An impact-resistant semi-prefabricated polyurethane runway and a preparation method thereof

By using a multi-layer core-shell structure and modified fillers in polyurethane runways, the problem of poor impact resistance of existing polyurethane runways is solved, and the impact resistance and durability of the runways are significantly improved.

CN118290701BActive Publication Date: 2024-10-25HUNAN YUNAO NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410447411.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2024-10-25
Estimated Expiration
2044-04-15

AI Technical Summary

Technical Problem

Existing polyurethane tracks have poor impact resistance, causing athletes' joints and muscles to suffer excessive impact, increasing the possibility of fatigue and injury.

Method used

An impact-resistant semi-prefabricated polyurethane runway is prepared by mixing polytetrahydrofuran ether glycol, diphenylmethane diisocyanate and ethyl acetate, and adding dibutyltin dilaurate, 1,4-butanediol, Carbon black and pigments form the base layer and surface layer, combined with modified fillers and modified monomers to form a multi-layer core-shell structure to improve impact resistance.

Benefits of technology

Significantly improves the impact resistance of the runway. Through the breakage of disulfide bonds and the three-dimensional polyhedral structure of silsesquioxane, it can effectively absorb impact energy, reduce runway damage, and restore broken disulfide bonds when the temperature changes, extending the runway. service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004791490920000121
    Figure BDA0004791490920000121
  • Figure BDA0004791490920000131
    Figure BDA0004791490920000131
Patent Text Reader

Abstract

The invention discloses an impact-resistant semi-prefabricated polyurethane runway and a preparation method thereof. The method comprises the following steps: uniformly spreading and drying a base layer material to form a base layer; mixing polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate for reaction; adding 1,4-butanediol to continue the reaction; then adding carbon black and a pigment to mix uniformly to obtain a surface layer material; spraying the surface layer material on the surface of the base layer and drying the surface layer material; the surface of the modified filler contains active hydroxyl groups, which can participate in the prepolymer preparation process; the modified monomer contains a spirocyclic structure, which can increase the mechanical properties of the base layer material; the molecular chain contains a large number of disulfide bonds; when the runway is impacted, the disulfide bonds are broken by the impact to consume energy, thereby preventing the runway from being damaged; when the outdoor temperature rises, the broken disulfide bonds are restored; the three-dimensional polyhedral structure of silsesquioxane can form a core-shell structure with the polyurethane molecular chain, thereby further improving the impact resistance of the runway.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane composite material preparation, and in particular to an impact-resistant semi-prefabricated polyurethane runway and a preparation method thereof. Background Art

[0002] The plastic track is also called the all-weather track for athletics. It is composed of polyurethane prepolymer, mixed polyether, waste tire rubber, EPDM rubber particles or PU particles, pigments, additives, and fillers. The plastic track has the advantages of good flatness, high compressive strength, appropriate hardness and elasticity, anti-skid, wear resistance, good shock absorption, easy site maintenance, bright colors, and neat appearance. The stable physical properties are conducive to the speed and technology of athletes, effectively improving sports performance and reducing the rate of falls. At present, the methods of laying sports venues with polyurethane materials mainly include cast-in-place method and prefabrication method. The construction method of the cast-in-place method is to mix the various components of polyurethane and then pour them directly in the construction area, while the construction method of the prefabrication method is to pre-cure the polyurethane into a roll, and then use an adhesive to bond the roll to the construction area. The semi-prefabrication is a product that combines the advantages of the cast-in-place method and the prefabrication method. However, the existing polyurethane track has poor shock absorption effect, which causes excessive impact on the joints and muscles of athletes, increasing the possibility of fatigue and injury. Summary of the invention

[0003] The purpose of the present invention is to provide an impact-resistant semi-prefabricated polyurethane runway and a preparation method thereof, so as to solve the problem that the impact resistance of the current polyurethane runway is generally mediocre.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing an impact-resistant semi-prefabricated polyurethane runway comprises the following steps:

[0006] The base layer material is evenly spread and dried to form a base layer, polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate are mixed, and stirred at a speed of 120-150r / min and a temperature of 80-85°C, and dibutyltin dilaurate is added. After reacting for 3-4 hours, 1,4-butanediol is added, and the reaction is continued for 30-40 minutes. Carbon black and pigment are added and mixed evenly to obtain a surface layer material. The surface layer material is sprayed on the surface of the base layer and dried to obtain an impact-resistant semi-prefabricated polyurethane runway.

[0007] Furthermore, the dosage ratio of the polytetramethylene glycol, diphenylmethane diisocyanate, 1,4-butanediol, carbon black and pigment is 100mmol:500mmol:500mmol:20g:8g, and the polytetramethylene glycol is 2000.

[0008] Further, the base layer material is made by the following steps:

[0009] Step A1: 4,4'-dithiodiphenylamine, 1,2-epoxydodecane and DMF are mixed evenly, and reacted for 3-5 hours at a speed of 150-200 r / min, a temperature of 40-50° C. and a pH value of 10-11 to obtain intermediate 1; intermediate 1, terephthalaldehyde, p-toluenesulfonic acid and toluene are mixed evenly, and reacted for 5-7 hours at a speed of 60-80 r / min and a temperature of 110-120° C. to obtain intermediate 2;

[0010] Step A2: Intermediate 2, KH550 and DMF are mixed, and reacted for 3-5 hours at a speed of 200-300 r / min and a temperature of 40-50° C. to obtain intermediate 3. Intermediate 3, KH570 and tetrahydrofuran are mixed evenly, and stirred at a speed of 120-150 r / min and a temperature of 25-30° C., and ethanol and deionized water are added. After stirring for 3-5 minutes, hydrochloric acid solution is added, and the mixture is reacted for 3-4 days, and then the mixture is heated to 50-55° C. and aged for 2-3 days to obtain intermediate 4.

[0011] Step A3: Mix the intermediate 4, diethanolamine and DMF, stir and add sodium hydroxide at a speed of 150-200 r / min and a temperature of 30-40°C, react for 2-3 hours, adjust the pH to neutral, and obtain a modified monomer; mix the modified monomer, polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate, stir and add dibutyltin dilaurate and a modified filler at a speed of 120-150 r / min and a temperature of 80-85°C, react for 3-4 hours, add 1,4-butanediol, and continue to react for 30-40 minutes to obtain a base layer material.

[0012] Furthermore, the molar ratio of 4,4'-dithiodiphenylamine and 1,2-epoxydodecane in step A1 is 1:4, the molar ratio of intermediate 1 and terephthalaldehyde is n:n+1, n is a natural number greater than 0, and the amount of toluenesulfonic acid used is 1% of the mass of intermediate 1.

[0013] Furthermore, the molar ratio of intermediate 2 and KH550 described in step A2 is 1:2, the dosage ratio of intermediate 3, KH570, tetrahydrofuran, ethanol, deionized water and hydrochloric acid solution is 1 mmol: 5 mmol: 20 mL: 10 mL: 5 mL: 1 mL, and the concentration of hydrochloric acid solution is 0.2 mol / L.

[0014] Furthermore, the molar ratio of propenyl, diethanolamine and sodium hydroxide on the intermediate 4 described in step A3 is 1:1:3.1, the molar ratio of the modified monomer, polytetramethylene ether diol, diphenylmethane diisocyanate and 1,4-butanediol is 1:2:10:5, the amount of the modified filler is 15% of the total mass of the modified monomer, polytetramethylene ether diol, diphenylmethane diisocyanate and 1,4-butanediol, the amount of dibutyltin dilaurate is 2% of the mass of the modified monomer, and the molecular weight of polytetramethylene ether diol is 2000.

[0015] Further, the modified filler is prepared by the following steps:

[0016] Step B1: graphite oxide, KH550, dicyclohexylcarbodiimide and toluene are mixed, stirred for 1-1.5 hours at a speed of 150-200 r / min and a temperature of 30-40° C., and the filtrate is removed by filtering, the substrate is dispersed in anhydrous ethanol, methyltriethoxysilane, dimethyldiethoxysilane and KH560 are added, and deionized water is added at a speed of 120-150 r / min and a temperature of 65-70° C., and the mixture is stirred and deionized water is added. After reacting for 1-2 hours, tetrabutyl titanate is added, and the reaction is continued for 3-4 hours. The temperature is raised to 120-125° C. and the reaction is carried out for 3-5 hours to obtain modified graphite;

[0017] Step B2: The modified graphite, 2,2'-diamino-4,4'-bithiazole and DMF are mixed evenly, and reacted for 6-8 hours at a rotation speed of 150-200 r / min, a temperature of 40-50°C, and a pH value of 10-11 to obtain a precursor. The precursor, manganese chloride, DMF, DMA and deionized water are mixed evenly, and the mixture is heat-treated for 70-75 hours at a frequency of 20-30 kHz and a temperature of 100°C, and then the mixture is cooled to 25-30°C and heat-treated for 45-50 hours to obtain a pre-modified filler.

[0018] Furthermore, the amount of KH550 described in step B1 is 5% of the mass of graphite oxide, the molar ratio of KH550 to dicyclohexylcarbodiimide is 1:1.1, and the amount ratio of substrate, methyltriethoxysilane, dimethyldiethoxysilane, KH560, deionized water and tetrabutyl titanate is 1g:10mmo l:10mmo l:5mmo l:50mL:2mmo l.

[0019] Furthermore, the molar ratio of the epoxy group on the modified graphite and 2,2'-diamino-4,4'-bithiazole in step B2 is 2:1, and the amount ratio of the precursor, manganese chloride, DMF, DMA and deionized water is 1g:3g:5mL:5mL:20mL.

[0020] Beneficial effects of the present invention: The impact-resistant semi-prefabricated polyurethane runway disclosed by the present invention is prepared by evenly spreading and drying a base layer material to form a base layer, mixing polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate, stirring and adding dibutyltin dilaurate, reacting, adding 1,4-butanediol, continuing the reaction, adding carbon black and pigment and mixing evenly to obtain a surface layer material, spraying the surface layer material on the surface of the base layer and drying the surface layer material, wherein the base layer material is prepared by reacting 4,4'-dithiodiphenylamine and 1,2-epoxydodecane as raw materials under alkaline conditions, so that the amino group on the 4,4'-dithiodiphenylamine reacts with the epoxy group on the 1,2-epoxydodecane to form a new hydroxyl group, and the surface layer material is sprayed on the surface of the base layer and dried. Intermediate 1 and terephthalaldehyde are subjected to a diacetalization reaction, so that two aldehyde groups on one side of the intermediate 1 molecule react with an aldehyde group on terephthalaldehyde to obtain intermediate 2, intermediate 2 is reacted with KH550, so that the aldehyde group on intermediate 2 reacts with the amino group on KH550 to obtain intermediate 3, intermediate 3 and KH570 are hydrolyzed and condensed to form a bridged polysilsesquioxane containing a double bond, intermediate 4 is reacted with diethanolamine, so that the double bond on intermediate 4 reacts with the secondary amino group on diethanolamine to obtain a modified monomer, the modified monomer, polytetramethylene glycol and diphenylmethane diisocyanate are reacted, and then a modified filler is added and blended to form a prepolymer, and finally 1,4-butanediol is added to expand the prepolymer. The base layer material is made by chain. The surface of the modified filler contains active hydroxyl groups, which can participate in the prepolymer preparation process. At the same time, the spirocyclic structure on the modified monomer can increase the mechanical properties of the base layer material, and the molecular chain contains a large number of disulfide bonds. When the runway is impacted, the disulfide bonds are broken by the impact to consume energy, thereby preventing the runway from being damaged. When the outdoor temperature rises, the broken disulfide bonds will recover. Through the three-dimensional polyhedral structure of silsesquioxane, it can form a core-shell structure with the polyurethane molecular chain, further improving the impact resistance of the runway. The modified filler uses graphite oxide and KH550 as raw materials. Under the action of dicyclohexylcarbodiimide, the carboxyl groups on the surface of graphite oxide and the amino groups on KH550 are The dehydration reaction allows siloxane to be grafted onto the surface, which is then hydrolyzed and condensed with methyltriethoxysilane, dimethyldiethoxysilane, KH560 and tetrabutyl titanate to form a titanium-containing silicone resin-coated surface. At the same time, the surface contains epoxy groups. The modified graphite and 2,2'-diamino-4,4'-bithiazole are reacted under alkaline conditions to obtain a precursor. The precursor is reacted with manganese chloride to allow the thiazole on the precursor to complex with manganese ions, forming an organic framework of manganese before the precursor to obtain a modified filler. The modified filler is a hard-soft-hard impact-resistant sandwich structure that can absorb impact energy and form a multi-layer core-shell structure with polyurethane molecules. When compounded with modified monomers, it can greatly improve the impact resistance of the runway. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] A method for preparing an impact-resistant semi-prefabricated polyurethane runway comprises the following steps:

[0024] The base layer material is evenly spread and dried to form a base layer, polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate are mixed, and stirred at a speed of 120 r / min and a temperature of 80°C, and dibutyltin dilaurate is added. After reacting for 3 hours, 1,4-butanediol is added and the reaction is continued for 30 minutes. Carbon black and pigment are added and mixed evenly to obtain a surface layer material. The surface layer material is sprayed on the surface of the base layer and dried to obtain an impact-resistant semi-prefabricated polyurethane runway.

[0025] The dosage ratio of the polytetramethylene glycol, diphenylmethane diisocyanate, 1,4-butanediol, carbon black and pigment is 100mmol:500mmol:500mmol:20g:8g, and the dosage ratio of the polytetramethylene glycol is 2000.

[0026] The base layer material is made by the following steps:

[0027] Step A1: 4,4'-dithiodiphenylamine, 1,2-epoxydodecane and DMF were mixed evenly, and reacted for 3 hours at a speed of 150 r / min, a temperature of 40° C. and a pH value of 10 to obtain intermediate 1; intermediate 1, terephthalaldehyde, p-toluenesulfonic acid and toluene were mixed evenly, and reacted for 5 hours at a speed of 60 r / min and a temperature of 110° C. to obtain intermediate 2;

[0028] Step A2: Intermediate 2, KH550 and DMF were mixed, and reacted at a speed of 200 r / min and a temperature of 40°C for 3 hours to obtain intermediate 3. Intermediate 3, KH570 and tetrahydrofuran were mixed evenly, and stirred at a speed of 120 r / min and a temperature of 25°C, and ethanol and deionized water were added. After stirring for 3 minutes, hydrochloric acid solution was added, and the mixture was reacted for 3 days, and then the mixture was heated to 50°C and aged for 2 days to obtain intermediate 4.

[0029] Step A3: Mix the intermediate 4, diethanolamine and DMF, stir and add sodium hydroxide at a speed of 150 r / min and a temperature of 30°C, react for 2 hours, adjust the pH to neutral, and obtain a modified monomer; mix the modified monomer, polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate, stir and add dibutyltin dilaurate and a modified filler at a speed of 120 r / min and a temperature of 80°C, react for 3 hours, add 1,4-butanediol, and continue to react for 30 minutes to obtain a base layer material.

[0030] The molar ratio of 4,4'-dithiodiphenylamine and 1,2-epoxydodecane in step A1 is 1:4, the molar ratio of intermediate 1 and terephthalaldehyde is 1:2, and the amount of toluenesulfonic acid used is 1% of the mass of intermediate 1.

[0031] The molar ratio of intermediate 2 and KH550 described in step A2 is 1:2, the dosage ratio of intermediate 3, KH570, tetrahydrofuran, ethanol, deionized water and hydrochloric acid solution is 1mmol:5mmol:20mL:10mL:5mL:1mL, and the concentration of hydrochloric acid solution is 0.2mol / L.

[0032] The molar ratio of propenyl, diethanolamine and sodium hydroxide on the intermediate 4 described in step A3 is 1:1:3.1, the molar ratio of the modified monomer, polytetramethylene ether diol, diphenylmethane diisocyanate and 1,4-butanediol is 1:2:10:5, the amount of the modified filler is 15% of the total mass of the modified monomer, polytetramethylene ether diol, diphenylmethane diisocyanate and 1,4-butanediol, the amount of dibutyltin dilaurate is 2% of the mass of the modified monomer, and the molecular weight of polytetramethylene ether diol is 2000.

[0033] The modified filler is prepared by the following steps:

[0034] Step B1: Graphite oxide, KH550, dicyclohexylcarbodiimide and toluene are mixed, stirred at a speed of 150 r / min and a temperature of 30°C for 1 hour, and the filtrate is removed by filtering, the substrate is dispersed in anhydrous ethanol, methyltriethoxysilane, dimethyldiethoxysilane and KH560 are added, stirred at a speed of 120 r / min and a temperature of 65°C, and deionized water is added, and the reaction is carried out for 1 hour, and tetrabutyl titanate is added, and the reaction is continued for 3 hours, and the temperature is raised to 120°C and the reaction is carried out for 3 hours to obtain modified graphite;

[0035] Step B2: The modified graphite, 2,2'-diamino-4,4'-bithiazole and DMF are mixed evenly, and reacted for 6 hours at a speed of 150 r / min, a temperature of 40°C and a pH value of 10 to obtain a precursor. The precursor, manganese chloride, DMF, DMA and deionized water are mixed evenly, and heat-treated for 70 hours at a frequency of 20 kHz and a temperature of 100°C, and then cooled to 25°C and kept warm for 45 hours to obtain a pre-modified filler.

[0036] The amount of KH550 described in step B1 is 5% of the mass of graphite oxide, the molar ratio of KH550 to dicyclohexylcarbodiimide is 1:1.1, and the amount ratio of substrate, methyltriethoxysilane, dimethyldiethoxysilane, KH560, deionized water and tetrabutyl titanate is 1g:10mmo l:10mmo l:5mmo l:50mL:2mmo l.

[0037] The molar ratio of the epoxy group on the modified graphite and 2,2'-diamino-4,4'-bithiazole described in step B2 is 2:1, and the amount ratio of the precursor, manganese chloride, DMF, DMA and deionized water is 1g:3g:5mL:5mL:20mL.

[0038] Example 2

[0039] A method for preparing an impact-resistant semi-prefabricated polyurethane runway comprises the following steps:

[0040] The base layer material is evenly spread and dried to form a base layer, polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate are mixed, and stirred at a speed of 120 r / min and a temperature of 85°C, and dibutyltin dilaurate is added. After reacting for 3.5 hours, 1,4-butanediol is added and the reaction is continued for 35 minutes. Carbon black and pigment are added and mixed evenly to obtain a surface layer material. The surface layer material is sprayed on the surface of the base layer and dried to obtain an impact-resistant semi-prefabricated polyurethane runway.

[0041] The dosage ratio of the polytetramethylene glycol, diphenylmethane diisocyanate, 1,4-butanediol, carbon black and pigment is 100mmol:500mmol:500mmol:20g:8g, and the dosage ratio of the polytetramethylene glycol is 2000.

[0042] The base layer material is made by the following steps:

[0043] Step A1: 4,4'-dithiodiphenylamine, 1,2-epoxydodecane and DMF were mixed evenly, and the mixture was reacted for 4 hours at a speed of 150 r / min, a temperature of 45°C and a pH value of 11 to obtain intermediate 1; intermediate 1, terephthalaldehyde, p-toluenesulfonic acid and toluene were mixed evenly, and the mixture was reacted for 6 hours at a speed of 60 r / min and a temperature of 115°C to obtain intermediate 2;

[0044] Step A2: Intermediate 2, KH550 and DMF were mixed, and reacted at a speed of 200 r / min and a temperature of 45°C for 4 hours to obtain intermediate 3. Intermediate 3, KH570 and tetrahydrofuran were mixed evenly, and stirred at a speed of 120 r / min and a temperature of 28°C, and ethanol and deionized water were added. After stirring for 4 minutes, hydrochloric acid solution was added, and the mixture was reacted for 4 days, and then the mixture was heated to 50°C and aged for 3 days to obtain intermediate 4.

[0045] Step A3: Mix the intermediate 4, diethanolamine and DMF, stir and add sodium hydroxide at a speed of 150 r / min and a temperature of 35°C, react for 3 hours, adjust the pH to neutral, and obtain a modified monomer; mix the modified monomer, polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate, stir and add dibutyltin dilaurate and a modified filler at a speed of 120 r / min and a temperature of 85°C, react for 4 hours, add 1,4-butanediol, and continue to react for 35 minutes to obtain a base layer material.

[0046] The molar ratio of 4,4'-dithiodiphenylamine and 1,2-epoxydodecane in step A1 is 1:4, the molar ratio of intermediate 1 and terephthalaldehyde is 2:3, and the amount of toluenesulfonic acid used is 1% of the mass of intermediate 1.

[0047] The molar ratio of intermediate 2 and KH550 described in step A2 is 1:2, the dosage ratio of intermediate 3, KH570, tetrahydrofuran, ethanol, deionized water and hydrochloric acid solution is 1mmol:5mmol:20mL:10mL:5mL:1mL, and the concentration of hydrochloric acid solution is 0.2mol / L.

[0048] The molar ratio of propenyl, diethanolamine and sodium hydroxide on the intermediate 4 described in step A3 is 1:1:3.1, the molar ratio of the modified monomer, polytetramethylene ether diol, diphenylmethane diisocyanate and 1,4-butanediol is 1:2:10:5, the amount of the modified filler is 15% of the total mass of the modified monomer, polytetramethylene ether diol, diphenylmethane diisocyanate and 1,4-butanediol, the amount of dibutyltin dilaurate is 2% of the mass of the modified monomer, and the molecular weight of polytetramethylene ether diol is 2000.

[0049] The modified filler is prepared by the following steps:

[0050] Step B1: Graphite oxide, KH550, dicyclohexylcarbodiimide and toluene are mixed, stirred at a speed of 150 r / min and a temperature of 35°C for 1.5 hours, and the filtrate is removed by filtering, the substrate is dispersed in anhydrous ethanol, methyltriethoxysilane, dimethyldiethoxysilane and KH560 are added, and deionized water is added under the conditions of a speed of 120 r / min and a temperature of 68°C, and the mixture is stirred and deionized water is added. After reacting for 2 hours, tetrabutyl titanate is added, and the reaction is continued for 4 hours. The temperature is raised to 120°C and the reaction is carried out for 4 hours to obtain modified graphite;

[0051] Step B2: The modified graphite, 2,2'-diamino-4,4'-bithiazole and DMF are mixed evenly, and reacted for 7 hours at a speed of 150 r / min, a temperature of 45°C and a pH value of 11 to obtain a precursor. The precursor, manganese chloride, DMF, DMA and deionized water are mixed evenly, and heat-treated for 75 hours at a frequency of 25 kHz and a temperature of 100°C, and then cooled to 28°C and kept warm for 45 hours to obtain a pre-modified filler.

[0052] The amount of KH550 described in step B1 is 5% of the mass of graphite oxide, the molar ratio of KH550 to dicyclohexylcarbodiimide is 1:1.1, and the amount ratio of substrate, methyltriethoxysilane, dimethyldiethoxysilane, KH560, deionized water and tetrabutyl titanate is 1g:10mmo l:10mmo l:5mmo l:50mL:2mmo l.

[0053] The molar ratio of the epoxy group on the modified graphite and 2,2'-diamino-4,4'-bithiazole described in step B2 is 2:1, and the amount ratio of the precursor, manganese chloride, DMF, DMA and deionized water is 1g:3g:5mL:5mL:20mL.

[0054] Example 3

[0055] A method for preparing an impact-resistant semi-prefabricated polyurethane runway comprises the following steps:

[0056] The base layer material is evenly spread and dried to form a base layer, polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate are mixed, and stirred at a speed of 150 r / min and a temperature of 85°C, and dibutyltin dilaurate is added. After reacting for 4 hours, 1,4-butanediol is added and the reaction is continued for 40 minutes. Carbon black and pigment are added and mixed evenly to obtain a surface layer material. The surface layer material is sprayed on the surface of the base layer and dried to obtain an impact-resistant semi-prefabricated polyurethane runway.

[0057] The dosage ratio of the polytetramethylene glycol, diphenylmethane diisocyanate, 1,4-butanediol, carbon black and pigment is 100mmol:500mmol:500mmol:20g:8g, and the dosage ratio of the polytetramethylene glycol is 2000.

[0058] The base layer material is made by the following steps:

[0059] Step A1: 4,4'-dithiodiphenylamine, 1,2-epoxydodecane and DMF were mixed evenly, and reacted for 5 hours at a speed of 200 r / min, a temperature of 50° C. and a pH value of 11 to obtain intermediate 1; intermediate 1, terephthalaldehyde, p-toluenesulfonic acid and toluene were mixed evenly, and reacted for 7 hours at a speed of 80 r / min and a temperature of 120° C. to obtain intermediate 2;

[0060] Step A2: Intermediate 2, KH550 and DMF were mixed, and reacted at a speed of 300 r / min and a temperature of 50° C. for 5 h to obtain intermediate 3. Intermediate 3, KH570 and tetrahydrofuran were mixed evenly, and stirred at a speed of 150 r / min and a temperature of 30° C., and ethanol and deionized water were added. After stirring for 5 min, hydrochloric acid solution was added, and the mixture was reacted for 4 days, and then the mixture was heated to 55° C. and aged for 3 days to obtain intermediate 4.

[0061] Step A3: Mix the intermediate 4, diethanolamine and DMF, stir and add sodium hydroxide at a speed of 200 r / min and a temperature of 40°C, react for 3 hours, adjust the pH to neutral, and obtain a modified monomer; mix the modified monomer, polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate, stir and add dibutyltin dilaurate and a modified filler at a speed of 150 r / min and a temperature of 85°C, react for 4 hours, add 1,4-butanediol, and continue to react for 40 minutes to obtain a base layer material.

[0062] The molar ratio of 4,4'-dithiodiphenylamine and 1,2-epoxydodecane in step A1 is 1:4, the molar ratio of intermediate 1 and terephthalaldehyde is 3:4, and the amount of toluenesulfonic acid used is 1% of the mass of intermediate 1.

[0063] The molar ratio of intermediate 2 and KH550 described in step A2 is 1:2, the dosage ratio of intermediate 3, KH570, tetrahydrofuran, ethanol, deionized water and hydrochloric acid solution is 1mmol:5mmol:20mL:10mL:5mL:1mL, and the concentration of hydrochloric acid solution is 0.2mol / L.

[0064] The molar ratio of propenyl, diethanolamine and sodium hydroxide on the intermediate 4 described in step A3 is 1:1:3.1, the molar ratio of the modified monomer, polytetramethylene ether diol, diphenylmethane diisocyanate and 1,4-butanediol is 1:2:10:5, the amount of the modified filler is 15% of the total mass of the modified monomer, polytetramethylene ether diol, diphenylmethane diisocyanate and 1,4-butanediol, the amount of dibutyltin dilaurate is 2% of the mass of the modified monomer, and the molecular weight of polytetramethylene ether diol is 2000.

[0065] The modified filler is prepared by the following steps:

[0066] Step B1: Graphite oxide, KH550, dicyclohexylcarbodiimide and toluene are mixed, stirred at a speed of 200 r / min and a temperature of 40°C for 1.5 hours, and the filtrate is removed by filtering, the substrate is dispersed in anhydrous ethanol, methyltriethoxysilane, dimethyldiethoxysilane and KH560 are added, and deionized water is added under the conditions of a speed of 150 r / min and a temperature of 70°C, and the mixture is stirred and deionized water is added. After reacting for 2 hours, tetrabutyl titanate is added, and the reaction is continued for 4 hours. The temperature is raised to 125°C and the reaction is carried out for 5 hours to obtain modified graphite;

[0067] Step B2: The modified graphite, 2,2'-diamino-4,4'-bithiazole and DMF are mixed evenly, and reacted for 8 hours at a speed of 200 r / min, a temperature of 50°C and a pH value of 11 to obtain a precursor. The precursor, manganese chloride, DMF, DMA and deionized water are mixed evenly, and heat-treated for 75 hours at a frequency of 30 kHz and a temperature of 100°C, and then cooled to 30°C and kept warm for 50 hours to obtain a pre-modified filler.

[0068] The amount of KH550 described in step B1 is 5% of the mass of graphite oxide, the molar ratio of KH550 to dicyclohexylcarbodiimide is 1:1.1, and the amount ratio of substrate, methyltriethoxysilane, dimethyldiethoxysilane, KH560, deionized water and tetrabutyl titanate is 1g:10mmo l:10mmo l:5mmo l:50mL:2mmo l.

[0069] The molar ratio of the epoxy group on the modified graphite and 2,2'-diamino-4,4'-bithiazole described in step B2 is 2:1, and the amount ratio of the precursor, manganese chloride, DMF, DMA and deionized water is 1g:3g:5mL:5mL:20mL.

[0070] Comparative Example 1

[0071] Compared with Example 1, no modified monomer was added in this comparative example, and the remaining steps were the same.

[0072] Comparative Example 2

[0073] Compared with Example 1, no modified filler was added in this comparative example, and the remaining steps were the same.

[0074] Comparative Example 3

[0075] Compared with Example 1, this comparative example uses graphite oxide instead of the modified filler, and the other steps are the same.

[0076] Comparative Example 4

[0077] Compared with Example 1, this comparative example uses graphite oxide, KH550, dicyclohexylcarbodiimide and toluene to mix, stir for 1 hour at a speed of 150 r / min and a temperature of 30°C, filter and remove the filtrate, disperse the substrate in anhydrous ethanol, add methyltriethoxysilane and dimethyldiethoxysilane, stir and add deionized water at a speed of 120 r / min and a temperature of 65°C, react for 1 hour, add tetrabutyl titanate, continue to react for 3 hours, heat to 120°C, and react for 3 hours. The obtained product replaces the modified filler.

[0078] The polyurethane runways prepared in Examples 1-3 and Comparative Examples 1-4 were cut into 300 mm × 300 mm × 0.2 mm, with a thickness ratio of the base layer to the fabric layer of 3:1. The impact absorption rate and tensile strength were tested in accordance with the standard of GB36246-2018, and the test results are shown in the following table.

[0079]

[0080]

[0081] It can be seen from the above table that the impact absorption rate of the polyurethane runway prepared in Examples 1-3 is 48.9-51.3%, and the tensile strength is 2.03-2.14 MPa, the impact absorption rate of Comparative Example 1 is 41.3%, and the tensile strength is 1.54 MPa, the impact absorption rate of Comparative Example 2 is 35.2%, and the tensile strength is 0.88 MPa, the impact absorption rate of Comparative Example 3 is 36.7%, and the tensile strength is 1.32 MPa, and the impact absorption rate of Comparative Example 4 is 39.3, and the tensile strength is 1.47 MPa, indicating that the present invention has a good impact resistance effect.

[0082] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing an impact-resistant semi-prefabricated polyurethane runway, characterized in that: The specific steps include: The base layer material is evenly spread and dried to form a base layer, polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate are mixed, stirred and dibutyltin dilaurate is added, and after reaction, 1,4-butanediol is added and the reaction is continued, and carbon black and pigment are added and mixed evenly to obtain a surface layer material, and the surface layer material is sprayed on the surface of the base layer and dried to obtain an impact-resistant semi-prefabricated polyurethane runway; The base layer material is made by the following steps: Step A1: 4,4'-dithiodiphenylamine, 1,2-epoxydodecane and DMF are mixed for reaction to obtain intermediate 1, and intermediate 1, terephthalaldehyde, p-toluenesulfonic acid and toluene are mixed for reaction to obtain intermediate 2; Step A2: intermediate 2, KH550 and DMF are mixed and reacted to obtain intermediate 3, intermediate 3, KH570 and tetrahydrofuran are mixed and stirred, and ethanol and deionized water are added, after stirring, hydrochloric acid solution is added, reacted, and then heated and aged to obtain intermediate 4; Step A3: The intermediate 4, diethanolamine and DMF are mixed and stirred, and sodium hydroxide is added. After reaction, the pH is adjusted to be neutral to obtain a modified monomer. The modified monomer, polytetramethylene glycol, diphenylmethane diisocyanate and ethyl acetate are mixed and stirred, and dibutyltin dilaurate and a modified filler are added. After reaction, 1,4-butanediol is added, and the reaction is continued to obtain a base layer material; The modified filler is prepared by the following steps: Step B1: After graphite oxide, KH550, dicyclohexylcarbodiimide and toluene are mixed and stirred, the filtrate is removed by filtering, the substrate is dispersed in anhydrous ethanol, methyltriethoxysilane, dimethyldiethoxysilane and KH560 are added, stirred and deionized water is added, tetrabutyl titanate is added, the reaction is continued, and the temperature is raised to react to obtain modified graphite; Step B2: mixing modified graphite, 2,2'-diamino-4,4'-bithiazole and DMF to obtain a precursor, and mixing the precursor, manganese chloride, DMF, DMA and deionized water for heat treatment to obtain a modified filler; The amount ratio of the polytetramethylene glycol, diphenylmethane diisocyanate, 1,4-butanediol, carbon black and pigment is 100mmol:500mmol:500mmol:20g:8g; The molar ratio of 4,4'-dithiodiphenylamine and 1,2-epoxydodecane in step A1 is 1:4, and the molar ratio of intermediate 1 and terephthalaldehyde is n:n+1, where n is 1, 2 or 3; The molar ratio of intermediate 2 and KH550 in step A2 is 1:2, and the amount ratio of intermediate 3, KH570, tetrahydrofuran, ethanol, deionized water and hydrochloric acid solution is 1mmol:5mmol:20mL:10mL:5mL:1mL; The molar ratio of propenyl, diethanolamine and sodium hydroxide on the intermediate 4 described in step A3 is 1:1:3.1, the molar ratio of the modified monomer, polytetramethylene glycol, diphenylmethane diisocyanate and 1,4-butanediol is 1:2:10:5, and the amount of the modified filler is 15% of the total mass of the modified monomer, polytetramethylene glycol, diphenylmethane diisocyanate and 1,4-butanediol; The amount of KH550 in step B1 is 5% of the mass of graphite oxide, the molar ratio of KH550 to dicyclohexylcarbodiimide is 1:1.1, and the amount ratio of substrate, methyltriethoxysilane, dimethyldiethoxysilane, KH560, deionized water and tetrabutyl titanate is 1g:10mmol:10mmol:5mmol:50mL:2mmol; The molar ratio of the epoxy group on the modified graphite and 2,2'-diamino-4,4'-bithiazole described in step B2 is 2:1, and the amount ratio of the precursor, manganese chloride, DMF, DMA and deionized water is 1g:3g:5mL:5mL:20mL.

2. An impact-resistant semi-prefabricated polyurethane runway, characterized in that: Prepared according to the preparation method according to claim 1.