Keratin-based biological adhesive prepared from waste feathers and preparation method of keratin-based biological adhesive
Through hydrolysis and oxidative modification of waste feathers, the pollution problems caused by low molecular entanglement and chemical modification of keratin bio-based adhesives are solved, and high-strength and environmentally friendly keratin-based adhesives are prepared, realizing waste resources Chemical utilization and wide application of adhesives.
Patent Information
- Application Number
- CN202411153020.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
AI Technical Summary
When existing keratin bio-based adhesives are self-assembled into crosslinked network structures, their molecular entanglement is low and their cohesion is poor, which limits their development as bio-based adhesives. Common chemical modification methods can cause environmental pollution or human body. harm.
By hydrolyzing and oxidatively modifying the waste feathers, using green and low concentrations of hydrogen peroxide to recombinantly cross-link the disulfide bonds of keratin, a high-strength, long-acting keratin-based adhesive is prepared, avoiding chemical modification reagents Use of
The resource utilization of waste has been realized, and economical, environmentally friendly, renewable and degradable multifunctional adhesives have been prepared, with a wide range of industrial application prospects and improved the strength and stability of the adhesive.
Smart Images

Figure CN118931492A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of keratin bio-based adhesives, and in particular to a keratin-based bio-adhesive prepared by utilizing waste feathers and a preparation method thereof. Background Art
[0002] Keratin is an abundant natural polymer protein that is widely found in tissues such as feathers, hair, and nails. Keratin forms β-pleated sheets and α-helical structures, which are stabilized by intermolecular and intramolecular disulfide bonds, giving the material a high strength and stable structure. Breaking the disulfide bonds releases cysteine residues, which can re-establish cross-linking to form different derivative materials. Therefore, the development of keratin-derived materials as biomass adhesives has considerable economic and environmental benefits. However, current studies have shown that keratin cannot self-assemble into a cross-linked network structure through protein domain interactions, resulting in low molecular entanglement and poor cohesion, which greatly limits its development as a bio-based adhesive. In addition, recently developed keratin-based adhesives require many chemical cross-linkers during the production process.
[0003] In response to this problem, researchers have begun to explore ways to enhance the performance of keratin through chemical modification. Common chemical modification methods include aldehyde cross-linking, enzyme treatment, and graft copolymerization. These modifications can not only improve the solubility and processability of keratin, but also significantly improve its mechanical properties and bonding properties, thereby broadening its application in the field of industrial adhesives. However, these modification agents can cause environmental pollution or harm to the human body. Therefore, current research focuses on the development of efficient and environmentally friendly chemical modification strategies, as well as systematic evaluation of the performance of modified keratin adhesives. Summary of the invention
[0004] The invention aims to provide a keratin-based biological adhesive prepared by utilizing waste feathers and a preparation method thereof.
[0005] In order to achieve the above experimental objectives, the present invention provides the following technical solutions:
[0006] A method for preparing a keratin-based biomass adhesive using waste feathers of the present invention comprises the following steps:
[0007] A. Washing, drying and chopping discarded feathers to obtain pre-treated feather fragments;
[0008] B. hydrolyzing the feather fragments obtained in step A, filtering, washing, and drying to obtain keratin;
[0009] C. The keratin obtained in step B is subjected to oxidative modification to cause its disulfide bonds to undergo reorganization and cross-linking, thereby preparing an adhesive.
[0010] Preferably, the oxidative modification in step C is performed using a hydrogen peroxide solution. Further preferably, the concentration of the hydrogen peroxide solution is 0.1-5% by mass.
[0011] Preferably, the ratio of keratin to hydrogen peroxide solution is 3 g:0.9 g to 1.8 g, preferably 3 g:0.9 g, and the mass fraction of hydrogen peroxide solution is 1%.
[0012] Preferably, the feathers in step A are one or more of chicken feathers, duck feathers, and goose feathers.
[0013] Preferably, the hydrolysis method in step B is alkaline hydrolysis, and the reagent is one or more of potassium hydroxide, sodium hydroxide, sodium ethoxide, urea, sodium dodecyl sulfate, and sodium metabisulfite.
[0014] Preferably, the concentration of the feather fragments in step B is 10-50 g / L, and the concentration of the alkaline hydrolysis agent is 50-400 g / L.
[0015] Preferably, 5 g of hair fragments are hydrolyzed with 5 g of sodium metabisulfite, 9 g of sodium lauryl sulfate and 40 g of urea dissolved in 100 ml of water.
[0016] Preferably, the hydrolysis temperature in step B is 70-100°C and the hydrolysis time is 1-3 hours. More preferably, the temperature is 70°C and the modification time is 2 hours.
[0017] Preferably, the adhesive prepared according to the above method can be used for preparing plywood.
[0018] Compared with the existing technology, the beneficial effects of the present invention are:
[0019] 1. The present invention uses waste feathers as raw materials to prepare functional material adhesives, which not only makes resource utilization of waste, but also has a wide range of applications in aerospace, construction, home furnishing, packaging and other industries, and has good industrial development prospects.
[0020] 2. The present invention avoids the harm caused by chemical modification reagents and utilizes green low-concentration hydrogen peroxide to cause disulfide bonds to undergo reorganization and cross-linking, thus having novelties in material collection and processing.
[0021] 3. The preparation process of the present invention is simple, and the obtained adhesive is not only economical and environmentally friendly, but also renewable and degradable, and has a good industrial application prospect.
[0022] The present invention uses green modification reagents to form new disulfide bonds between the thiol groups of keratin chains, forming a cross-linked network structure in the synthetic adhesive system, aiming to develop a multifunctional keratin-based adhesive with high strength and long-lasting adhesive properties. The present invention uses molecular oxidation modification and compounding to be an effective method for preparing functional adhesives, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the process diagram of adhesive preparation
[0024] Figure 2 The SEM images of the adhesives of Comparative Example 1 (A) and Example 1 (B) are shown in FIG.
[0025] Figure 3 The XPS spectra of S2p of keratin adhesive comparative example 1 (A) and example 1 (B) (proving that keratin disulfide bonds undergo reorganization and cross-linking) DETAILED DESCRIPTION
[0026] In order to make the contents of the present invention easier to understand, the scheme of the present invention is further described below in conjunction with specific implementation methods.
[0027] Example 1
[0028] 1) Cleaning, drying and chopping the discarded duck feathers to obtain pre-treated hair fragments;
[0029] 2) Measure 100 mL of deionized water, add 5 g of sodium metabisulfite, 9 g of sodium dodecyl sulfate and 40 g of urea, stir evenly to prepare an alkaline solution;
[0030] 3) Weigh 5 g of the hair fragments obtained in step 1) and add them to the alkali solution prepared in step 2), and place them in a 70° C. water bath and heat and stir for 2 h.
[0031] 4) filtering the hydrolyzate obtained in step 3) to obtain a viscous keratin hydrolyzate, and then freeze-drying the keratin hydrolyzate to obtain keratin powder; 5) weighing 3 g of the keratin powder obtained in step 4) and mixing it with 0.9 mL of a 1% by mass hydrogen peroxide solution,
[0032] Adhesive 1 was prepared.
[0033] Example 2
[0034] 1) Cleaning, drying and chopping the discarded duck feathers to obtain pre-treated hair fragments;
[0035] 2) Measure 100 mL of deionized water, add 5 g of sodium metabisulfite, 9 g of sodium dodecyl sulfate and 40 g of urea, stir evenly to prepare an alkaline solution;
[0036] 3) Weigh 5 g of the hair fragments obtained in step 1) and add them to the alkali solution prepared in step 2), and place them in a 70° C. water bath and heat and stir for 2 h.
[0037] 4) filtering the hydrolyzate obtained in step 3) to obtain a viscous keratin hydrolyzate, and then freeze-drying the keratin hydrolyzate to obtain keratin powder; 5) weighing 3 g of the keratin powder obtained in step 4) and mixing it with 0.9 mL of a 5% by mass hydrogen peroxide solution to prepare an adhesive 2.
[0038] Example 3
[0039] 1) Cleaning, drying and chopping the discarded duck feathers to obtain pre-treated hair fragments;
[0040] 2) Measure 100 mL of deionized water, add 5 g of sodium metabisulfite, 9 g of sodium dodecyl sulfate and 40 g of urea, stir evenly to prepare an alkaline solution;
[0041] 3) Weigh 5 g of the hair fragments obtained in step 1) and add them to the alkali solution prepared in step 2), and place them in a 70° C. water bath and heat and stir for 2 h.
[0042] 4) filtering the hydrolyzate obtained in step 3) to obtain a viscous keratin hydrolyzate, and then freeze-drying the keratin hydrolyzate to obtain keratin powder; 5) weighing 3 g of the keratin powder obtained in step 4) and mixing it with 1.8 mL of a 5% by mass hydrogen peroxide solution to prepare an adhesive 3.
[0043] Comparative Example 1
[0044] 1) Cleaning, drying and chopping the discarded duck feathers to obtain pre-treated hair fragments;
[0045] 2) Measure 100 mL of deionized water, add 5 g of sodium metabisulfite, 9 g of sodium dodecyl sulfate and 40 g of urea, stir evenly to prepare an alkaline solution;
[0046] 3) Weigh 5 g of the hair fragments obtained in step 1) and add them to the alkali solution prepared in step 2), and place them in a 70° C. water bath and heat and stir for 2 h.
[0047] 4) filtering the hydrolyzate obtained in step 3) to obtain a viscous keratin hydrolyzate, and then freeze-drying the hydrolyzate to obtain keratin powder; 5) weighing 3 g of the keratin powder obtained in step 4) and mixing it with 0.9 mL of water to prepare an adhesive 4.
[0048] Performance Testing
[0049] 1. Experimental Methods
[0050] The bonding strength of plywood is an important indicator for evaluating adhesives. The method for measuring the bonding strength of plywood prepared by the adhesive obtained by the present invention is based on the scheme of the national standard GB / T 17657-2013 "Experimental methods for physical and chemical properties of artificial boards and veneer artificial boards". A poplar board with a size of 200mm×200mm×1.6mm is selected, coated with glue to form a three-layer board, and then placed in a hot press for hot pressing according to conditions to obtain an environmentally friendly plywood. It is sheared according to the standard (contact area 25mm×25mm), and then its bonding strength is tested with a universal tensile machine. Each sample is repeated 5 times to confirm the repeatability of the bonding strength data.
[0051] 2. Experimental results
[0052] like Figure 1 , 2 , 3 and the following table show that hydrolyzed keratin can be prepared into adhesive, but the adhesive strength is not high (Comparative Example 1), which does not meet the national standard of 0.7MPa. After it is oxidized and modified with hydrogen peroxide, the disulfide bonds between molecules are reorganized and cross-linked, and the adhesive strength is greatly improved (Examples 1-3), but with the increase of the amount of oxidant (Example 3) and concentration (Example 2), the cross-linking strength is partially destroyed, affecting the bonding strength, so compared with Example 1, the bonding strength of Examples 2 and 3 is reduced.
[0053] serial number Example 1 Example 2 Example 3 Comparative Example 1 Bonding strength (MPa) 2.3 1.5 1.2 0.65
[0054] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing a keratin-based biomass adhesive using waste feathers, characterized in that: The steps include: A. Washing, drying and chopping discarded feathers to obtain pre-treated feather fragments; B. hydrolyzing the feather fragments obtained in step A, filtering, washing, and drying to obtain keratin; C. The keratin obtained in step B is subjected to oxidative modification to cause its disulfide bonds to undergo reorganization and cross-linking, thereby preparing an adhesive.
2. The method according to claim 1, characterized in that: The oxidative modification in step C is performed using a hydrogen peroxide solution; more preferably, the concentration of the hydrogen peroxide solution is 0.1-5% by mass.
3. The method according to claim 2, characterized in that The usage ratio of keratin to hydrogen peroxide solution is 3g:0.9g-1.8g, preferably 3g:0.9g, and the mass fraction of hydrogen peroxide solution is 1%.
4. The method according to claim 1, characterized in that: The feathers in step A are one or more of chicken feathers, duck feathers and goose feathers.
5. The method according to claim 1, characterized in that The hydrolysis method in step B is alkaline hydrolysis, and the reagent is one or more of potassium hydroxide, sodium hydroxide, sodium ethoxide, urea, sodium dodecyl sulfate, and sodium metabisulfite.
6. The method according to claim 1, characterized in that In step B, the concentration of the feather fragments is 10-50 g / L, and the concentration of the alkaline hydrolysis agent is 50-400 g / L.
7. The method according to claim 1, characterized in that Every 5 g of hair fragments were hydrolyzed with 5 g of sodium metabisulfite, 9 g of sodium dodecyl sulfate and 40 g of urea dissolved in 100 ml of water.
8. The method according to claim 1, characterized in that The hydrolysis temperature in step B is 70-100° C. and the hydrolysis time is 1-3 h.
9. The method according to claim 8, characterized in that The hydrolysis temperature in step B is 70° C. and the hydrolysis time is 2 h.
10. An adhesive prepared according to any method of claims 1-9.
Citation Information
Cited By
Preparation method of protein amido straw cellulose salt-absorbing and water-retaining composite material
CN121064644A
A preparation method of a protein amide-based straw cellulose salt-absorbing and water-retaining composite material
NL4000302A