Continuous casting method for narrow-gauge medium-thick plates
By determining the target plate width to be twice the width of the sheet metal and optimizing the cooling method, the problem of difficult welding when producing narrow-specification medium-thick plates using the multiple-size slitting method was solved, thereby improving production efficiency and yield.
Patent Information
- Application Number
- CN202410353226.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Existing technologies, when producing narrow-gauge medium-thick plates, suffer from welding difficulties due to the use of multiple-length splitting methods.
By determining that the desired width of the target plate is less than or equal to 1800 mm, the width of the mother plate is determined to be twice the width of the target plate, and the billet shape of the continuous casting slab is determined based on the twice the width. The water distribution in the secondary cooling spray zone is adjusted to increase the non-uniform solidification area, and the cooling method is optimized to reduce center segregation.
It improved production efficiency and yield, reduced the amount of trimming, and solved the problem of difficult welding.
Smart Images

Figure CN118305290B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of continuous casting in iron and steel metallurgy, and more particularly to a method for casting narrow-gauge medium-thick plates using continuous casting. Background Technology
[0002] Currently, the demand for narrow-gauge medium-thick plates is increasing. Steel companies are using narrow-section continuous slabs to directly roll out narrow-gauge medium-thick plates, and then cut them according to length requirements. However, the current production method still suffers from low efficiency. Summary of the Invention
[0003] In view of the above problems, the present invention provides a method for casting narrow-gauge medium-thick plates by continuous casting, the main purpose of which is to solve the problem of difficult welding caused by the current method of producing narrow-gauge plates by multiple-length splitting.
[0004] To solve at least one of the above-mentioned technical problems, in a first aspect, the present invention provides a method for casting a continuous casting slab of a narrow-gauge medium-thick plate, the method comprising:
[0005] Determine the desired width of the target board material, wherein the desired width is less than or equal to 1800 mm;
[0006] The width of the motherboard is determined based on the desired width of the target board, wherein the width of the motherboard is twice the width of the target board.
[0007] The billet shape of the continuously cast slab is determined based on the aforementioned multiple-length width.
[0008] Optionally, the above method further includes: cutting the mother board using a multiple-scale slitting method to obtain the target board.
[0009] Optionally, the thickness of the above-mentioned continuously cast slab is greater than or equal to 150 mm and less than or equal to 450 mm.
[0010] Optionally, the width of the continuously cast slab is greater than or equal to 1600 mm and less than or equal to 2400 mm.
[0011] Optionally, the above method further includes: adjusting the water distribution in the secondary cooling spray zone to increase the non-uniform solidification area of the continuously cast slab in a preset direction, wherein the preset direction is a direction perpendicular to the casting direction.
[0012] Optionally, the above method further includes: determining the adjustment range of the secondary cooling spray zone based on the solidified shell thickness of the continuously cast slab.
[0013] Optionally, the adjustment range of the above-mentioned second cooling spray zone is greater than or equal to 5 sector segments and less than or equal to 12 sector segments.
[0014] Optionally, the distance between the above-mentioned secondary cooling spray zone and the meniscus of the crystallizer is greater than or equal to 6m and less than or equal to 40m.
[0015] Optionally, the ratio of the target total cooling water volume of the secondary cooling spray zone to the original total cooling water volume of the slab edge is greater than or equal to 0 and less than or equal to 0.5, and the ratio of the target total cooling water volume of the secondary cooling spray zone to the original total cooling water volume of the slab center is greater than or equal to 1.1 and less than or equal to 1.3.
[0016] Optionally, the blowing pressure at the edge of the slab is less than or equal to 200 Pa, and the blowing pressure in the center of the slab is greater than or equal to 150 Pa and less than or equal to 300 Pa.
[0017] Secondly, embodiments of the present invention also provide a continuous casting slab casting apparatus for narrow-gauge medium-thick plates, comprising:
[0018] The first determining unit is used to determine the desired width of the target material, wherein the desired width is less than or equal to 1800 mm;
[0019] The second determining unit is used to determine the width of the mother plate based on the desired width of the target plate, wherein the width of the mother plate is twice the width of the target plate.
[0020] The third determining unit is used to determine the billet shape of the continuously cast slab based on the aforementioned multiple-length width.
[0021] To achieve the above objectives, according to a third aspect of the present invention, a computer-readable storage medium is provided, the computer-readable storage medium comprising a stored program, wherein, when the program is executed by a processor, the steps of the above-described method for casting narrow-gauge medium-thick plate slabs are implemented.
[0022] To achieve the above objectives, according to a fourth aspect of the present invention, an electronic device is provided, comprising at least one processor and at least one memory connected to the processor; wherein the processor is configured to invoke program instructions in the memory to execute the steps of the above-described method for casting narrow-gauge medium-thick plates using continuous casting slabs.
[0023] By employing the above technical solution, the present invention provides a method and related equipment for continuous casting of narrow-specification medium-thick plates. Addressing the welding difficulties encountered in current methods of producing narrow-specification plates using multiple-length slitting, the present invention determines the desired width of the target plate, wherein the desired width is less than or equal to 1800 mm; determines the width of the master plate based on the desired width of the target plate, wherein the width of the master plate is twice the width of the target plate; and determines the billet shape of the continuous casting slab based on the multiple-length width. In this solution, utilizing the advantages of larger size and mass of wide and thick slabs, a master plate with a length and width multiple-length specifications is rolled. After slitting the master plate, multiple narrow-specification steel plates can be obtained. When producing the same quantity and size of narrow-specification steel plates, this method can reduce the amount of trimming, improve production efficiency, and increase yield.
[0024] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, and in order to make the above and other objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described below. Attached Figure Description
[0025] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:
[0026] Figure 1 A schematic flowchart of a continuous casting method for narrow-gauge medium-thick plates provided by an embodiment of the present invention is shown.
[0027] Figure 2 This diagram illustrates a central segregation zone in a slab according to an embodiment of the present invention.
[0028] Figure 3 This diagram illustrates the shape of an elemental segregation in the width direction according to an embodiment of the present invention.
[0029] Figure 4 This illustration shows another schematic diagram of a slab center segregation zone provided by an embodiment of the present invention;
[0030] Figure 5 This illustration shows another shape diagram of element segregation in the width direction according to an embodiment of the present invention;
[0031] Figure 6 This is a schematic block diagram showing the composition of a continuous casting slab casting device for narrow-gauge medium-thick plates provided in an embodiment of the present invention;
[0032] Figure 7This diagram illustrates the composition of an electronic device for casting narrow-gauge medium-thick plates according to an embodiment of the present invention. Detailed Implementation
[0033] Exemplary embodiments of the invention will now be described in more detail with reference to the accompanying drawings. While exemplary embodiments of the invention are shown in the drawings, it should be understood that the invention may be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that this invention will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0034] To address the welding difficulties encountered in producing narrow-gauge plates using the multiple-length slitting method, this invention provides a continuous casting method for narrow-gauge medium-thick plates, such as... Figure 1 As shown, the method includes:
[0035] S101. Determine the desired width of the target board material, wherein the desired width is less than or equal to 1800 mm;
[0036] For example, the desired width of the target board is the width of the desired narrow-specification medium-thick board, which is generally determined based on the user order. When the width is less than or equal to 1800mm, the target board is determined to be a narrow-specification board.
[0037] S102. Determine the width of the mother plate based on the desired width of the target board, wherein the width of the mother plate is twice the width of the target board.
[0038] S103. Determine the billet shape of the continuous casting slab based on the above-mentioned multiple width.
[0039] By employing the above technical solution, the continuous casting slab casting method for narrow-specification medium-thick plates provided by this invention addresses the welding difficulties encountered in current methods of producing narrow-specification plates using multiple-length slitting. This invention determines the desired width of the target plate, wherein the desired width is less than or equal to 1800 mm; determines the width of the master plate based on the desired width of the target plate, wherein the width of the master plate is twice the width of the target plate; and determines the billet shape of the continuous casting slab based on the multiple-length width. In this solution, utilizing the advantages of larger size and mass of wide and thick slabs, a master plate with a length and width multiple-length specifications is rolled. After slitting the master plate, multiple narrow-specification steel plates can be obtained. When producing the same quantity and size of narrow-specification steel plates, this method can reduce the amount of trimming, improve production efficiency, and increase yield.
[0040] In one embodiment, the method further includes: cutting the mother board using a multiple-scale slitting method to obtain the target board material.
[0041] For example, cutting metal into multiples of a fixed size as required by the order is called a multiple length. When delivering metal in multiple lengths, the length of the delivered metal material must be an integer multiple of the length specified by the buyer in the order contract (called a single length) (plus the allowance for saw cuts). For example, if the buyer requires a single length of 2m in the order contract, then the length when cut into double lengths will be 4m, and the length when cut into triple lengths will be 6m, with one or two saw cuts added respectively. The saw cut allowance is specified in the standard.
[0042] It should be noted that when delivering goods in multiple sizes, only positive deviations are allowed, and negative deviations are not permitted.
[0043] For example, in this application embodiment, the above-mentioned master plate is cut using a multiple-length slitting method to obtain the target plate. Taking advantage of the larger size and weight of the wide and thick slabs, master plates with lengths and widths multiples are rolled, and then the master plates are slitted to obtain multiple narrow-specification steel plates. When producing the same quantity and size of narrow-specification steel plates, the multiple-length slitting method can reduce the amount of trimming, improve production efficiency and yield.
[0044] In one embodiment, the thickness of the continuously cast slab is greater than or equal to 150 mm and less than or equal to 450 mm.
[0045] For example, when using the multiple-length slitting method to produce narrow-specification medium-thick plates, the center segregation of the original slab is exposed at the edges after slitting, easily leading to welding and machining problems. Therefore, strict requirements are placed on the control of slab center segregation. Traditional continuous slab casting aims for uniform solidification across the wide surface, employing a relatively uniform secondary spray cooling method to achieve better light or heavy compression effects, thereby reducing center segregation. However, during the process of molten steel gradually solidifying from the periphery to the center, due to the influence of selective crystallization during solidification, the center segregation in the width direction of the slab remains high after solidification, and the compositional segregation in the center of the width of the slab is still quite severe after rolling. When using this type of slab for producing narrow-specification medium-thick plates using multiple-length slitting, welding and machining problems are easily encountered.
[0046] For example, the greater the thickness of the continuously cast slab, the more severe the central solidification segregation. When producing narrow-gauge steel plates using the splitting method, the central segregation is exposed at the edge of the steel plate, easily causing weld black lines. Currently, central segregation of slabs less than 150mm thick is relatively easy to control, while 450mm thick slabs are produced less frequently. Slabs thicker than 450mm have a very long rolling length, which easily causes plate bending. Therefore, in this application embodiment, the thickness of the aforementioned continuously cast slab is controlled to be greater than or equal to 150mm and less than or equal to 450mm. Since this application embodiment pursues solidification uniformity across the wide surface during the casting process, a relatively uniform secondary spray cooling method is adopted to achieve better light or heavy pressure reduction, thereby reducing central segregation. Furthermore, by using slabs with a thickness greater than or equal to 150mm and less than or equal to 450mm, the process of molten steel gradually solidifying from the periphery to the center is avoided. Due to the influence of solidification selection and crystallization, the central segregation in the width direction of the slab remains high after solidification, leading to the problem of compositional segregation in the center of the width after slab rolling.
[0047] In one embodiment, the width of the continuously cast slab is greater than or equal to 1600 mm and less than or equal to 2400 mm.
[0048] For example, narrow-gauge steel plates are generally less than 1800mm, and there is currently no clear minimum requirement. When rolling narrow-gauge plates, if slab raw materials with a width less than 1600mm are used, rolling to double the width can easily lead to severe edge defects, increasing trimming and reducing the yield. If the width is greater than 2400mm, continuous casting production becomes difficult due to severe surface longitudinal cracks, easily causing edge defects, and making it difficult to guarantee slab quality. Therefore, this embodiment of the invention controls the width of the continuously cast slab to be greater than or equal to 1600mm and less than or equal to 2400mm.
[0049] In one embodiment, the method further includes: adjusting the water distribution in the secondary cooling spray zone to increase the non-uniform solidification area of the continuous casting slab in a preset direction, wherein the preset direction is a direction perpendicular to the casting direction.
[0050] It is understandable that the aforementioned preset direction can be interpreted as the width direction, which is perpendicular to the throwing direction.
[0051] In one embodiment, the method further includes: determining the adjustment range of the secondary cooling spray zone based on the solidified shell thickness of the continuously cast slab.
[0052] For example, such as Figure 2 As shown, when the slab is cooled by a relatively uniform secondary cooling spray, a segregation zone will form in the center of the slab, such as... Figure 3As shown, the elemental segregation is basically "A"-shaped in the width direction. According to solidification selectivity and crystallization, the steel that solidifies first produces less compositional segregation, while the steel that solidifies last tends to accumulate solute elements, resulting in severe compositional segregation. Therefore, increasing the cooling intensity at the center of the slab and promoting the early solidification of steel near the center of the wide face can reduce compositional segregation near the center of the wide face of the slab, dispersing the solute-enriched steel on both sides of the central area of the slab. Figure 4 As shown, the central segregation zone of the slab shifts to both sides, as... Figure 5 As shown, the elemental segregation in the slab width direction is basically "M" shaped. By adjusting the secondary cooling spray in continuous casting, the compositional segregation band in the slab width direction is shifted to the 1 / 4 and 3 / 4 positions on both sides. After rolling and splitting, the compositional segregation in the width center is lighter, thus solving the welding and processing problems caused by the multiple-length splitting method in the production of narrow-specification medium-thick plates.
[0053] In one embodiment, the adjustment range of the above-mentioned two cold spray zones is greater than or equal to 5 sector segments and less than or equal to 12 sector segments.
[0054] For example, in actual production applications, the number of fan-shaped sections on each casting machine is different. For instance, a 200mm thick casting machine has 12 fan-shaped sections, and a 400mm thick casting machine has 17. For a 200mm slab, the first four fan-shaped sections are typically used to increase the thickness of the solidified shell. Adjustments in the fifth to ninth fan-shaped sections pose no production risk. Adjusting the cooling water beyond the ninth section will lose its effectiveness. Similarly, for a 400mm thick casting machine, cooling water can be adjusted in the fifth to twelfth fan-shaped sections. After the twelfth fan-shaped section, the slab is essentially solidified, and adjusting the cooling water has no effect on center segregation. Therefore, in this embodiment, the adjustment range of the secondary cooling spray zone is controlled to be greater than or equal to 5 fan-shaped sections and less than or equal to 12 fan-shaped sections to achieve the optimal cooling effect.
[0055] In one embodiment, the distance between the above-mentioned two cold spray zones and the meniscus of the crystallizer is greater than or equal to 6m and less than or equal to 40m.
[0056] For example, the distance between the above-mentioned second cooling spray zone and the meniscus of the crystallizer is determined based on the interval of the sector segment.
[0057] In one embodiment, the ratio of the target total cooling water volume of the secondary cooling spray zone for the edge of the slab to the original total cooling water volume is greater than or equal to 0 and less than or equal to 0.5, and the ratio of the target total cooling water volume of the secondary cooling spray zone for the center area of the slab to the original total cooling water volume is greater than or equal to 1.1 and less than or equal to 1.3.
[0058] For example, in this embodiment of the invention, the cooling water in the 0-200mm range of the edge in the slab width direction (i.e., the direction perpendicular to the drawing direction) is reduced or shut off. On the one hand, this ensures that the slab edge temperature is always >850℃, reducing transverse cracks at the slab corners. It should be noted that if the edge temperature is below 850℃, cracks are more likely to occur. On the other hand, it reduces the cooling effect to 1 / 4 of the width at the edge, controlling severe segregation at the 1 / 4 and 3 / 4 positions. If it exceeds this range, the edge temperature is likely to be too low, and severe segregation will concentrate at the 1 / 2 width position, which can easily cause black weld lines after splitting.
[0059] In one embodiment, the blowing pressure at the edge of the slab is less than or equal to 200 Pa, and the blowing pressure at the center of the slab is greater than or equal to 150 Pa and less than or equal to 300 Pa.
[0060] For example, since the blowing pressure affects the atomization effect of the cooling water, the air pressure needs to be controlled below 200 Pa after the cooling water at the edge is reduced, and the atomization effect is better when the cooling water at the center is increased and the pressure is controlled at 150-300 Pa.
[0061] Furthermore, the following are specific embodiments of the implementation of this application:
[0062] Data analysis was conducted on the solidified shell thickness during the continuous casting process of slabs with a thickness of 200-400mm and a width of 1600-2400mm to ensure shell strength and the amount of molten steel inside the slab, thus enabling adjustments to the intensity of the secondary cooling spray. The specific method is as follows:
[0063] (1) The adjustment range of the secondary cooling spray zone is determined to be 5-12 sector segments based on the thickness of the solidified billet shell, and the distance from the meniscus of the crystallizer is 6-40m.
[0064] (2) Reduce the total cooling water volume at the edge of the slab by 50-100% and increase the total cooling water volume in the center of the slab by 10-30%;
[0065] (3) The blowing pressure at the edge of the slab is ≤200Pa, and the blowing pressure at the center of the slab is 150-300Pa.
[0066] Example 1
[0067] (1) Narrow-sized steel plates with a target width of 1800mm and a thickness of 12mm are produced by multiple-length cutting of 200mm×2400mm blanks.
[0068] (2) The solidified shell thickness is greater than 50mm at a position less than 6m from the meniscus of the crystallizer. The secondary cooling spray zone with a cross section of 200mm×2400mm can be adjusted to 5-8 fan-shaped sections, 6-16m from the meniscus of the crystallizer.
[0069] (3) Reduce the total cooling water volume at the edge of the slab by 70% and increase the total cooling water volume in the center of the slab by 10%;
[0070] (4) The blowing pressure at the edge of the slab is 100 Pa, and the blowing pressure at the center of the slab is 200 Pa.
[0071] The low-magnification test results of the slab are shown in Table 1.
[0072] Table 1 Low Rating
[0073]
[0074] Example 2
[0075] (1) Narrow specification steel plate with a target width of 1800mm and a thickness of 18mm, select 300mm×2400mm blank shape for multiple length production;
[0076] (2) The solidified shell thickness is greater than 55mm at a position less than 6m from the meniscus of the crystallizer. The secondary cooling spray zone with a cross section of 300mm×2400mm can be adjusted to 5-10 fan-shaped sections, with a distance of 6-34m from the meniscus of the crystallizer.
[0077] (3) Reduce the cooling water volume at the edge of the slab by 100% and increase the cooling water volume in the center of the slab by 30%;
[0078] (4) The blowing pressure at the edge of the slab is 200 Pa, and the blowing pressure at the center of the slab is 300 Pa.
[0079] The low-magnification test results of the slab are shown in Table 2.
[0080] Table 2 Low Rating
[0081]
[0082]
[0083] Example 3
[0084] (1) Narrow specification steel plate with a target width of 1800mm and a thickness of 25mm, select 400mm×2400mm blank shape for multiple length splitting production;
[0085] (2) The solidified shell thickness is greater than 60mm at a position less than 6m from the meniscus of the crystallizer. The secondary cooling spray zone with a cross section of 400mm×2400mm can be adjusted to 5-12 fan-shaped sections, with a distance of 6-40m from the meniscus of the crystallizer.
[0086] (3) Reduce the total cooling water volume at the edge of the slab by 80% and increase the total cooling water volume in the center of the slab by 30%;
[0087] (4) The blowing pressure at the edge of the slab is 100 Pa, and the blowing pressure at the center of the slab is 300 Pa.
[0088] The low-magnification test results of the slab are shown in Table 3.
[0089] Table 3 Low Rating
[0090]
[0091] Furthermore, as a response to the above Figure 1 In addition to the implementation of the method shown, this embodiment of the invention also provides a continuous casting slab casting device for narrow-gauge medium-thick plates, used for the above-mentioned... Figure 1 The method shown is implemented accordingly. This device embodiment corresponds to the foregoing method embodiment. For ease of reading, this device embodiment will not repeat the details of the foregoing method embodiment, but it should be clear that the device in this embodiment can implement all the contents of the foregoing method embodiment. Figure 6 As shown, the device includes: a first determining unit 21, a second determining unit 22, and a third determining unit 23, wherein...
[0092] The first determining unit 21 is used to determine the desired width of the target plate, wherein the desired width is less than or equal to 1800 mm;
[0093] The second determining unit 22 is used to determine the width of the mother plate based on the desired width of the target plate, wherein the width of the mother plate is twice the width of the target plate.
[0094] The third determining unit 23 is used to determine the billet shape of the continuously cast slab based on the aforementioned multiple width.
[0095] The processor contains a kernel, which retrieves the corresponding program unit from memory. One or more kernels can be configured. By adjusting the kernel parameters, a continuous casting method for producing narrow-gauge medium-thick plates can be implemented, solving the welding difficulties encountered when using the multiple-length slitting method to produce narrow-gauge plates.
[0096] This invention provides a computer-readable storage medium including a stored program that, when executed by a processor, implements the above-described method for continuous casting of narrow-gauge medium-thick plates.
[0097] This invention provides a processor for running a program, wherein the program executes the continuous casting method for narrow-gauge medium-thick plates.
[0098] This invention provides an electronic device, which includes at least one processor and at least one memory connected to the processor; wherein the processor is used to call program instructions in the memory to execute the continuous casting slab casting method for narrow-gauge medium-thick plates as described above.
[0099] This invention provides an electronic device 30, such as... Figure 7 As shown, the electronic device includes at least one processor 301, and at least one memory 302 and bus 303 connected to the processor; wherein, the processor 301 and the memory 302 communicate with each other through the bus 303; the processor 301 is used to call program instructions in the memory to execute the above-mentioned continuous casting slab casting method for narrow-specification medium-thick plates.
[0100] The smart electronic devices mentioned in this article can be PCs, tablets, mobile phones, etc.
[0101] This application also provides a computer program product that, when executed on a process management electronic device, is suitable for executing a program that initializes the steps of the continuous casting slab casting method for the aforementioned narrow-gauge medium-thick plate.
[0102] It should be noted that the descriptions of each embodiment in the above embodiments have different focuses. For parts that are not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.
[0103] Those skilled in the art will understand that embodiments of this application can be provided as methods, systems, or computer program products. Therefore, this application can take the form of a completely hardware embodiment, a completely software embodiment, or an embodiment combining software and hardware aspects. Furthermore, this application can take the form of a computer program product embodied on one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.
[0104] This application is described with reference to flowchart illustrations and / or block diagrams of methods, apparatus (systems), and computer program products according to embodiments of this application. It will be understood that each block of the flowchart illustrations and / or block diagrams, and combinations of blocks in the flowchart illustrations and / or block diagrams, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, special-purpose computer, embedded computer, or other programmable data processing apparatus to produce a machine, such that the instructions, which execute via the processor of the computer or other programmable data processing apparatus, create a machine for implementing the flowchart illustrations. Figure 1 One or more processes and / or boxes Figure 1 A device that provides the functions specified in one or more boxes.
[0105] These computer program instructions may also be stored in a computer-readable storage medium that can direct a computer or other programmable data processing device to function in a particular manner, such that the instructions stored in the computer-readable storage medium produce an article of manufacture including instruction means, which are implemented in a process Figure 1 One or more processes and / or boxes Figure 1 The function specified in one or more boxes.
[0106] These computer program instructions may also be loaded onto a computer or other programmable data processing equipment to cause a series of operational steps to be performed on the computer or other programmable equipment to produce a computer-implemented process, thereby providing instructions that execute on the computer or other programmable equipment for implementing the process. Figure 1 One or more processes and / or boxes Figure 1 The steps of the function specified in one or more boxes.
[0107] This application also provides a computer program product, which includes computer software instructions that, when executed on a processing device, cause the processing device to perform actions such as... Figure 1 The control flow of the memory in the corresponding embodiment.
[0108] A computer program product includes one or more computer instructions. When the computer program instructions are loaded and executed on a computer, all or part of the flow or function according to the embodiments of this application is generated. The computer may be a general-purpose computer, a special-purpose computer, a computer network, or other programmable device. The computer instructions may be stored in a computer-readable storage medium or transmitted from one computer-readable storage medium to another. For example, computer instructions may be transmitted from one website, computer, server, or data center to another website, computer, server, or data center via wired (e.g., coaxial cable, fiber optic, digital subscriber line (DSL)) or wireless (e.g., infrared, wireless, microwave, etc.) means. The computer-readable storage medium may be any available medium that a computer can store or a data storage device such as a server or data center that integrates one or more available media. The available medium may be a magnetic medium (e.g., floppy disk, hard disk, magnetic tape), an optical medium (e.g., DVD), or a semiconductor medium (e.g., solid-state disk (SSD)).
[0109] Those skilled in the art will clearly understand that, for the sake of convenience and brevity, the specific working processes of the systems, devices, and units described above can be referred to the corresponding processes in the foregoing method embodiments, and will not be repeated here.
[0110] In the several embodiments provided in this application, it should be understood that the disclosed systems, apparatuses, and methods can be implemented in other ways. For example, the apparatus embodiments described above are merely illustrative; for instance, the division of units is only a logical functional division, and in actual implementation, there may be other division methods. For example, multiple units or components may be combined or integrated into another system, or some features may be ignored or not executed. Furthermore, the coupling or direct coupling or communication connection shown or discussed may be through some interfaces, or indirect coupling or communication connection between apparatuses or units, and may be electrical, mechanical, or other forms.
[0111] The units described as separate components may or may not be physically separate. The components shown as units may or may not be physical units; that is, they may be located in one place or distributed across multiple network units. Some or all of the units can be selected to achieve the purpose of this embodiment according to actual needs.
[0112] Furthermore, the functional units in the various embodiments of this application can be integrated into one processing unit, or each unit can exist physically separately, or two or more units can be integrated into one unit. The integrated unit can be implemented in hardware or as a software functional unit.
[0113] If the integrated unit is implemented as a software functional unit and sold or used as an independent product, it can be stored in a computer-readable storage medium. Based on this understanding, the technical solution of this application, in essence, or the part that contributes to the prior art, or all or part of the technical solution, can be embodied in the form of a software product. This computer software product is stored in a storage medium and includes several instructions to cause a computer device (which may be a personal computer, server, or network device, etc.) to execute all or part of the steps of the methods of the various embodiments of this application. The aforementioned storage medium includes various media capable of storing program code, such as USB flash drives, portable hard drives, read-only memory (ROM), random access memory (RAM), magnetic disks, or optical disks.
[0114] The above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit it. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of this application.
Claims
1. A method for continuously casting slabs of narrow-gauge medium-thick plates, characterized in that, include: Determine the desired width of the target sheet material, wherein the desired width is less than or equal to 1800 mm; The width of the mother board is determined based on the desired width of the target board, wherein the width of the mother board is twice the width of the target board. The billet shape of the continuous casting slab is determined based on the aforementioned multiple-length width; The mother board is cut using a slitting method to obtain the target board material; Adjust the water distribution in the secondary cooling spray zone to increase the non-uniform solidification area of the continuously cast slab in a preset direction, wherein the preset direction is a direction perpendicular to the casting direction; The distance between the secondary cooling spray zone and the meniscus of the crystallizer is greater than or equal to 6m and less than or equal to 40m. The ratio of the target total cooling water volume to the original total cooling water volume in the secondary cooling spray zone for the edge of the slab is greater than or equal to 0 and less than or equal to 0.
5. The ratio of the target total cooling water volume to the original total cooling water volume in the secondary cooling spray zone for the central area of the slab is greater than or equal to 1.1 and less than or equal to 1.
3. Increasing the cooling intensity at the center of the slab promotes the early solidification of molten steel near the center of the wide face, reduces compositional segregation near the center of the wide face of the slab, and disperses molten steel enriched with solute elements on both sides of the central area of the slab.
2. The method according to claim 1, characterized in that, The thickness of the continuously cast slab is greater than or equal to 150 mm and less than or equal to 450 mm.
3. The method according to claim 1, characterized in that, The width of the continuously cast slab is greater than or equal to 1600 mm and less than or equal to 2400 mm.
4. The method according to claim 1, characterized in that, Also includes: The adjustment range of the secondary cooling spray zone is determined based on the solidified shell thickness of the continuously cast slab.
5. The method according to claim 4, characterized in that, The adjustment range of the second cold spray zone is greater than or equal to 5 sector segments and less than or equal to 12 sector segments.
6. The method according to claim 1, characterized in that, The blowing pressure at the edge of the slab is less than or equal to 200 Pa. The blowing pressure in the central area of the slab is greater than or equal to 150 Pa and less than or equal to 300 Pa.
Citation Information
Patent Citations
Bulb steel production technology
CN101190442A
Control method for continuous casting center cracks of small square billet of steel for large-specification and high-niobium-content steel bars
CN115323109A