical gradient structure;

[0073] (5.1) Pour the uniform dispersion I obtained in step (2) into the template and freeze it at -30℃ for 1 hour. Then pour the uniform dispersion II obtained in step (4) into the template. Place the sandpaper with the sandpaper of the same size as the template on the surface of the uniform dispersion II and freeze it at -20℃ for 14 hours. Then thaw it as a whole for 8 hours. Repeat the above freezing-thawing process. The freezing-thawing process is carried out 3 times in total.

[0074] (5.2) After the freeze-thaw cycle in step (5.1), the entire template is immersed in deionized water for 12 hours. The water is changed and the immersion is repeated twice to remove the polyethylene glycol, thus obtaining a hydrogel evaporator with a graded gradient structure.

[0075] The final hydrogel evaporator with a hierarchical gradient structure is as follows: Figure 2 As shown, it has a composite layer structure, consisting of an upper layer with a thickness of 3 mm and a lower layer with a thickness of 9 mm. Both the upper and lower layers have a three-dimensional porous network structure. The porosity of the upper layer is 68%, with all pores having a diameter range of 1-20 μm, and the average pore diameter of the upper layer is 4 μm. The porosity of the lower layer is 75%, with some pores having a diameter range of 1-20 μm and others having a diameter range of 70-90 μm, and the average pore diameter of the lower layer is 14 μm. All pores in the lower layer are interconnected and interpenetrating. Figure 3 As shown, the difference in pore size between the upper and lower layers forms a gradient pore structure in the hydrogel;

[0076] like Figure 4 , Figure 5 As shown, the hydrogel evaporator with a hierarchical gradient structure exhibits an absorbance of 97.1% in the 250–2500 nm spectral range, and under one solar load (1 kW / m²), it achieves an absorbance of 97.1%. 2 The evaporation rate of deionized water is 2.51 kg m³. -2 h -1 Without using a hydrogel evaporator with a graded gradient structure, the evaporation rate of pure water is 0.38 kg m³. -2 h -1 During the continuous 8-hour evaporation of brine (10wt% NaCl solution) by the hydrogel evaporator with a graded gradient structure, there was virtually no significant salt accumulation on the surface of the hydrogel evaporator.

[0077] The hydrogel evaporator with a graded gradient structure prepared above can be used for seawater desalination or wastewater treatment in printing and dyeing plants.

[0078] Comparative Example 1

[0079] A method for preparing a hydrogel evaporator is basically the same as in Example 1, except that in step (2), when preparing the uniform dispersion I, nanocellulose is replaced with an equal mass of deionized water (same as in Example 1).

[0080] The structure of the final hydrogel evaporator is basically the same as that in Example 1, except that the pore size of all the pores in the lower layer ranges from 40 to 70 μm, the average pore size is 57 μm, and the porosity of the lower layer is 73%.

[0081] During the continuous evaporation of brine (10wt% NaCl solution) for 8 hours, significant salt accumulation was observed on the surface of the hydrogel evaporator.

[0082] Comparing Comparative Example 1 and Example 1, it can be seen that the lack of secondary pores in the lower layer of the hydrogel evaporator prepared in Comparative Example 1 leads to the absence of salt exchange channels, and salt gradually accumulates in the pores of the hydrogel evaporator as evaporation proceeds.

[0083] Example 2

[0084] A method for preparing a hydrogel evaporator with a hierarchical gradient structure, comprising the following specific steps:

[0085] (1) Preparation of raw materials;

[0086] Nanocellulose: prepared by TEMPO oxidation, with a length of 0.5–1.5 μm;

[0087] Polyvinyl alcohol: Manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., CAS number is 9002-89-5, product specification is: 1750±50 type;

[0088] Deionized water;

[0089] Polyethylene glycol: molecular weight 6000;

[0090] Carbon nanotubes: Carboxylated multi-walled carbon nanotubes, manufactured by Shanghai Maclean Biochemical Technology Co., Ltd., CAS number 308068-56-6, product number C835711;

[0091] Sandpaper: 36 mesh;

[0092] (2) Prepare a uniform dispersion I;

[0093] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Polyethylene glycol was then added and stirring was continued for another 2 hours until completely dissolved. The mixture was then cooled to 25°C and ultrasonically dispersed for 30 minutes to obtain a uniform dispersion I. The content of nanocellulose was 0.25 wt%, polyvinyl alcohol was 5 wt%, and polyethylene glycol was 2.5 wt%.

[0094] (3) Preparation of carbon nanotube dispersion;

[0095] Carbon nanotubes were added to deionized water and dispersed using a high-speed homogenizer at 10,000 rpm for 20 minutes to achieve uniform dispersion, resulting in a carbon nanotube dispersion with a carbon nanotube content of 0.75 wt%.

[0096] (4) Prepare uniform dispersion II;

[0097] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Then, the carbon nanotube dispersion obtained in step (3) was added to it, and the mixture was heated and stirred until uniformly dispersed. After cooling to 25°C, it was ultrasonically treated for 30 minutes to obtain uniform dispersion II. The content of nanocellulose was 0.4 wt%, the content of polyvinyl alcohol was 8 wt%, and the content of carbon nanotubes was 0.75 wt%.

[0098] (5) Prepare a hydrogel evaporator with a hierarchical gradient structure;

[0099] (5.1) Pour the uniform dispersion I obtained in step (2) into the template and freeze it at -30℃ for 2 hours. Then pour the uniform dispersion II obtained in step (4) into the template. Place the sandpaper with the sandpaper of the same size as the template on the surface of the uniform dispersion II and freeze it at -30℃ for 16 hours. Then thaw it as a whole for 8 hours. Repeat the above freezing-thawing process. The freezing-thawing process is carried out 5 times in total.

[0100] (5.2) After the freeze-thaw cycle in step (5.1), the entire template is immersed in deionized water for 12 hours. The water is changed and the immersion is repeated twice to remove the polyethylene glycol, thus obtaining a hydrogel evaporator with a graded gradient structure.

[0101] The resulting hydrogel evaporator with a hierarchical gradient structure has a composite layer structure, consisting of an upper layer with a thickness of 4 mm and a lower layer with a thickness of 9 mm. Both the upper and lower layers have a three-dimensional porous network structure. The porosity of the upper layer is 65%, with all pores ranging from 1 to 20 μm in diameter, and the average pore diameter of the upper layer is 4.8 μm. The porosity of the lower layer is 82%, with some pores ranging from 1 to 20 μm in diameter and others ranging from 70 to 90 μm in diameter, and the average pore diameter of the lower layer is 16.7 μm. All pores in the lower layer are interconnected.

[0102] like Figure 4 , Figure 5 As shown, the hydrogel evaporator with a hierarchical gradient structure has an absorbance of 96.8% in the spectral range of 250–2500 nm. Figure 6 As shown, under a sun (1kW / m²) 2 The evaporation rate of deionized water is 2.52 kg m³. - 2 h -1 During the continuous evaporation of brine (10wt% NaCl solution) for 8 hours, there was virtually no significant salt accumulation on the surface of the hydrogel evaporator.

[0103] The hydrogel evaporator with a graded gradient structure prepared above can be used for seawater desalination or wastewater treatment in printing and dyeing plants.

[0104] Comparative Example 2

[0105] A method for preparing a hydrogel evaporator with a non-hierarchical conventional pore structure is basically the same as in Example 2, except that in step (2), when preparing the uniform dispersion I, polyethylene glycol is replaced with an equal mass of deionized water (same as in Example 2).

[0106] The structure of the hydrogel evaporator with non-hierarchical conventional pore structure obtained in the end is basically the same as that in Example 2, except that: the pore size of all pores in the upper and lower layers ranges from 1 to 20 μm, the average pore size is 4 to 6 μm, the porosity of the upper layer is 70%, and the porosity of the lower layer is 70%.

[0107] like Figure 6 As shown, a hydrogel evaporator without hierarchical conventional pore structure under one sun (1kW / m²) 2 The evaporation rate of deionized water is 2.01 kg m³. -2 h -1 During the continuous evaporation of brine (10wt% NaCl solution) for 8 hours, significant salt accumulation was observed on the surface of the hydrogel evaporator, such as... Figure 7 As shown in (b).

[0108] Comparing Comparative Example 2 and Example 2, it can be seen that since polyethylene glycol was not added when preparing the uniform dispersion I in Comparative Example 2, the pore size distribution of the lower hydrogel is consistent with that of the upper layer. This results in the absence of a hierarchical gradient pore structure between the upper and lower hydrogels, leading to a reduction in the water transport capacity and salt rejection effect of the hydrogel evaporator. This is because polyethylene glycol acts as a pore-forming agent in the preparation of the lower hydrogel. If polyethylene glycol is not added during the preparation of the lower hydrogel, the resulting lower hydrogel will only have a small pore structure composed of nanocellulose and polyvinyl alcohol.

[0109] Example 3

[0110] A method for preparing a hydrogel evaporator with a hierarchical gradient structure, comprising the following specific steps:

[0111] (1) Preparation of raw materials;

[0112] Nanocellulose: prepared by TEMPO oxidation, with a length of 0.5–1.5 μm;

[0113] Polyvinyl alcohol: Manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., CAS number is 9002-89-5, product specification is: 1750±50 type;

[0114] Deionized water;

[0115] Polyethylene glycol: molecular weight 6000;

[0116] Carbon nanotubes: Carboxylated multi-walled carbon nanotubes, manufactured by Shanghai Maclean Biochemical Technology Co., Ltd., CAS number 308068-56-6, product number C835711;

[0117] Sandpaper: 36 mesh;

[0118] (2) Prepare a uniform dispersion I;

[0119] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Polyethylene glycol was then added and stirring was continued for 1.5 hours until completely dissolved. The mixture was then cooled to 25°C and ultrasonically dispersed for 30 minutes to obtain a uniform dispersion I. The contents of nanocellulose were 0.3 wt%, polyvinyl alcohol was 6 wt%, and polyethylene glycol was 2.5 wt%.

[0120] (3) Preparation of carbon nanotube dispersion;

[0121] Carbon nanotubes were added to deionized water and dispersed using a high-speed homogenizer at 10,000 rpm for 40 minutes to achieve uniform dispersion, resulting in a carbon nanotube dispersion with a carbon nanotube content of 0.75 wt%.

[0122] (4) Prepare uniform dispersion II;

[0123] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Then, the carbon nanotube dispersion obtained in step (3) was added to it, and the mixture was heated and stirred until uniformly dispersed. After cooling to 25°C, it was ultrasonically treated for 30 minutes to obtain uniform dispersion II. The content of nanocellulose was 0.4 wt%, the content of polyvinyl alcohol was 8 wt%, and the content of carbon nanotubes was 0.75 wt%.

[0124] (5) Prepare a hydrogel evaporator with a hierarchical gradient structure;

[0125] (5.1) Pour the uniform dispersion I obtained in step (2) into the template and freeze it at -30℃ for 1.5h. Then pour the uniform dispersion II obtained in step (4) into the template. Place the sandpaper with the sandpaper of the same size as the template on the surface of the uniform dispersion II and freeze it at -30℃ for 16h. Then thaw it as a whole for 6h. Repeat the above freezing-thawing process. The freezing-thawing process is carried out 5 times in total.

[0126] (5.2) After the freeze-thaw cycle in step (5.1), the entire template is immersed in deionized water for 12 hours. The water is changed and the immersion is repeated 3 times to remove the polyethylene glycol, thus obtaining a hydrogel evaporator with a graded gradient structure.

[0127] The resulting hydrogel evaporator with a hierarchical gradient structure has a composite layer structure, consisting of an upper layer with a thickness of 3 mm and a lower layer with a thickness of 10 mm. Both the upper and lower layers have a three-dimensional porous network structure. The porosity of the upper layer is 70%, with all pores having a diameter range of 1-20 μm and an average pore diameter of 5.2 μm. The porosity of the lower layer is 79%, with some pores having a diameter range of 1-20 μm and others having a diameter range of 70-90 μm and an average pore diameter of 15 μm. All pores in the lower layer are interconnected.

[0128] like Figure 5 As shown, the hydrogel evaporator with a hierarchical gradient structure has an absorbance of 96.8% in the 250–2500 nm spectral range, and under one sun (1 kW / m²), it achieves an absorbance of 96.8%. 2 The evaporation rate of deionized water is 2.48 kg m³. -2 h -1 During the continuous evaporation of brine (10wt% NaCl solution) for 8 hours, there was virtually no significant salt accumulation on the surface of the hydrogel evaporator. Figure 7 As shown in (a).

[0129] The hydrogel evaporator with a graded gradient structure prepared above can be used for seawater desalination or wastewater treatment in printing and dyeing plants.

[0130] Example 4

[0131] A method for preparing a hydrogel evaporator with a hierarchical gradient structure, comprising the following specific steps:

[0132] (1) Preparation of raw materials;

[0133] Nanocellulose: prepared by TEMPO oxidation, with a length of 0.5–1.5 μm;

[0134] Polyvinyl alcohol: Manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., CAS number is 9002-89-5, product specification is: 1750±50 type;

[0135] Deionized water;

[0136] Polyethylene glycol: molecular weight 6000;

[0137] Carbon nanotubes: Carboxylated multi-walled carbon nanotubes, manufactured by Shanghai Maclean Biochemical Technology Co., Ltd., CAS number 308068-56-6, product number C835711;

[0138] Sandpaper: 36 mesh;

[0139] (2) Prepare a uniform dispersion I;

[0140] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Polyethylene glycol was then added and stirring was continued for 1 hour until completely dissolved. The mixture was then cooled to 25°C and ultrasonically dispersed for 30 minutes to obtain a uniform dispersion I. The content of nanocellulose was 0.35 wt%, polyvinyl alcohol was 7 wt%, and polyethylene glycol was 2 wt%.

[0141] (3) Preparation of carbon nanotube dispersion;

[0142] Carbon nanotubes were added to deionized water and dispersed using a high-speed homogenizer at 10,000 rpm for 30 minutes to achieve uniform dispersion, resulting in a carbon nanotube dispersion with a carbon nanotube content of 1 wt%.

[0143] (4) Prepare uniform dispersion II;

[0144] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Then, the carbon nanotube dispersion obtained in step (3) was added to it, and the mixture was heated and stirred until uniformly dispersed. After cooling to 25°C, it was ultrasonically treated for 30 minutes to obtain uniform dispersion II. The content of nanocellulose was 0.35 wt%, the content of polyvinyl alcohol was 7 wt%, and the content of carbon nanotubes was 1 wt%.

[0145] (5) Prepare a hydrogel evaporator with a hierarchical gradient structure;

[0146] (5.1) Pour the uniform dispersion I obtained in step (2) into the template and freeze it at -30℃ for 1 hour. Then pour the uniform dispersion II obtained in step (4) into the template. Place the sandpaper with the sandpaper of the same size as the template on the surface of the uniform dispersion II and freeze it at -40℃ for 15 hours. Then thaw it as a whole for 7 hours. Repeat the above freezing-thawing process. The freezing-thawing process is carried out 3 times in total.

[0147] (5.2) After the freeze-thaw cycle in step (5.1), the entire template is immersed in deionized water for 12 hours. The water is changed and the immersion is repeated 3 times to remove the polyethylene glycol, thus obtaining a hydrogel evaporator with a graded gradient structure.

[0148] The resulting hydrogel evaporator with a hierarchical gradient structure has a composite layer structure, consisting of an upper layer with a thickness of 3 mm and a lower layer with a thickness of 10 mm. Both the upper and lower layers have a three-dimensional porous network structure. The porosity of the upper layer is 65%, with all pores ranging from 1 to 20 μm in diameter, and the average pore diameter of the upper layer is 5.7 μm. The porosity of the lower layer is 85%, with some pores ranging from 1 to 20 μm in diameter and others ranging from 70 to 90 μm in diameter, and the average pore diameter of the lower layer is 15.5 μm. All pores in the lower layer are interconnected.

[0149] like Figure 4 , Figure 5 As shown, the hydrogel evaporator with a graded gradient structure exhibits an absorbance of 97.1% in the 250–2500 nm spectral range. During continuous 8-hour evaporation of brine (10 wt% NaCl solution), there was virtually no significant salt accumulation on the surface of the hydrogel evaporator. Figure 8 As shown, under a sun (1kW / m²) 2 The evaporation rate of deionized water is 2.47 kg m³. -2 h -1 Under a sun (1kW / m 2The evaporation rate of brine (3.5 wt% NaCl solution) is 2.48 kg / m³. -2 h -1 Under a sun (1kW / m 2 The evaporation rate of brine (7 wt% NaCl solution) is 2.45 kg / m³. -2 h -1 Under a sun (1kW / m 2 The evaporation rate of brine (10 wt% NaCl solution) is 2.42 kg / m³. -2 h -1 Under a sun (1kW / m 2 The evaporation rate of brine (15 wt% NaCl solution) is 2.41 kg m³. -2 h -1 The data from the above tests show that as the salt concentration increases, the evaporation rate of the hydrogel evaporator shows almost no decreasing trend, and is not much different from the evaporation rate in pure water, demonstrating an excellent salt-repellent effect.

[0150] The hydrogel evaporator with a graded gradient structure prepared above can be used for seawater desalination or wastewater treatment in printing and dyeing plants.

[0151] Example 5

[0152] A method for preparing a hydrogel evaporator with a hierarchical gradient structure, comprising the following specific steps:

[0153] (1) Preparation of raw materials;

[0154] Nanocellulose: prepared by TEMPO oxidation, with a length of 0.5–1.5 μm;

[0155] Polyvinyl alcohol: Manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., CAS number is 9002-89-5, product specification is: 1750±50 type;

[0156] Deionized water;

[0157] Polyethylene glycol: molecular weight 6000;

[0158] Carbon nanotubes: Carboxylated multi-walled carbon nanotubes, manufactured by Shanghai Maclean Biochemical Technology Co., Ltd., CAS number 308068-56-6, product number C835711;

[0159] Sandpaper: 36 mesh;

[0160] (2) Prepare a uniform dispersion I;

[0161] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Polyethylene glycol was then added and stirring was continued for another 2 hours until completely dissolved. The mixture was then cooled to 25°C and ultrasonically dispersed for 30 minutes to obtain a uniform dispersion I. The contents of nanocellulose were 0.35 wt%, polyvinyl alcohol was 7 wt%, and polyethylene glycol was 3 wt%.

[0162] (3) Preparation of carbon nanotube dispersion;

[0163] Carbon nanotubes were added to deionized water and dispersed using a high-speed homogenizer at 10,000 rpm for 40 minutes to achieve uniform dispersion, resulting in a carbon nanotube dispersion with a carbon nanotube content of 0.5 wt%.

[0164] (4) Prepare uniform dispersion II;

[0165] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Then, the carbon nanotube dispersion obtained in step (3) was added to it, and the mixture was heated and stirred until uniformly dispersed. After cooling to 25°C, it was ultrasonically treated for 30 minutes to obtain uniform dispersion II. The content of nanocellulose was 0.35 wt%, the content of polyvinyl alcohol was 7 wt%, and the content of carbon nanotubes was 0.5 wt%.

[0166] (5) Prepare a hydrogel evaporator with a hierarchical gradient structure;

[0167] (5.1) Pour the uniform dispersion I obtained in step (2) into the template and freeze it at -30℃ for 2 hours. Then pour the uniform dispersion II obtained in step (4) into the template. Place the sandpaper with the sandpaper of the same size as the template on the surface of the uniform dispersion II and freeze it at -20℃ for 14 hours. Then thaw it as a whole for 7 hours. Repeat the above freezing-thawing process. The freezing-thawing process is carried out 4 times in total.

[0168] (5.2) After the freeze-thaw cycle in step (5.1), the entire template is immersed in deionized water for 12 hours. The water is changed and the immersion is repeated twice to remove the polyethylene glycol, thus obtaining a hydrogel evaporator with a graded gradient structure.

[0169] The resulting hydrogel evaporator with a hierarchical gradient structure has a composite layer structure, consisting of an upper layer with a thickness of 4 mm and a lower layer with a thickness of 9 mm. Both the upper and lower layers have a three-dimensional porous network structure. The porosity of the upper layer is 66%, with all pores ranging from 1 to 20 μm in diameter, and the average pore diameter of the upper layer is 5.3 μm. The porosity of the lower layer is 77%, with some pores ranging from 1 to 20 μm in diameter and others ranging from 70 to 90 μm in diameter, and the average pore diameter of the lower layer is 17 μm. All pores in the lower layer are interconnected.

[0170] like Figure 5 As shown, the hydrogel evaporator with a hierarchical gradient structure exhibits an absorbance of 97% in the 250–2500 nm spectral range, and under one solar load (1 kW / m²), it achieves an absorbance of 97%. 2 The evaporation rate of deionized water is 2.42 kg m³. -2 h -1 During the continuous evaporation of brine (10wt% NaCl solution) for 8 hours, there was virtually no significant salt accumulation on the surface of the hydrogel evaporator.

[0171] The hydrogel evaporator with a graded gradient structure prepared above can be used for seawater desalination or wastewater treatment in printing and dyeing plants.

[0172] Example 6

[0173] A method for preparing a hydrogel evaporator with a hierarchical gradient structure, comprising the following specific steps:

[0174] (1) Preparation of raw materials;

[0175] Nanocellulose: prepared by TEMPO oxidation, with a length of 0.5–1.5 μm;

[0176] Polyvinyl alcohol: Manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., CAS number is 9002-89-5, product specification is: 1750±50 type;

[0177] Deionized water;

[0178] Polyethylene glycol: molecular weight 6000;

[0179] Carbon nanotubes: Carboxylated multi-walled carbon nanotubes, manufactured by Shanghai Maclean Biochemical Technology Co., Ltd., CAS number 308068-56-6, product number C835711;

[0180] Sandpaper: 36 mesh;

[0181] (2) Prepare a uniform dispersion I;

[0182] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Polyethylene glycol was then added and stirring was continued for another 2 hours until completely dissolved. The mixture was then cooled to 25°C and ultrasonically dispersed for 30 minutes to obtain a uniform dispersion I. The contents of nanocellulose were 0.3 wt%, polyvinyl alcohol was 6 wt%, and polyethylene glycol was 3 wt%.

[0183] (3) Preparation of carbon nanotube dispersion;

[0184] Carbon nanotubes were added to deionized water and dispersed using a high-speed homogenizer at 10,000 rpm for 30 minutes to achieve uniform dispersion, resulting in a carbon nanotube dispersion with a carbon nanotube content of 1 wt%.

[0185] (4) Prepare uniform dispersion II;

[0186] Nanocellulose and polyvinyl alcohol were added together to deionized water, and then placed in a constant temperature oil bath at 95°C and magnetically stirred at 1000 rpm for 2 hours until completely dissolved. Then, the carbon nanotube dispersion obtained in step (3) was added to it, and the mixture was heated and stirred until uniformly dispersed. After cooling to 25°C, it was ultrasonically treated for 30 minutes to obtain uniform dispersion II. The content of nanocellulose was 0.3 wt%, the content of polyvinyl alcohol was 6 wt%, and the content of carbon nanotubes was 1 wt%.

[0187] (5) Prepare a hydrogel evaporator with a hierarchical gradient structure;

[0188] (5.1) Pour the uniform dispersion I obtained in step (2) into the template and freeze it at -30℃ for 2 hours. Then pour the uniform dispersion II obtained in step (4) into the template. Place the sandpaper with the sandpaper of the same size as the template on the surface of the uniform dispersion II and freeze it at -40℃ for 15 hours. Then thaw it as a whole for 6 hours. Repeat the above freezing-thawing process. The freezing-thawing process is carried out 5 times in total.

[0189] (5.2) After the freeze-thaw cycle in step (5.1), the entire template is immersed in deionized water for 12 hours. The water is changed and the immersion is repeated twice to remove the polyethylene glycol, thus obtaining a hydrogel evaporator with a graded gradient structure.

[0190] The resulting hydrogel evaporator with a hierarchical gradient structure has a composite layer structure consisting of an upper layer with a thickness of 4 mm and a lower layer with a thickness of 10 mm. Both the upper and lower layers have a three-dimensional porous network structure. The porosity of the upper layer is 68%, with all pores having a diameter range of 1-20 μm and an average pore diameter of 6 μm. The porosity of the lower layer is 81%, with some pores having a diameter range of 1-20 μm and others having a diameter range of 70-90 μm. The average pore diameter of the lower layer is 14.9 μm, and all pores in the lower layer are interconnected.

[0191] like Figure 5 As shown, the hydrogel evaporator with a hierarchical gradient structure exhibits an absorbance of 97.1% in the 250–2500 nm spectral range, and under one solar load (1 kW / m²), it achieves an absorbance of 97.1%. 2 The evaporation rate of deionized water is 2.5 kg m³. -2 h -1 During the continuous evaporation of brine (10wt% NaCl solution) for 8 hours, there was virtually no significant salt accumulation on the surface of the hydrogel evaporator.

[0192] To verify the performance of the hydrogel evaporator with a graded gradient structure prepared above for seawater desalination and purification of dyeing and printing wastewater, the hydrogel evaporator with a graded gradient structure prepared above was used to desalinate seawater and purify methylene blue dye solution (concentration of 1000 ppm) and rhodamine B dye solution (concentration of 1000 ppm), respectively.

[0193] Seawater desalination: Seawater was desalinated using the hydrogel evaporator with a graded gradient structure prepared above. The changes in the concentration of metal ions in the seawater before and after treatment are as follows: Figure 9 As shown in the figure, the concentration of the four metal ions in seawater is greatly reduced, far below the WHO standard, indicating that the hydrogel evaporator with a graded gradient structure prepared above has excellent purification performance for seawater.

[0194] Purification of methylene blue and rhodamine B staining solutions: The methylene blue and rhodamine B staining solutions were purified using the hydrogel evaporator with a graded gradient structure prepared above. The UV absorption spectra before and after purification are shown below. Figure 10 As shown in the figure, the absorbance of the purified methylene blue dye solution and rhodamine B dye solution is almost zero in the wavelength range of 400 to 800 nm, which shows that the hydrogel evaporator with a hierarchical gradient structure prepared above has excellent purification performance for waste dye solutions.

Claims

1. A hydrogel evaporator with a hierarchical gradient structure, characterized in that, It has a composite layer structure, including an adjacent upper layer and a lower layer, both of which have a three-dimensional porous network structure; the pore size of all pores in the upper layer ranges from 1 to 20 μm, and the average pore size of the upper layer is 4 to 6 μm; in the lower layer, some pores have a pore size range of 1 to 20 μm, and others have a pore size range of 70 to 90 μm, with an average pore size of 14 to 17 μm, and all pores in the lower layer are interconnected; The framework of the three-dimensional porous network structure in both the upper and lower layers is constructed from nanocellulose and polyvinyl alcohol, with the upper layer containing 0.5~1wt% carbon nanotubes; Nanocellulose was prepared by TEMPO oxidation. The length of the nanocellulose was 0.5~1.5μm, and the carbon nanotubes were carboxylated carbon nanotubes.

2. The hydrogel evaporator with a graded gradient structure according to claim 1, characterized in that, The porosity of the upper layer is 65-70%, and the porosity of the lower layer is 75-85%.

3. A hydrogel evaporator with a graded gradient structure according to claim 1, characterized in that, The thickness of the upper layer is 3~4mm, and the thickness of the lower layer is 9~10mm.

4. A hydrogel evaporator with a graded gradient structure according to any one of claims 1 to 3, characterized in that, The hydrogel evaporator with a graded gradient structure exhibits an absorbance of 96.8%–97.1% in the 250–2500 nm spectral range, and its evaporation rate for deionized water under one sun is 2.42–2.52 kg m³. -2 h -1 .

5. A method for preparing a hydrogel evaporator with a hierarchical gradient structure as described in any one of claims 1 to 4, characterized in that, A uniform dispersion I containing nanocellulose, polyvinyl alcohol, polyethylene glycol, and deionized water is poured into a template and frozen. Then, a uniform dispersion II containing nanocellulose, polyvinyl alcohol, deionized water, and carbon nanotubes is poured into the template and frozen. The whole process is then thawed. The freezing-thawing process is repeated, and the polyethylene glycol is washed away to obtain a hydrogel evaporator with a hierarchical gradient structure. In uniform dispersion I, the content of nanocellulose is 0.25~0.35wt%, the content of polyvinyl alcohol is 5~7wt%, and the content of polyethylene glycol is 2~3wt%. In the uniform dispersion II, the content of nanocellulose is 0.3~0.4wt%, the content of polyvinyl alcohol is 6~8wt%, and the content of carbon nanotubes is 0.5~1wt%. The freezing-thawing process is repeated 3 to 5 times, with each freezing time ranging from 14 to 16 hours and each thawing time ranging from 6 to 8 hours.

6. The method according to claim 5, characterized in that, The preparation process of uniform dispersion I is as follows: nanocellulose and polyvinyl alcohol are added to deionized water and heated and stirred. Then polyethylene glycol is added and stirred until completely dissolved. Then ultrasonic dispersion is performed to obtain uniform dispersion I. The preparation process of uniform dispersion II is as follows: nanocellulose and polyvinyl alcohol are added to deionized water and heated and stirred. Then, carbon nanotube dispersion is added to it, and heating, stirring and ultrasonic dispersion are carried out in sequence to obtain uniform dispersion II.

7. The method according to claim 5, characterized in that, All freezing temperatures are within the range of -20 to -40°C.

8. The application of a hydrogel evaporator with a graded gradient structure as described in any one of claims 1 to 4, characterized in that, Used for seawater desalination or wastewater treatment in printing and dyeing plants.

Citation Information

Patent Citations

  • Double-layer aerogel as well as preparation method and application thereof as solar evaporator

    CN110218277A

  • Composite membrane material, preparation method thereof and solar evaporator

    CN115746383A