Erbium-ytterbium co-doped silica glass optical fiber and its preparation method

By introducing Lu3+ ions to disperse rare earth ions in ytterbium-erbium co-doped optical fibers and employing sol-liquid phase doping technology, the energy conversion efficiency problem of ytterbium-erbium co-doped optical fibers in the space environment has been solved, achieving improved efficiency and radiation resistance, making them suitable for space laser communication.

CN118290034BActive Publication Date: 2026-11-17SHANGHAI INST OF OPTICS & FINE MECHANICS CHINESE ACAD OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410416274.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2026-11-17
Estimated Expiration
2044-04-08

AI Technical Summary

Technical Problem

Existing ytterbium-erbium co-doped optical fibers suffer from color center defects due to cosmic ray radiation in the space environment, resulting in increased background loss and reduced energy conversion efficiency. Furthermore, high-concentration doping leads to rare earth ion aggregation and phosphorus volatilization, affecting fiber laser performance and energy conversion efficiency.

Method used

High-efficiency erbium-ytterbium co-doped quartz glass optical fibers were fabricated by dispersing rare earth ions with Lu3+ ions and using sol-liquid phase doping technology combined with high-temperature oxidation reaction and carbon dioxide laser processing. This ensures uniform distribution of rare earth ions and stability of phosphorus, thereby improving energy transfer efficiency.

Benefits of technology

Maintaining high fiber laser efficiency in radiation environments reduces pump power requirements, saves energy consumption, and is suitable for space applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118290034B_ABST
    Figure CN118290034B_ABST
Patent Text Reader

Abstract

This invention relates to a high-efficiency erbium-ytterbium co-doped optical fiber and its preparation method. Specifically, this invention provides a high-efficiency erbium-ytterbium co-doped silica optical fiber with a core composition ranging from: Lu₂O₃: 0.01–0.3 mol%, Yb₂O₃: 0.6–0.9 mol%, Er₂O₃: 0.03–0.1 mol%, Ce₂O₃: 0.1–0.24 mol%, P₂O₅: 8–12 mol%, GeO₂: 0.1–1 mol%, and SiO₂: 86.5–90.12 mol%. This invention also provides a method for preparing the high-efficiency erbium-ytterbium co-doped silica optical fiber. Through a two-step phosphorus doping process involving both gas-phase and sol-liquid doping, high-concentration doping of phosphorus and rare earth elements can be achieved, further improving the doping uniformity and concentration of rare earth elements. This is beneficial for improving the energy transfer efficiency from ytterbium ions to erbium ions, resulting in higher laser efficiency in the optical fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of optical fiber manufacturing, and in particular to a high-efficiency ytterbium-erbium co-doped optical fiber and its preparation method. Technical Background

[0002] In recent years, with the rapid development of emerging industries such as the Industrial Internet, smart cities, and autonomous driving, the volume of information and data has exploded. 5G communication technology based on long-distance terrestrial fiber optic communication is gradually facing limitations such as insufficient communication bandwidth, transmission rates approaching the Shannon limit, and complex ground environments. Building a satellite internet in space, using laser light sources for laser communication between the ground and satellites, offers advantages such as wide coverage, high transmission efficiency, and low latency, making it a potential technological solution for developing next-generation communication technologies. Ytterbium-erbium co-doped fiber is an essential core gain material in 1.5-micron band laser communication systems, amplifying signal power. However, the presence of various cosmic ray radiation in the space environment can cause various color center defects in the core of conventional ytterbium-erbium co-doped fiber, leading to a sharp increase in background loss and a continuous decrease in fiber energy conversion efficiency, resulting in reduced output power and even the inability to amplify optical signals. Furthermore, energy is extremely precious in space applications; higher fiber energy conversion efficiency translates to higher energy utilization and significant savings in manufacturing costs. Therefore, in order to meet the requirements of long-term high-performance operation in the space environment, it is necessary to ensure that ytterbium-erbium optical fibers maintain high energy conversion efficiency during long-term operation in the radiation environment.

[0003] Studies have shown that to achieve high energy conversion efficiency in ytterbium-erbium co-doped optical fibers, a high energy transfer efficiency from ytterbium to erbium must be ensured. Therefore, high concentrations of luminescent rare-earth ions (erbium and ytterbium) and phosphorus are required in the fiber (Journal of Lightwave Technology, 1998, Vol. 16, No. 11). However, the solubility of rare-earth ions in quartz glass is relatively low. High-concentration doping can lead to the aggregation of luminescent rare-earth ions in the quartz glass, resulting in fluorescence quenching, severe upconversion luminescence, and energy consumption in the 1.5 μm signal band, significantly reducing the fiber laser slope efficiency. Furthermore, phosphorus pentoxide, the oxide of phosphorus, has a boiling point of only 360℃. During core rod fabrication, a prolonged high-temperature process exceeding 1000℃ is required, causing significant phosphorus volatilization and loss, resulting in low phosphorus doping concentration and poor doping uniformity. Simultaneously, the large-scale volatilization of phosphorus also carries away luminescent rare-earth ions (such as erbium and ytterbium), leading to a low fiber absorption coefficient.

[0004] In existing technologies, measures such as radiation hardening are often used to reduce the efficiency attenuation of optical fibers under irradiation conditions. However, these measures neglect the energy conversion efficiency of the original optical fiber before irradiation, resulting in a low efficiency of the original fiber before irradiation. Therefore, there is a need for a high-efficiency radiation-resistant erbium-ytterbium co-doped optical fiber with excellent overall performance, exhibiting high original efficiency before irradiation and minimal efficiency attenuation after irradiation. This fiber is expected to be used in space environments. Summary of the Invention

[0005] To overcome the above shortcomings, this invention proposes a high-efficiency erbium-ytterbium co-doped optical fiber, its preparation method, and its application. The original optical fiber has high laser slope efficiency before radiation and low efficiency attenuation after radiation, exhibiting excellent overall performance.

[0006] To achieve the above technical objectives, this application adopts the following technical solution.

[0007] In a first aspect, this invention provides a high-efficiency ytterbium-erbium co-doped silica glass optical fiber. The core is mainly composed of SiO2, and the doping elements include at least Lu, Yb, Er, Ce, P, and Ge. The core composition range is: Lu2O3: 0.01–0.3 mol%, Yb2O3: 0.6–0.9 mol%, Er2O3: 0.01–0.1 mol%, Ce2O3: 0.1–0.24 mol%, P2O5: 8–12 mol%, GeO2: 0.2–1 mol%, SiO2: 85.46–91.16 mol%. Lu is element number 71, and its ionic radius is closest to that of ytterbium (element number 70) and erbium (element number 68). During the sol-gel immersion doping process, an appropriate amount of Lu is introduced... 3+ The ions can effectively disperse the luminescent ytterbium and erbium ions, effectively preventing the formation of rare earth ion clusters in the glass matrix under high concentration doping. More importantly, Lu 3+ The ions have a full electron configuration and do not undergo the 4f-4f energy level transitions common in rare earth ions. Therefore, Lu 3+ Ions are spectrally inert; they neither absorb nor emit light. Therefore, doping with Lu... 3+ Ions do not degrade the laser performance of erbium-ytterbium co-doped fibers and are suitable as dispersants for erbium-ytterbium co-doped fibers.

[0008] A second aspect of the present invention provides a method for preparing erbium-ytterbium co-doped optical fibers, characterized by comprising the following steps:

[0009] S1: According to the designed glass group ratio, add the chloride or nitrate raw materials of the four rare earth elements Yb, Er, Ce and Lu to a mixed solution of methanol or ethanol and water. After stirring and dissolving thoroughly, add diammonium hydrogen phosphate to make the solution alkaline. Continue stirring to obtain a clear and transparent solution, then add tetrapropoxysilane. Stir at a constant temperature of 20-40℃ for 1-8 days to allow the tetrapropoxysilane to undergo a complete hydrolysis and polymerization reaction, and obtain a stable and clear sol mixture.

[0010] S2: The three raw materials SiCl4, GeCl4 and POCl3 are heated and evaporated at a constant temperature of 32-40℃. They are then transported into a clean high-purity quartz tube through oxygen. An oxidation reaction occurs at a temperature of 1350-1500℃, depositing a layer of white porous soot of P2O5, GeO2 and SiO2 on the inner wall of the quartz tube. This ensures that the deposited layer has strong adhesion and is not easy to fall off.

[0011] S3: Immerse the quartz tube with a white porous soot layer on the inner wall at a constant temperature of 25-45℃ in the sol solution obtained in step S1 for 3-5 hours, thereby doping Lu, Yb, Er, Ce, P and Ge elements into the white porous soot layer of silica. After high-temperature dehydration and carbon removal treatment, the white porous soot layer forms a transparent doped glass layer.

[0012] S4: Repeat steps S2 and S3 multiple times to increase the thickness of the transparent doped glass layer;

[0013] S5: The deposition tube is heated to above 2100℃ using an oxyhydrogen flame. It is then moved at a constant speed of 20-50mm / min from one end of the rotary sealing joint to the other end of the ash collection box, maintaining a slight positive pressure inside the tube. After multiple rounds of heating, the quartz tube is collapsed into a solid doped preform.

[0014] S6: After the preform is formed by gas laser processing, it is prepared into an optical fiber preform that meets the size specifications. After being drawn and coated under a high-temperature drawing tower, it is made into erbium-ytterbium co-doped quartz glass optical fiber of a specific size.

[0015] Lu 3+ The mass fraction of ions in the fiber core is 0.05% to 1.41%, which achieves good dispersion while ensuring that the fiber loss does not increase significantly, thus improving the fiber laser amplification efficiency.

[0016] Preferably, in step S1, diammonium hydrogen phosphate is added to the mixed solution to make the pH value of the sol solution between 7.5 and 9, so that the solution is weakly alkaline, which is conducive to the formation of a uniform three-dimensional network structure after the hydrolysis and condensation of tetrapropoxysilane, and improves the doping uniformity of rare earth ions.

[0017] Preferably, in step S1, tetrapropoxysilane is added to a clear and transparent solution, and the solution is stirred at a constant temperature of 30-40°C for 3-5 days to allow the tetrapropoxysilane to undergo a complete hydrolysis and polymerization reaction to form a sol.

[0018] Preferably, in step S3, immersion in the solution at a constant temperature of 30-35℃ can reduce the fluctuation of doping concentration caused by ambient temperature fluctuations, and improve doping uniformity and process repeatability.

[0019] Preferably, in step S5, carbon dioxide laser processing of the preform can reduce the hydroxyl content in the optical fiber, thereby reducing optical fiber loss. Compared with traditional mechanical grinding, it is more flexible and convenient to process irregular structures.

[0020] Compared with the prior art, the beneficial effects of the present invention are:

[0021] (1) By introducing an appropriate amount of Yb 3+ and Er 3+ Lu 3+ Ions, can be used for luminescent ions Yb 3+ and Er 3+ Dispersing ions and suppressing the formation of rare earth ion clusters helps to reduce upconversion luminescence and improve energy conversion efficiency. Meanwhile, Lu... 3+ It does not emit light itself and will not adversely affect the performance of fiber lasers.

[0022] (2) The use of sol-gel doping technology is beneficial to the dispersion and uniformity of doped elements. On the other hand, the liquid-phase phosphorus doping allows rare earth ions to pre-bind with phosphorus, ensuring the activation of Yb ions. 3+ and Er 3+ Being in a phosphorus-encapsulated local environment is beneficial to Yb 3+ Ions to Er 3+ The energy transfer process of ions can also effectively compensate for the volatilization of phosphorus at high temperatures, thereby obtaining a core rod with high phosphorus doping, which is beneficial to improving the efficiency of fiber lasers and also enhances radiation resistance.

[0023] In summary, improving the efficiency of fiber lasers operating in radiation environments can effectively reduce pump power and save energy consumption while achieving the same output power. This is very important for space applications and can reduce the overall system manufacturing cost.

[0024] It should be understood that, within the scope of this invention, the above-described technical features of this invention and the technical features specifically described below (such as in the embodiments) can be combined with each other to form new or preferred technical solutions. Due to space limitations, they will not be described in detail here. Attached Figure Description

[0025] Figure 1This application presents an optical path diagram for testing laser amplification efficiency and radiation resistance; where 1 is a 1550nm seed source, 2 is an optical fiber isolator, 3 is a passive optical fiber, 4 is a fusion splice, 5 is the erbium-ytterbium co-doped optical fiber under test, 6 is a fusion splice, 7 is a passive optical fiber, 8 is a bundle combiner, 9 is a power meter, 10 is a 940nm semiconductor laser, and 11 is an X-ray irradiator.

[0026] Figure 2 The output power of the optical fiber before irradiation in Examples 1-4 and Comparative Examples 1-2 varies with the pump light power.

[0027] Figure 3 Figure 1: Gain attenuation over time during fiber irradiation as described in Examples 1-4.

[0028] Figure 4 Comparative Examples 1 and 2: Gain attenuation over time during irradiation of the optical fiber.

[0029] Figure 5 : Fiber refractive index distribution diagram of Example 4. Detailed Implementation

[0030] The present invention will be described in detail below with reference to embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make several modifications and improvements without departing from the concept of the present invention. These all fall within the protection scope of the present invention.

[0031] In the description of this invention, "efficiency," "energy conversion efficiency," "slope efficiency," and "amplification efficiency" have essentially the same meaning; they all evaluate the efficiency of an optical fiber in utilizing pump light energy when outputting laser light. A higher slope means lower pump energy is required for the same output, which is more beneficial for reducing costs in space applications. In this invention, a master oscillator power amplifier (MOPA) and a back-pumped test optical path are used to evaluate the performance of the optical fiber, such as... Figure 1As shown, the seed source is a 1550nm distributed feedback laser diode, with a fixed seed signal light power of 200mW and power fluctuation <1%. A reverse pumping method is used, with a 940nm laser diode as the pump source, achieving a maximum output power of 12W. The erbium-ytterbium co-doped fiber under test is placed inside an X-ray irradiator, and the irradiation dose at the fiber location is calibrated. The remaining components are placed outside the irradiator via passive fiber connections. Without turning on the X-ray irradiator (i.e., under radiation-free conditions), the pump power is gradually increased to 3W, 5W, 8W, 10W, and 12W, while the signal light amplification output power value η0 is recorded using a power meter. The slope obtained after linear fitting is the slope efficiency value of the fiber laser amplification before irradiation. To evaluate the fiber's radiation resistance, the pump power is set to 12W, and the maximum output power P0 is recorded. Then the X-ray irradiator is turned on, with an irradiation dose rate of 100 rad / min. Under X-ray irradiation, the output laser power will gradually decrease, and the output power value P is recorded in real time. t After 100 minutes of irradiation, the X-ray irradiator is turned off. Due to the laser bleaching effect, the output power will gradually recover.

[0032] Internationally, radiation-induced gain variation is commonly used to evaluate the radiation resistance of optical fibers. The formula for calculating the radiation gain attenuation G is as follows:

[0033] G = 10 * lg(P) t / P0)

[0034] During X-ray irradiation, the output power P is affected by the color center defects induced in the fiber core by the X-rays. t As the gain gradually decreases, the gain attenuation G becomes negative. The smaller the absolute value of G, the better the radiation resistance of the optical fiber.

[0035] The slope efficiency η of fiber laser amplification after irradiation t The calculation formula is as follows:

[0036] η t =η0*P t / P0

[0037] Compared to the slope efficiency η0 before irradiation, the slope efficiency η after irradiation t The smaller the attenuation, the better the radiation resistance of the optical fiber. In actual use in a radiation environment, the optical fiber requires less pump light energy to achieve the same output power, making it suitable for applications where energy is extremely precious, such as space.

[0038] It is important to note that the radiation resistance of optical fibers is related not only to the total radiation dose but also directly to the dose rate and the type of radiation source. A higher dose rate results in poorer radiation resistance. In actual space environments, the radiation dose rate is low, typically less than 0.3 rad / min, and there are many different types of radiation sources. The same conditions cannot be used for evaluation in terrestrial environments, and the evaluation process would be too time-consuming. Therefore, this invention uses high-dose-rate X-rays (100 rad / min) to rapidly assess the radiation resistance of optical fibers. The gain and efficiency attenuation in this test will be greater than the results in actual space environments. However, under strict control of other variables, it can accurately reflect and evaluate the radiation resistance of different optical fibers.

[0039] The following is a detailed description with reference to the embodiments. The core composition of the embodiments and comparative examples was analyzed by electron probe microscopy, as shown in Table 1.

[0040] Table 1 shows the core composition (mole fraction) of each embodiment and comparative example. In Examples 1-4, the core composition is lutetium-cerium-erbium-ytterbium-phosphorus-germanium co-doped quartz glass. Comparative Example 1 is a commercially available optical fiber with a core composition of erbium-ytterbium-phosphorus co-doped quartz glass. Comparative Example 2 is an optical fiber prepared using a conventional solution doping method with a core composition of erbium-ytterbium-cerium co-doped quartz glass.

[0041]

[0042] Table 1: Core composition of each embodiment and comparative example

[0043] Example 1:

[0044] This invention provides a high-efficiency erbium-ytterbium co-doped silica double-clad optical fiber, the core glass composition of which is: 0.01 mol% Lu₂O₃, 0.24 mol% Ce₂O₃, 0.6 mol% Yb₂O₃, 0.03 mol% Er₂O₃, 8 mol% P₂O₅, 1 mol% GeO₂, and 90.12 mol% SiO₂. The fiber core diameter is 12 micrometers, and the silica inner cladding diameter is 125 micrometers. The preparation method of this erbium-ytterbium co-doped optical fiber mainly includes the following steps:

[0045] Weigh out the three raw materials, ytterbium chloride hexahydrate, erbium chloride hexahydrate, and lutetium chloride hexahydrate, according to the fiber core glass composition. Add water and methanol or ethanol in a 1:6 ratio and stir. At the same time, add diammonium hydrogen phosphate to make the pH value 7.5. After the raw materials are completely dissolved, add tetrapropoxysilane to make it hydrolyze. Stir at a constant temperature of 20°C for 8 days before use.

[0046] Three liquid raw materials, SiCl4, GeCl4 and POCl3, are heated at a constant temperature of 32°C and then introduced into a clean high-purity quartz tube through oxygen at a flow rate of 500 sccm. The outer wall of the quartz tube is heated with an oxyhydrogen flame, and an oxidation reaction occurs at a temperature of 1450°C, depositing a layer of white porous soot of P2O5, GeO2 and SiO2 on the inner wall of the quartz tube.

[0047] The quartz tube with a white porous soot layer on the inner wall was immersed in the obtained sol solution and soaked at a constant temperature of 25°C for 5 hours, thereby doping the white porous soot layer of silica with Yb, Er, Ce, Lu, P and Ge elements.

[0048] After the quartz tube undergoes multiple deposition, soaking, and doping processes involving dehydration and carbon removal, it is heated to over 2100°C using an oxyhydrogen flame. The tube is then moved at a constant speed of 20-50 mm / min from one end of the rotary sealing joint to the other end of the ash collection box, maintaining a slight positive pressure inside the tube. After multiple rounds of heating, the quartz tube collapses into a solid doped preform.

[0049] A circular preform was fabricated using a carbon dioxide laser. Two 5mm diameter holes were drilled symmetrically on both sides of the fiber core, and two high-stress boron rods were inserted to prepare a polarization-maintaining fiber preform that meets the size specifications. After being drawn and coated under a high-temperature drawing tower, a 12 / 125μm erbium-ytterbium co-doped silica glass polarization-maintaining fiber was produced.

[0050] Adopting such Figure 1 The fiber amplifier shown was used to test the slope efficiency of the fiber before irradiation. The fiber length was 10 meters. Then, under X-ray irradiation, the radiation-induced gain attenuation of the fiber over time was tested. The X-ray dose rate was 100 rad / min, and the irradiation time was 100 min. Figure 2 As shown, the original fiber slope efficiency is 35.9%. Figure 3 As shown, the gain attenuation G = -1.64 dB after irradiation for 100 min is calculated to be 24.6% when the irradiation dose is 10000 rad.

[0051] Example 2:

[0052] This invention provides a high-efficiency erbium-ytterbium co-doped silica double-clad optical fiber, the core glass composition of which is: 0.1 mol% Lu₂O₃, 0.2 mol% Ce₂O₃, 0.65 mol% Yb₂O₃, 0.04 mol% Er₂O₃, 9.8 mol% P₂O₅, 0.8 mol% GeO₂, and 88.41 mol% SiO₂. The fiber core diameter is 12 micrometers, and the silica inner cladding diameter is 125 micrometers. The preparation method of this erbium-ytterbium co-doped optical fiber mainly includes the following steps:

[0053] Weigh out the three raw materials, ytterbium chloride hexahydrate, erbium chloride hexahydrate, and lutetium chloride hexahydrate, according to the fiber core glass composition. Add water and methanol or ethanol in a 1:6 ratio and stir. At the same time, add diammonium hydrogen phosphate to make the pH value 7.9. After the raw materials are completely dissolved, add tetrapropoxysilane to make it hydrolyze. Stir at 35°C for 2 days before use.

[0054] Three liquid raw materials, SiCl4, GeCl4 and POCl3, are heated at a constant temperature of 35°C and then introduced into a clean high-purity quartz tube through oxygen at a flow rate of 500 sccm. The outer wall of the quartz tube is heated with an oxyhydrogen flame, and an oxidation reaction occurs at a temperature of 1450°C, depositing a layer of white porous soot of P2O5, GeO2 and SiO2 on the inner wall of the quartz tube.

[0055] The quartz tube with a white porous soot layer on the inner wall was immersed in the obtained sol solution and soaked at a constant temperature of 35°C for 3 hours, thereby doping the white porous soot layer of silica with Lu, Yb, Er, Ce, P and Ge elements.

[0056] After the quartz tube undergoes multiple deposition, soaking, and doping processes involving dehydration and carbon removal, it is heated to over 2100°C using an oxyhydrogen flame. The tube is then moved at a constant speed of 20-50 mm / min from one end of the rotary sealing joint to the other end of the ash collection box, maintaining a slight positive pressure inside the tube. After multiple rounds of heating, the quartz tube collapses into a solid doped preform.

[0057] A circular preform was fabricated using a carbon dioxide laser. Two 5.2mm diameter holes were drilled symmetrically on both sides of the fiber core, and two high-stress boron rods were inserted to prepare a polarization-maintaining fiber preform that meets the size specifications. After being drawn and coated under a high-temperature drawing tower, a 12 / 125μm erbium-ytterbium co-doped silica glass polarization-maintaining fiber was produced.

[0058] Adopting such Figure 1 The fiber amplifier shown was used to test the slope efficiency of the fiber before irradiation. The fiber length was 10 meters. Then, under X-ray irradiation, the radiation-induced gain attenuation of the fiber over time was tested. The X-ray dose rate was 100 rad / min, and the irradiation time was 100 min. Figure 2 As shown, the original fiber slope efficiency is 38.9%. Figure 3 As shown, the gain attenuation G = -1.34 dB after 100 min of irradiation. The calculated fiber slope efficiency is 28.6% when the irradiation dose is 10000 rad.

[0059] Example 3:

[0060] This invention provides a high-efficiency erbium-ytterbium co-doped silica double-clad optical fiber, the core glass composition of which is: 0.14 mol% Lu₂O₃, 0.16 mol% Ce₂O₃, 0.68 mol% Yb₂O₃, 0.05 mol% Er₂O₃, 9.3 mol% P₂O₅, 0.55 mol% GeO₂, and 89.12 mol% SiO₂. The fiber core diameter is 12 micrometers, and the silica inner cladding diameter is 125 micrometers. The preparation method of this erbium-ytterbium co-doped optical fiber mainly includes the following steps:

[0061] Weigh out the three raw materials, ytterbium chloride hexahydrate, erbium chloride hexahydrate, and lutetium chloride hexahydrate, according to the fiber core glass composition. Add water and methanol or ethanol in a 1:6 ratio and stir. At the same time, add diammonium hydrogen phosphate to make the pH value 8.5. After the raw materials are completely dissolved, add tetrapropoxysilane to make it hydrolyze. Stir at 32°C for 4 days before use.

[0062] Three liquid raw materials, SiCl4, GeCl4 and POCl3, are heated at a constant temperature of 38°C and then introduced into a clean high-purity quartz tube through oxygen at a flow rate of 500 sccm. The outer wall of the quartz tube is heated with an oxyhydrogen flame, and an oxidation reaction occurs at a temperature of 1450°C, depositing a layer of white porous soot of P2O5, GeO2 and SiO2 on the inner wall of the quartz tube.

[0063] The quartz tube with a white porous soot layer on the inner wall was immersed in the obtained sol solution at a constant temperature of 40°C for 3.5 hours, thereby doping the white porous soot layer of silica with Lu, Yb, Er, Ce, P and Ge elements.

[0064] After the quartz tube undergoes multiple deposition, soaking, and doping processes involving dehydration and carbon removal, it is heated to over 2100°C using an oxyhydrogen flame. The tube is then moved at a constant speed of 20-50 mm / min from one end of the rotary sealing joint to the other end of the ash collection box, maintaining a slight positive pressure inside the tube. After multiple rounds of heating, the quartz tube collapses into a solid doped preform.

[0065] A circular preform was fabricated using a carbon dioxide laser. Two 5.2mm diameter holes were drilled symmetrically on both sides of the fiber core, and two high-stress boron rods were inserted to prepare a polarization-maintaining fiber preform that meets the size specifications. After being drawn and coated under a high-temperature drawing tower, a 12 / 125μm erbium-ytterbium co-doped silica glass polarization-maintaining fiber was produced.

[0066] Adopting such Figure 1 The fiber amplifier shown was used to test the slope efficiency of the fiber before irradiation. The fiber length was 10 meters. Then, under X-ray irradiation, the radiation-induced gain attenuation of the fiber over time was tested. The X-ray dose rate was 100 rad / min, and the irradiation time was 100 min. Figure 2 As shown, the original fiber slope efficiency is 36.5%. Figure 3 As shown, after 100 minutes of irradiation, the gain attenuation G = -1.07 dB. When the irradiation dose is 10000 rad, the fiber slope efficiency is calculated to be 28.5%.

[0067] Example 4:

[0068] This invention provides a high-efficiency erbium-ytterbium co-doped silica double-clad optical fiber, the core glass composition of which is: 0.3 mol% Lu₂O₃, 0.1 mol% Ce₂O₃, 0.9 mol% Yb₂O₃, 0.1 mol% Er₂O₃, 12 mol% P₂O₅, 0.1 mol% GeO₂, and 86.5 mol% SiO₂. The fiber core diameter is 12 micrometers, and the silica inner cladding diameter is 125 micrometers. The preparation method of this erbium-ytterbium co-doped optical fiber mainly includes the following steps:

[0069] Weigh out the three raw materials, ytterbium chloride hexahydrate, erbium chloride hexahydrate, and lutetium chloride hexahydrate, according to the fiber core glass composition. Add water and methanol or ethanol in a 1:6 ratio and stir. At the same time, add diammonium hydrogen phosphate to make the pH value 9.2. After the raw materials are completely dissolved, add tetrapropoxysilane to make it hydrolyze. Stir at 40°C for 1 day before use.

[0070] Three liquid raw materials, SiCl4, GeCl4 and POCl3, are heated at a constant temperature of 40°C and then introduced into a clean high-purity quartz tube through oxygen at a flow rate of 500 sccm. The outer wall of the quartz tube is heated with an oxyhydrogen flame, and an oxidation reaction occurs at a temperature of 1450°C, depositing a layer of white porous soot of P2O5, GeO2 and SiO2 on the inner wall of the quartz tube.

[0071] The quartz tube with a white porous soot layer on the inner wall was immersed in the obtained sol solution and soaked at a constant temperature of 45°C for 3 hours, thereby doping the white porous soot layer of silica with Lu, Yb, Er, Ce, P and Ge elements.

[0072] After the quartz tube undergoes multiple deposition, soaking, and doping processes involving dehydration and carbon removal, it is heated to over 2100°C using an oxyhydrogen flame. The tube is then moved at a constant speed of 20-50 mm / min from one end of the rotary sealing joint to the other end of the ash collection box, maintaining a slight positive pressure inside the tube. After multiple rounds of heating, the quartz tube collapses into a solid doped preform.

[0073] Octagonal preforms were fabricated using carbon dioxide laser processing to prepare unbiased fiber preforms conforming to specific dimensions. These preforms were then drawn and coated under a high-temperature drawing tower to produce 12 / 125 μm erbium-ytterbium co-doped silica glass unbiased optical fibers. The refractive index distribution of the fiber is as follows: Figure 5 As shown, the refractive index pit at the center of the optical fiber is relatively small, indicating that it has a good inhibitory effect on the volatilization of phosphorus and rare earth elements.

[0074] Adopting such Figure 1 The fiber amplifier shown was used to test the slope efficiency of the fiber before irradiation. The fiber length was 10 meters. Then, under X-ray irradiation, the radiation-induced gain attenuation of the fiber over time was tested. The X-ray dose rate was 100 rad / min, and the irradiation time was 100 min. Figure 2 As shown, the original fiber slope efficiency is 35.5%. Figure 3 As shown, after 100 min of X-ray irradiation, the gain attenuation G = -1.85 dB. The calculated fiber slope efficiency is 23.2% when the irradiation dose is 10000 rad.

[0075] Comparative Example 1

[0076] We purchased non-radiation-resistant erbium-ytterbium co-doped optical fiber from a foreign company. Electron probe microanalysis (EPMA) showed that the fiber core material was Er, Yb, and P co-doped SiO2 glass, with a composition of 0.8 mol% Yb2O3, 0.15 mol% Er2O3, 10.5 mol% P2O5, and 88.55 mol% SiO2.

[0077] Adopting such Figure 1 The fiber amplifier shown was used to test the slope efficiency of the fiber before irradiation. The fiber length was 10 meters. Then, under X-ray irradiation, the radiation-induced gain attenuation of the fiber over time was tested. The X-ray dose rate was 100 rad / min, and the irradiation time was 100 min. Figure 2 As shown, the original fiber slope efficiency is 34.4%. Figure 4 As shown, after 100 minutes of irradiation, the gain attenuation G = -5.9 dB. The calculated fiber slope efficiency at an irradiation dose of 10000 rad is 8.8%. It can be seen that the original efficiency of this fiber is low, and its radiation resistance is extremely poor. After irradiation, the efficiency drops to 8.8%, which is insufficient for use in radiation scenarios such as space.

[0078] Comparative Example 2

[0079] As a comparative example, an optical fiber was fabricated by doping Ce₂O₃ into the fiber core, without doping with Lu₂O₃ or GeO₂. The core glass composition was: 0.2 mol% Ce₂O₃, 0.66 mol% Yb₂O₃, 0.04 mol% Er₂O₃, 10 mol% P₂O₅, 0.8 GeO₂, and 88.3 mol% SiO₂. The fiber core diameter was 12 micrometers, and the quartz inner cladding diameter was 125 micrometers. This embodiment of erbium-ytterbium co-doped optical fiber fabrication employs a conventional solution doping method, mainly including the following steps:

[0080] Weigh out ytterbium chloride hexahydrate and erbium chloride hexahydrate according to the fiber core glass composition, add methanol or ethanol and stir until the raw materials are completely dissolved before use.

[0081] Two liquid raw materials, SiCl4 and POCl3, are heated at a constant temperature of 38°C and then introduced into a clean, high-purity quartz tube through an oxygen flow rate of 500 sccm. The outer wall of the quartz tube is heated using an oxyhydrogen flame, and an oxidation reaction occurs at a temperature of 1450°C, depositing a layer of white porous soot of P2O5 and SiO2 on the inner wall of the quartz tube.

[0082] The quartz tube with a white porous soot layer on its inner wall was immersed in the alcohol solution obtained in step 1 and kept at a constant temperature of 25°C for 3 hours, thereby doping the white porous soot layer with Yb, Er, Ce and P elements.

[0083] After the quartz tube is dehydrated and repeatedly deposited, soaked and doped, the deposition tube is heated to above 2100℃ using an oxyhydrogen flame. It is then moved at a constant speed of 20-50 mm / min from one end of the rotary sealing joint to the other end of the ash collection box, maintaining a slight positive pressure inside the tube. After repeated heating, the quartz tube collapses into a solid doped preform.

[0084] A circular preform was fabricated using a carbon dioxide laser. Two 5mm diameter holes were drilled symmetrically on both sides of the fiber core, and two high-stress boron rods were inserted to prepare a polarization-maintaining fiber preform that meets the size specifications. After being drawn and coated under a high-temperature drawing tower, a 12 / 125μm erbium-ytterbium co-doped silica glass polarization-maintaining fiber was produced.

[0085] Adopting such Figure 1 The fiber amplifier shown was used to test the slope efficiency of the fiber before irradiation. The fiber length was 10 meters. Then, under X-ray irradiation, the radiation-induced gain attenuation of the fiber over time was tested. The X-ray dose rate was 100 rad / min, and the irradiation time was 100 min. Figure 2 As shown, the original fiber slope efficiency is 32.7%. Figure 4 As shown, the gain attenuation G = -2.6dB after 100 min of irradiation. The calculated fiber slope efficiency is 18% when the irradiation dose is 10000 rad.

[0086] Compared with Example 2, it can be seen that the fiber core of Comparative Example 2 does not contain the dispersant Lu2O3, while other components are basically the same as in Example 2. Prepared using conventional solution doping technology, the fiber slope efficiency before irradiation was only 32.7%, and after irradiation, the fiber gain attenuation was significant, with an efficiency of only 18%. In contrast, the fiber slope efficiency of Example 2 was 38.9% before irradiation, and after irradiation, the gain attenuation was small, with the fiber slope efficiency remaining at 28.6%. This indicates that Lu doping... 3+ Yb 3+ and Er 3+This dispersion effect helps improve efficiency. The conventional technique used in Comparative Example 2 has certain disadvantages in terms of doping uniformity, resulting in lower energy conversion efficiency of the optical fiber, which cannot meet the requirements for long-term service in radiation scenarios such as space. The preparation method proposed in this invention, however, has a significant advantage in optical fiber efficiency.

[0087] from Figure 2 It can be seen that the pre-irradiation efficiencies of Examples 1-4 are all greater than 35%, indicating that the optical fiber of the present invention has a high energy conversion efficiency. This is because the core composition and preparation method can improve the uniformity of rare earth doping and avoid clustering, thereby improving the slope efficiency of the optical fiber. Figure 3 and Figure 5 As can be seen, the fiber gain attenuation of the present invention is significantly less than that of commercial fiber and fiber prepared by conventional methods, and it can maintain high efficiency after radiation, making it suitable for use in laser amplifiers in radiation scenarios such as space.

[0088] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the embodiments described above. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A ytterbium-erbium co-doped silica glass optical fiber, characterized in that, The fiber core is SiO2 glass doped with Lu, Yb, Er, Ce, P, and Ge elements. The core composition range is: Lu2O3: 0.01~0.3 mol%, Yb2O3: 0.6~0.9 mol%, Er2O3: 0.03~0.1 mol%, Ce2O3: 0.1~0.24 mol%, P2O5: 8~12 mol%, GeO2: 0.1~1 mol%, SiO2: 86.5~90.12 mol% The method for preparing the optical fiber includes: S1: Add the chloride or nitrate raw materials of the four rare earth elements Yb, Er, Ce and Lu that meet the theoretical composition ratio to a mixed solution of methanol or ethanol and water. After stirring thoroughly to dissolve the raw materials, add diammonium hydrogen phosphate to make the pH value of the solution greater than 7. Continue stirring to obtain a clear and transparent solution, then add tetrapropoxysilane. Stir at a constant temperature of 20-40℃ for 1-8 days to allow the tetrapropoxysilane to undergo a complete hydrolysis and polymerization reaction, and obtain a clear and transparent silica-doped sol solution. S2: Three liquid raw materials, SiCl4, GeCl4 and POCl3, are heated at a constant temperature of 32-40℃ and introduced into a clean high-purity quartz glass tube through oxygen. An oxidation reaction occurs at a temperature of 1350-1500℃, depositing a layer of white porous soot of P2O5, GeO2 and SiO2 on the inner wall of the quartz glass tube, ensuring that the deposited layer has strong adhesion and is not easy to fall off. S3: The quartz glass tube with a white porous soot layer on the inner wall is immersed in the sol solution obtained in step S1 at a constant temperature of 25-45℃ for 3-5 hours, thereby obtaining a white porous soot layer of silica doped with Lu, Yb, Er, Ce, P and Ge elements on the inner wall of the quartz glass tube. After high-temperature dehydration and decarbonization treatment, the white porous soot layer forms a transparent doped glass layer.

2. The ytterbium-erbium co-doped silica glass optical fiber according to claim 1, characterized in that, The composition range of the fiber core is: 0.14 mol% Lu2O3, 0.16 mol% Ce2O3, 0.68 mol% Yb2O3, 0.05 mol% Er2O3, 9.3 mol% P2O5, 0.55 mol% GeO2, and 89.12 mol% SiO2.

3. The ytterbium-erbium co-doped silica glass optical fiber according to claim 1, characterized in that, The fiber core contains non-luminescent rare earth ions Lu 3+ For luminescent rare earth ions Yb 3+ and Er 3+ Disperse, Lu 3+ The mass fraction of ions in the fiber core material is 0.05% to 1.41%.

4. A method for preparing ytterbium-erbium co-doped silica glass optical fiber as described in any one of claims 1-3, characterized in that, It includes the following main steps: S1: Add the chloride or nitrate raw materials of the four rare earth elements Yb, Er, Ce and Lu that meet the theoretical composition ratio to a mixed solution of methanol or ethanol and water. After stirring thoroughly to dissolve the raw materials, add diammonium hydrogen phosphate to make the pH value of the solution greater than 7. Continue stirring to obtain a clear and transparent solution, then add tetrapropoxysilane. Stir at a constant temperature of 20-40℃ for 1-8 days to allow the tetrapropoxysilane to undergo a complete hydrolysis and polymerization reaction, and obtain a clear and transparent silica-doped sol solution. S2: Three liquid raw materials, SiCl4, GeCl4 and POCl3, are heated at a constant temperature of 32-40℃ and introduced into a clean high-purity quartz glass tube through oxygen. An oxidation reaction occurs at a temperature of 1350-1500℃, depositing a layer of white porous soot of P2O5, GeO2 and SiO2 on the inner wall of the quartz glass tube, ensuring that the deposited layer has strong adhesion and is not easy to fall off. S3: The quartz glass tube with a white porous soot layer on the inner wall is immersed in the sol solution obtained in step S1 at a constant temperature of 25-45℃ for 3-5 hours, thereby obtaining a white porous soot layer of silica doped with Lu, Yb, Er, Ce, P and Ge elements on the inner wall of the quartz glass tube. After high temperature dehydration and carbon removal treatment, the white porous soot layer forms a transparent doped glass layer. S4: Repeat steps S2 and S3 multiple times to increase the thickness of the transparent doped glass layer; S5: The quartz glass tube is heated to above 2100℃ using an oxyhydrogen flame, maintaining a slight positive pressure inside the tube. The heating head moves at a constant speed of 20-50mm / min from one end of the rotary sealing joint to the other end of the ash collection box. After multiple round trips of heating, the quartz glass tube collapses into a solid doped core rod. S6: After the core rod undergoes gas laser surface processing and mechanical drilling, it is prepared into an optical fiber preform that meets the size specifications. It is then drawn into the ytterbium-erbium co-doped quartz glass optical fiber under a high-temperature drawing tower.

5. The method for preparing a ytterbium-erbium co-doped silica glass optical fiber according to claim 4, characterized in that, In step S1, diammonium hydrogen phosphate is added to the mixed solution to bring the pH of the solution to between 7.5 and 9.

6. The method for preparing a ytterbium-erbium co-doped silica glass optical fiber according to claim 4, characterized in that, In step S1, tetrapropoxysilane is added to the clear and transparent solution, and the solution is stirred at a constant temperature of 30-40°C for 3-5 days to allow the tetrapropoxysilane to undergo a complete hydrolysis and polymerization reaction, resulting in a clear and transparent sol solution.

7. The method for preparing a ytterbium-erbium co-doped silica glass optical fiber according to claim 4, characterized in that, In step S3, the quartz glass tube is immersed in the sol solution obtained in step S1 at a constant temperature of 30-35°C.

8. The method for preparing a ytterbium-erbium co-doped silica glass optical fiber according to claim 4, characterized in that, In step S6, the core rod undergoes surface processing with a carbon dioxide laser to obtain an optical fiber preform of a certain size and specification.

9. The application of a ytterbium-erbium co-doped silica glass optical fiber according to claim 1 or 2, characterized in that, The ytterbium-erbium co-doped silica glass fiber is used in space radiation environments.

Citation Information

Patent Citations

  • Anti-photodarkening ytterbium-doped quartz optical fiber and preparation method thereof

    CN109502961A

  • Anti-radiation polarization-maintaining erbium-ytterbium co-doped optical fiber and preparation method and application thereof

    CN115304266A