A method for removing bisphenol A from wastewater by catalyzing persulfate with nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material

The combination of nitrogen-doped spiral carbon nanotube-wrapped iron carbide composites and persulfate solves the problem of bisphenol A degradation in wastewater, achieves efficient removal, and is suitable for advanced treatment of high-concentration and high-salt wastewater.

CN118307119BActive Publication Date: 2024-10-11GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410414361.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-10-11
Estimated Expiration
2044-04-08

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively degrade bisphenol A in sewage and wastewater. Advanced oxidation technology inhibits free radical activity due to natural organic matter and inorganic ions, resulting in poor degradation results.

Method used

Nitrogen-doped spiral carbon nanotubes are used to wrap iron carbide composites and are mixed with persulfate to construct a method for efficiently removing bisphenol A from wastewater through catalysis. The spiral carbon nanotubes are used to increase the electrochemical activity and pore area of ​​the material and enhance Catalytic performance.

Benefits of technology

It can efficiently remove bisphenol A from wastewater at room temperature, has good stability and adaptability, is suitable for deep treatment of high-concentration and high-salt wastewater, and significantly improves the removal rate of pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307119B_ABST
    Figure CN118307119B_ABST
Patent Text Reader

Abstract

The present invention provides a method for removing bisphenol A from wastewater by catalyzing persulfate with a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material, and belongs to the technical field of wastewater treatment. The present invention prepares a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material by adding helical carbon nanotubes to a precursor mixture containing a carbon source, a nitrogen source and an iron source. The composite material has helical carbon nanotubes with high stability and strong magnetism, and can effectively increase the defect points and contact area on the surface of the material. The prepared composite material has the advantages of strong ferromagnetism, high stability and high catalytic activity, and can effectively catalyze persulfate, thereby constructing an advanced oxidation system for efficiently removing bisphenol A from wastewater, which provides technical support for deep treatment of industrial wastewater containing endocrine disruptors at room temperature, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater treatment, and in particular to a method for removing bisphenol A in wastewater by catalyzing persulfate using a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material. Background Art

[0002] Bisphenol A is a widely used chemical, mainly used to make plastic and resin products, such as beverage bottles and food containers. Due to its structure similar to estrogen, bisphenol A can interfere with the endocrine system and may cause a variety of health problems. It enters the environment through industrial production and product waste, and exists in water bodies, soil and food chains. Due to its chemical stability, bisphenol A is difficult to effectively degrade through conventional water treatment technologies such as filtration, adsorption or disinfection, and ultimately poses a threat to the environment and human health through water circulation. Advanced oxidation technology can be used to degrade bisphenol A through sulfate free radicals (SO 4 ·- , E 0 =2.60V) and hydroxyl radicals (HO · ,E 0 =2.80V) effectively degrades new endocrine disruptors. However, due to the natural organic matter and inorganic ions (such as sulfate (SO 4 2- ), chloride ion (Cl - ) and carbonate (CO 3 2- )) and other complex components can quench SO 4 ·- and HO · Free radicals, thus inhibiting the effect of advanced oxidation technology in degrading endocrine disruptors in actual wastewater. Therefore, it is necessary to develop a treatment technology that effectively degrades bisphenol A in wastewater. Summary of the invention

[0003] The purpose of the present invention is to provide a method for removing bisphenol A in wastewater by catalyzing persulfate with a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material, which can effectively degrade bisphenol A in wastewater.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for removing bisphenol A in wastewater by catalyzing persulfate with a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material, comprising the following steps:

[0006] The wastewater containing bisphenol A, the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material and persulfate are mixed for degradation;

[0007] The method for preparing the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material comprises the following steps:

[0008] An iron source, a carbon source and a nitrogen source are mixed, the obtained mixture is mixed with the helical carbon nanotubes, and the mixture is dried and calcined in sequence to obtain a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material.

[0009] Preferably, the usage ratio of the bisphenol A-containing wastewater to the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material is 47-53 mL: 32-80 mg.

[0010] Preferably, the persulfate includes sodium persulfate, potassium persulfate, sodium monopersulfate or potassium monopersulfate; the concentration of the persulfate in the bisphenol A-containing wastewater is 0.2-3.5 mM, the degradation temperature is 20-50° C., the pH value is 3-11, and the time is 20-40 min.

[0011] Preferably, the iron source comprises a ferric chloride solution; the carbon source comprises a glucose solution; the nitrogen source comprises a melamine solution; and the volume ratio of the ferric chloride solution, the glucose solution and the melamine solution is 30-50:50-70:80-120.

[0012] Preferably, the solvents used in the ferric chloride solution are anhydrous ethanol and water, and the volume ratio of the anhydrous ethanol to water is 1-2:1-2; the dosage ratio of anhydrous ferric chloride to the solvent in the ferric chloride solution is 2-4 g:30-50 mL.

[0013] Preferably, the glucose solution comprises glucose, water and anhydrous ethanol, and the usage ratio of the glucose, water and anhydrous ethanol is 2-4 g: 15-25 mL: 35-45 mL.

[0014] Preferably, the solvents used in the melamine solution are anhydrous ethanol and water, and the volume ratio of anhydrous ethanol to water is 1-2:1-2; the amount ratio of melamine to solvent in the melamine solution is 1-3g:80-120mL.

[0015] Preferably, the mass ratio of the helical carbon nanotubes to anhydrous ferric chloride is 0.4-0.6:2-4.

[0016] Preferably, the temperature for mixing the mixture with the helical carbon nanotubes is 50-70° C., and the time is 1-3 hours; the temperature for drying is 160-200° C., and the time is 10-14 hours.

[0017] Preferably, the calcination is carried out in a protective atmosphere, which includes nitrogen and / or argon; the calcination temperature is 700-900°C, and the time is 2-4h; the heating rate to the calcination temperature is 4-6°C / min.

[0018] The present invention prepares a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material by adding helical carbon nanotubes to a precursor mixture containing a carbon source, a nitrogen source and an iron source. The helical carbon nanotubes with high stability and strong magnetism can effectively increase the defect points and contact area on the surface of the material, and the helical carbon nanotubes can effectively increase the capacitance of the material, so that the material has more electrochemical active sites and can generate a larger voltage at the same current density, and has better electrocatalytic performance than conventional materials. Its excellent pore area provides an effective redox active center and a carrier for electron transfer. The nitrogen element can enhance the anchoring of iron carbide on the carbon nanotubes. The composite material prepared by modifying iron carbide with helical carbon nanotubes can not only retain active sites, but also utilize the spatial confinement effect to enhance the reaction concentration and accelerate the reaction speed. Therefore, the prepared composite material has the advantages of strong ferromagnetism, high stability and high catalytic activity. The material can effectively catalyze persulfate. The advanced oxidation system for efficiently removing bisphenol A endocrine disruptors in wastewater constructed by catalyzing persulfate can efficiently remove bisphenol A endocrine disruptors in wastewater, provide technical guidance for deep treatment of industrial wastewater containing endocrine disruptors at room temperature, and have good application prospects in the deep treatment of bisphenol A in wastewater.

[0019] The nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material prepared by the method provided by the present invention has good stability, can be used in a wide pH range, is easy to recycle, and can be reused. The composite material can be used to efficiently catalyze persulfate to deeply treat high-concentration and high-salinity wastewater contaminated by bisphenol A at room temperature, has strong adaptability and high application value, and can effectively activate persulfate to deeply treat pollutants in high-concentration and high-salinity wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a SEM image of the helical carbon nanotube used in Example 1;

[0021] Figure 2 This is a SEM image of the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material of Example 1;

[0022] Figure 3 This is a HR-TEM image of the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material of Example 1;

[0023] Figure 4 This is a structural model diagram of the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material prepared in Example 1;

[0024] Figure 5 X-ray crystal diffraction patterns of the composite materials prepared in Example 1, Comparative Example 1 and Comparative Example 2;

[0025] Figure 6 The Raman images of the composite materials prepared in Example 1, Comparative Example 1 and Comparative Example 2;

[0026] Figure 7 It is a data graph of electron transfer rate of the reaction between bisphenol A and sodium persulfate on the material surface of Example 1, Comparative Example 2 and Comparative Example 3;

[0027] Figure 8 This is a diagram showing the effect of removing bisphenol A from the composite materials of Example 1 and Comparative Examples 1 to 3;

[0028] Fig. 9 This is a graph showing the effect of different reaction temperatures on the removal of bisphenol A from the composite material of Example 1;

[0029] Fig.10 This is a diagram showing the effect of different pH values ​​on the removal of bisphenol A from the composite material of Example 1;

[0030] Fig.11 This is a graph showing the effect of the dosage of NaCl on the removal of bisphenol A from the composite material of Example 1;

[0031] Fig.12 This is a graph showing the effect of the dosage of PBS on the removal of bisphenol A from the composite material of Example 1;

[0032] Fig.13 This is a diagram showing the effect of the composite material of Example 1 on removing bisphenol A from different wastewaters. DETAILED DESCRIPTION

[0033] The present invention provides a method for removing bisphenol A in wastewater by catalyzing persulfate with a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material, comprising the following steps:

[0034] The wastewater containing bisphenol A, the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material and persulfate are mixed for degradation;

[0035] The method for preparing the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material comprises the following steps:

[0036] An iron source, a carbon source and a nitrogen source are mixed, the obtained mixture is mixed with the helical carbon nanotubes, and the mixture is dried and calcined in sequence to obtain a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material.

[0037] In the present invention, unless otherwise specified, the required raw materials or reagents are commercially available products well known to those skilled in the art.

[0038] The present invention has no particular limitation on the source of the bisphenol A-containing wastewater, which can be obtained in a manner well known in the art.

[0039] The present invention preferably uses a bisphenol A aqueous solution to simulate bisphenol A-containing wastewater, and the concentration of bisphenol A in the bisphenol A aqueous solution is preferably 70 to 85 μM, more preferably 78 μM.

[0040] In the present invention, the usage ratio of the bisphenol A-containing wastewater to the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material is preferably 47-53 mL: 32-80 mg, and more preferably 50 mL: 32-80 mg.

[0041] In the present invention, the persulfate preferably includes sodium persulfate, potassium persulfate, sodium monopersulfate or potassium monopersulfate, more preferably sodium persulfate; the concentration of the persulfate in the bisphenol A-containing wastewater is preferably 0.2-3.5 mM, more preferably 1-2 mM; the degradation temperature is preferably 20-50°C, more preferably 25-45°C; the pH value is 3-11, more preferably 4-5, and the time is preferably 20-40 min, more preferably 30 min.

[0042] In the present invention, in the method for preparing the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material:

[0043] In the present invention, the iron source preferably includes a ferric chloride solution; the solvent used in the ferric chloride solution is preferably anhydrous ethanol and water, and the volume ratio of the anhydrous ethanol to water is preferably 1-2:1-2, more preferably 1:1; the amount ratio of anhydrous ferric chloride to the solvent in the ferric chloride solution is preferably 2-4 g:30-50 mL, more preferably 2.5-3.5 g:35-45 mL, and further preferably 3 g:40 mL.

[0044] In the present invention, the carbon source includes a glucose solution; the glucose solution preferably includes glucose, water and anhydrous ethanol, and the usage ratio of the glucose, water and anhydrous ethanol is preferably 2-4g:15-25mL:35-45mL, more preferably 2.5-3.5g:18-23mL:37-43mL, and more preferably 3g:20mL:39-40mL. The present invention preferably dissolves the carbon source in water, and then adds anhydrous ethanol to the resulting aqueous solution.

[0045] In the present invention, the nitrogen source includes a melamine solution; the solvent used in the melamine solution is preferably anhydrous ethanol and water, and the volume ratio of the anhydrous ethanol to water is preferably 1-2:1-2, more preferably 1:1; the amount ratio of melamine to solvent in the melamine solution is limited to 1-3g:80-120mL, more preferably 1.5-2.5g:90-110mL, and further preferably 2g:100mL. In the present invention, the nitrogen source is preferably dissolved in the solvent at 55-65°C, and stirred continuously until the solution is colorless.

[0046] In the present invention, the volume ratio of the ferric chloride solution, the glucose solution and the melamine solution is preferably 30-50:50-70:80-120, more preferably 35-45:55-66:90-110, and further preferably 40:60:100.

[0047] In the present invention, the mixing time of the iron source, carbon source and nitrogen source is preferably 25 to 35 minutes, more preferably 27 to 32 minutes, and more preferably 30 minutes. In the present invention, the iron source and the carbon source are preferably mixed first, and then added to the nitrogen source, and stirred at a rate of 50 r / min for 17 to 30 minutes.

[0048] The present invention has no particular limitation on the source of the helical carbon nanotubes, and any commercially available product known in the art may be used. In the embodiments of the present invention, the helical carbon nanotubes used are long carbon nanotubes purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.

[0049] In the present invention, the mass ratio of the helical carbon nanotubes to anhydrous ferric chloride is preferably 0.4-0.6:2-4, more preferably 0.47-0.52:2.5-3.5, and further preferably 0.5:3.

[0050] In the present invention, the temperature for mixing the mixture with the helical carbon nanotubes is preferably 50-70°C, more preferably 55-65°C, and further preferably 60°C, and the time is preferably 1-3h, more preferably 1.5-2.5h, and further preferably 2h.

[0051] In the present invention, the drying temperature is preferably 160 to 200° C., more preferably 170 to 180° C., and the drying time is preferably 10 to 14 h, more preferably 11 to 13 h, and further preferably 12 h.

[0052] In the present invention, the dried product is preferably ground into powder and then calcined.

[0053] In the present invention, the calcination is preferably carried out in a protective atmosphere, and the protective atmosphere preferably includes nitrogen and / or argon; the calcination temperature is preferably 700-900°C, more preferably 750-850°C, and further preferably 800°C; the time is preferably 2-4h, more preferably 2.5-3.5h, and further preferably 3h; the heating rate to the calcination temperature is preferably 4-6°C / min, more preferably 4.5-5.5°C / min, and further preferably 5°C / min.

[0054] In the present invention, the calcined product is preferably cooled and then ground to obtain a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material. The present invention has no particular limitation on the particle size of the particles obtained by grinding, and can be adjusted according to actual needs.

[0055] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0056] The constant temperature magnetic stirrer in the following examples and comparative examples is Hangzhou Jingfei Instrument, MS-H.

[0057] The helical carbon nanotubes, N-doped carbon nanotubes, amino-modified carbon nanotubes and hydroxylated carbon nanotubes used in the following examples are all from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., and all are long carbon nanotubes.

[0058] Example 1

[0059] 3.0 g of anhydrous ferric chloride is dissolved in 40 mL of a solvent, the solvent being composed of anhydrous ethanol and water in a volume ratio of 1:1, and stirred until completely dissolved to obtain an anhydrous ferric chloride solution; 3.0 g of glucose is dissolved in 20 mL of water, stirred until completely dissolved, and then 40 mL of anhydrous ethanol is added and mixed evenly to obtain a glucose solution; 2.0 g of melamine is added to 100 mL of a solvent in a 250 mL beaker, the solvent being composed of anhydrous ethanol and water in a volume ratio of 1:1, the beaker is placed on a constant temperature magnetic stirrer, and stirred at 60° C. at a rate of 50 r / min until the solution becomes colorless to obtain a melamine solution;

[0060] Anhydrous ferric chloride solution and glucose solution were injected into the melamine solution and stirred at a rate of 50 r / min for 30 min; then 0.5 g of helical carbon nanotubes (twist angle 60°) were added and stirred at 60°C for 2 h to make the mixture uniform, and the obtained mixture was dried in an oven at 180°C for 12 h to obtain a solid precursor; the solid precursor was ground into powder and loaded into a porcelain boat, which was placed in a tube furnace and heated at N 2 The temperature was raised to 800°C at a rate of 5°C / min under a carbon dioxide atmosphere. After being kept at 800°C for 3 hours, the tubular furnace was cooled at room temperature. After the tubular furnace was cooled, the porcelain boat was taken out and the obtained black solid was ground into powder particles with a particle size of 1.3 μm to obtain a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material.

[0061] Example 2

[0062] Dissolve 2.5 g of anhydrous ferric chloride in 35 mL of a solvent consisting of anhydrous ethanol and water in a volume ratio of 1:1, and stir until completely dissolved to obtain an anhydrous ferric chloride solution; dissolve 2.5 g of glucose in 18 mL of water, stir until completely dissolved, add 37 mL of anhydrous ethanol and mix well to obtain a glucose solution; add 1.5 g of melamine into 90 mL of a solvent in a 250 mL beaker, the solvent consisting of anhydrous ethanol and water in a volume ratio of 1:1, place the beaker on a constant temperature magnetic stirrer, stir at 57°C at a rate of 50 r / min until the solution is colorless, to obtain a melamine solution;

[0063] Anhydrous ferric chloride solution and glucose solution were added to the melamine solution, and after stirring at a rate of 50 r / min for 17 min, 0.47 g of helical carbon nanotubes (twist angle 60°) were added, and stirred at 55°C for 2.5 h to obtain a uniform mixed solution; the mixed solution was then dried in an oven at 170°C for 13 h to obtain a solid precursor; the solid precursor was ground into powder and loaded into a porcelain boat, which was placed in a tube furnace and heated at N 2 The temperature was raised to 750°C at a rate of 4.5°C / min under an atmosphere, and the tube furnace was cooled at room temperature after being kept at 750°C for 2.5 hours. After the tube furnace was cooled, the porcelain boat was taken out, and the obtained black solid was ground into powder particles with a particle size of 1.1 μm to obtain nitrogen-doped helical carbon nanotube-wrapped iron carbide composite materials.

[0064] Example 3

[0065] 3.5 g of anhydrous ferric chloride was dissolved in 45 mL of a solvent consisting of anhydrous ethanol and water in a volume ratio of 1:1, and stirred until completely dissolved to obtain an anhydrous ferric chloride solution; 3.5 g of glucose was dissolved in 23 mL of water, stirred until completely dissolved, and then 43 mL of anhydrous ethanol was added and mixed evenly to prepare a glucose solution; 2.5 g of melamine was added to 110 mL of a solvent in a 250 mL beaker, the solvent consisting of anhydrous ethanol and water in a volume ratio of 1:1, the beaker was placed on a constant temperature magnetic stirrer, and stirred at 61° C. at a rate of 50 r / min until the solution was colorless to obtain a melamine solution;

[0066] Anhydrous ferric chloride solution and glucose solution were added to the melamine solution, and after stirring at a rate of 50 r / min for 23 min, 0.52 g of helical carbon nanotubes (twist angle 60°) were added, and stirred at 65°C for 1.5 h to obtain a uniform mixed solution, and the mixed solution was dried in an oven at 190°C for 11 h to obtain a solid precursor; the solid precursor was ground into powder and loaded into a porcelain boat, which was placed in a tube furnace and heated at N 2The temperature was raised to 850°C at a rate of 5.5°C / min under an atmosphere, and the tube furnace was cooled at room temperature after being kept at 850°C for 2.5 hours. After the tube furnace was cooled, the porcelain boat was taken out, and the obtained black solid was ground into powder particles with a particle size of 1.4 μm to obtain nitrogen-doped helical carbon nanotube-wrapped iron carbide composite materials.

[0067] Comparative Example 1

[0068] 3.0 g of anhydrous ferric chloride was dissolved in 40 mL of a solvent consisting of anhydrous ethanol and water in a volume ratio of 1:1, and stirred until completely dissolved to form an anhydrous ferric chloride solution; 3.0 g of glucose was added to 20 mL of water and stirred until completely dissolved, and then 40 mL of anhydrous ethanol was added and mixed evenly to obtain a glucose solution;

[0069] The anhydrous ferric chloride solution and the glucose solution were stirred at 60°C at a rate of 50 r / min for 30 min, and then the nitrogen-doped carbon nanotubes were added and stirred for 2 h. The resulting mixture was placed in an oven at 180°C and dried for 12 h. The resulting solid precursor was ground into powder and loaded into a porcelain boat, which was then placed in a tube furnace and heated at N 2 The temperature was raised to 800°C at a rate of 5°C / min under an atmosphere and calcined at 800°C for 3 hours. The tube furnace was then cooled at room temperature. After the tube furnace was cooled, the solid in the porcelain boat was taken out and ground into powder to obtain a nitrogen-doped carbon nanotube-encapsulated nitrogen-doped iron carbide composite material.

[0070] Comparative Example 2

[0071] 3.0 g of anhydrous ferric chloride was dissolved in 40 mL of a solvent consisting of anhydrous ethanol and water in a volume ratio of 1:1, and stirred until completely dissolved to form an anhydrous ferric chloride solution; 3.0 g of glucose was added to 20 mL of water and stirred until completely dissolved, and then 40 mL of anhydrous ethanol was added and mixed evenly to obtain a glucose solution;

[0072] The anhydrous ferric chloride solution and the glucose solution were stirred at 60°C at a rate of 50 r / min for 30 min, and then the amino carbon nanotubes were added and stirred for 2 h. The resulting mixture was placed in an oven at 180°C and dried for 12 h. The resulting solid precursor was ground into powder and loaded into a porcelain boat, which was then placed in a tube furnace and heated at N 2 The temperature was raised to 800°C at a rate of 5°C / min under an atmosphere and calcined at 800°C for 3 hours. The tubular furnace was then cooled at room temperature. After the tubular furnace was cooled, the solid in the porcelain boat was taken out and ground into powder to obtain a nitrogen-doped amino carbon nanotube-wrapped iron carbide composite material.

[0073] Comparative Example 3

[0074] 3.0 g of anhydrous ferric chloride was dissolved in 40 mL of a solvent consisting of anhydrous ethanol and water in a volume ratio of 1:1, and stirred until completely dissolved to obtain an anhydrous ferric chloride solution; 3.0 g of glucose was added to 20 mL of water and stirred until completely dissolved, and then 40 mL of anhydrous ethanol was added and mixed evenly to obtain a glucose solution;

[0075] The anhydrous ferric chloride solution and the glucose solution were stirred at 60°C at a rate of 50 r / min for 30 min, and then the hydroxylated carbon nanotubes were added and stirred for 2 h. The resulting mixture was placed in an oven at 180°C and dried for 12 h. The resulting solid precursor was ground into powder and loaded into a porcelain boat, which was then placed in a tube furnace and heated at N 2 The temperature was raised to 800°C at a rate of 5°C / min under an atmosphere and calcined at 800°C for 3 hours. The tube furnace was then cooled at room temperature. After the tube furnace was cooled, the solid in the porcelain boat was taken out and ground into powder to obtain a nitrogen-doped hydroxylated carbon nanotube-wrapped iron carbide composite material.

[0076] Characterization and performance testing

[0077] 1) The SEM image of the helical carbon nanotubes used in Example 1 is as follows Figure 1 As shown, the twist angle is 60°.

[0078] 2) The SEM image of the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material prepared in Example 1 is as follows: Figure 2 As shown. Figure 2 It can be seen that the surface of the prepared composite material has a large number of porous structures and spiral carbon nanotubes are attached.

[0079] 3) The HR-TEM image of the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material prepared in Example 1 is as follows: Figure 3 As shown. Figure 3 It can be seen that the iron carbide nanoparticles are relatively completely encapsulated in the helical carbon nanotubes.

[0080] 4) The structural model of the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material prepared in Example 1 is as follows Figure 4 The modeling software is VASP, and the long-range van der Waals interaction is described by DFT-D3 method. To avoid mutual interference between periodic images, the periodic images are perpendicular to the Fe 3 The direction of the C surface model has been increased Density functional theory calculations show that the N element is important for anchoring Fe 3 C is crucial to the inner wall of carbon nanotubes. 2 O 8 2- In Fe 3C, the adsorption energies on the surfaces of conventional carbon nanotubes and helical carbon nanotubes are -0.7, -1.12 and -1.67 eV respectively. 2 O 8 2- Fe 3 C. The surface transfer of electrons on conventional carbon nanotubes and helical carbon nanotubes is 0.22, 0.23 and 0.26 respectively. Therefore, the helical carbon nanotubes can increase the adsorption capacity and catalytic activity of nitrogen-doped helical carbon nanotubes for persulfate.

[0081] 3) The X-ray crystal diffraction patterns of the materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 are as follows: Figure 5 As shown. Figure 5 It can be seen that the surface of the material of Example 1 mainly contains iron carbide phase (Fe 3 C, JCPDS: 35-0072), ferrous carbide phase (Fe 2 C, JCPDS: 26-0782), iron nitride phase (Fe 3 N, JCPDS: 49-1664) and graphite (Graphite, JCPDS: 26-1079). The surface of the material of Comparative Example 1 mainly contains graphite (Graphite, JCPDS: 26-1079). The surface of the material of Comparative Example 2 mainly contains iron carbide (Fe 3 C, JCPDS: 35-0072), ferrous carbide phase (Fe 3 C, JCPDS: 26-0782) and graphite phase (Graphite, JCPDS: 26-1079).

[0082] 4) Raman images of the materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 are as follows: Figure 6 shown. Figure 6 I D / I G The numerical value can reflect the defect degree of the material. The surface defect degree of the material in Example 1 (I D / I G =1.18) is not greater than that of Comparative Example 1 (I D / I G =2.18), Comparative Example 2 (I D / I G =1.23), and the value of comparative example 3 (I D / I G =1.51), it can be inferred that the degradation of BPA by this system has little correlation with the defect degree of the material.

[0083] 5) The electron transfer rates of bisphenol A and sodium persulfate reacting on the surfaces of the materials of Example 1, Comparative Example 1 and Comparative Example 2 were compared by linear sweep voltammetry.

[0084] First, the prepared 0.5% Nafion membrane solution and the catalytic material (the composite material prepared in Example 1, Comparative Example 1 or Comparative Example 2) were ultrasonically treated for 2 h at an ultrasonic power of 150 W and then titrated on glassy carbon to ensure a coverage concentration of 0.3 mg / cm 3 , as the working electrode. At the same time, AgCl was used as the reference electrode, carbon rod as the auxiliary electrode, and a solution containing 3mmol / L sodium persulfate and 0.078mmol / L bisphenol A was used as the electrolyte. The linear sweep voltammetry (LSV) method was used to test the electron transfer rate of the reaction on the surface of the material on a CHI660E electrochemical workstation (Shanghai Chenhua). The results are shown in Figure 7 .

[0085] from Figure 7 It can be observed that in Example 1, the peak current of the reaction between persulfate and bisphenol A on the surface of the material reaches a maximum value, suggesting that the number of electron gains and losses is the highest under this condition, and thus the electron transfer rate is the fastest. These results show that in Fe 3 Introducing a nitrogen source (melamine) during the synthesis of C nanomaterials can increase the crystal form of the iron carbide phase, while introducing part of the iron nitride phase and graphene phase. In contrast, in Comparative Example 1, no crystal form of the iron carbide phase was observed, and in Comparative Example 2, although the lattice phase of iron carbide appeared, its peak was relatively weak. Adding helical carbon nanotubes can increase part of the ferrous carbide phase. Furthermore, the simultaneous introduction of a nitrogen source (melamine) and carbon nanotubes can increase the defect sites on the surface of the material. 3 The introduction of iron nitride phase, ferrous carbide phase and graphene phase into C nanomaterials will increase the Fe 3 In addition, the newly introduced graphene phase significantly improves the electron transfer efficiency of the material, while the large increase in defect sites gives the composite material extremely high catalytic activity, which helps to improve its efficiency in treating refractory organic pollutants in wastewater.

[0086] Test Example 1

[0087] Effect of different materials on the removal of bisphenol A by sodium persulfate activation:

[0088] 50 mL of 78 μM bisphenol A aqueous solution was placed in a conical flask, and then the pH value was adjusted to 4 using a 0.5 M sulfuric acid solution. Next, 80 mg of the composite material prepared in Example 1 was added to the solution, and then oscillated at a rate of 200 r / min in a constant temperature oscillator for 20 min. Subsequently, sodium persulfate was added to a concentration of 0.2 mM, and the degradation reaction was started at 25 ° C. At 2, 5, 10, 15 and 30 min time points of the reaction, 0.5 mL of sample was taken respectively, added to 0.5 mL of methanol, and filtered through a 0.22 μm polytetrafluoroethylene (PTFE) filter. Finally, the content of bisphenol A in the sample was detected using a high performance liquid chromatograph (Agilent 1200).

[0089] The same method as above was used to test the composite material of Example 1 by replacing it with the materials of Comparative Example 1, Comparative Example 2 and Comparative Example 3. Figure 8 The figures are the effects of removing bisphenol A from the composite materials of Example 1 and Comparative Examples 1 to 3, wherein -20 to 0 min represents the adsorption time, and 0 to 90 min represents the degradation time.

[0090] according to Figure 8 It shows that at room temperature, the degradation rate of bisphenol A by 0.2 mM sodium persulfate does not exceed 5%. The materials of Example 1, Comparative Example 1 and Comparative Example 2 have weak adsorption effects on bisphenol A within 20 minutes, and their degradation rates of bisphenol A are 7.5%, 4.5% and 8.4%, respectively. After adding sodium persulfate oxidant, the degradation rate of bisphenol A by activated sodium persulfate at room temperature in the material of Example 1 can reach 78.6% within 30 minutes, while the degradation rates of bisphenol A by activated sodium persulfate at room temperature in the materials of Comparative Example 1 and Comparative Example 2 are 32.5% and 31.3%, respectively. Bisphenol A is mainly degraded by non-oxidative free radicals or direct electron transfer pathways. These results show that the material of Example 1 can efficiently repair bisphenol A pollution in water bodies containing organic matter by activating the sodium persulfate oxidation system at room temperature. The preparation of composite iron carbide-based materials by encapsulating iron carbide nanomaterials in modified carbon nanotubes can significantly improve the performance of iron carbide, porous carbon and carbon nanotubes in activating sodium persulfate to produce non-oxidative free radicals or direct electron transfer pathways, thereby improving the application prospects of iron carbide-based materials.

[0091] Test Example 2

[0092] Effect of reaction temperature on the removal of bisphenol A by sodium persulfate activation of the composite material prepared in Example 1:

[0093] 50 mL of 78 μM bisphenol A aqueous solution was added to a conical flask, and the pH value of the bisphenol A aqueous solution was adjusted to 3 using a 0.5 M sulfuric acid solution. Subsequently, 80 mg of the composite material prepared in Example 1 was added thereto, and after oscillating at room temperature in a constant temperature oscillator for 20 min, sodium persulfate was added to make its concentration 0.2 mM, and the temperature was raised to 45° C. to start the degradation reaction. At 30 min after degradation, 0.5 mL of the sample was taken, added to 0.5 mL of methanol, and filtered through a 0.22 μm PTFE filter. Finally, the content of bisphenol A in the sample was detected by high performance liquid chromatography.

[0094] The reaction temperature was changed to 25°C, 30°C, 35°C and 40°C respectively. The other conditions were the same as the above method. The effects of different reaction temperatures on the removal of bisphenol A by the sodium persulfate system activated by the material in Example 1 were compared. The results are shown in Fig. 9 shown.

[0095] according to Fig. 9 It shows that at 45°C, the removal rate of bisphenol A within 30 minutes reached 94.3%, while at 25°C, 30°C, 35°C and 40°C, the removal rates of bisphenol A within 30 minutes were 78.6%, 80.0%, 85.4% and 88.9%, respectively. The results show that in the range of 25-45°C, the temperature increase significantly promotes the removal effect of sodium persulfate on bisphenol A catalyzed by the nitrogen-doped iron carbide composite material wrapped in spiral carbon nanotubes. In addition, above 45°C, the removal rate of bisphenol A is slightly improved or almost unchanged. It is worth noting that the materials studied in this study still maintain good stability after thermal energy injection and are not easy to age. Compared with traditional iron-carbon materials, the materials of the present invention significantly improve the performance of activated sodium persulfate in degrading pollutants, thereby improving the application value of iron carbide-based nanomaterials.

[0096] Test Example 3

[0097] Effect of pH value on the removal of bisphenol A by sodium persulfate activated composite material prepared in Example 1:

[0098] Add 50 mL of 78 μM bisphenol A aqueous solution to a conical flask, and adjust the pH to 3 using 0.5 M sulfuric acid solution. Subsequently, add 80 mg of the composite material prepared in Example 1 to the bisphenol A aqueous solution, oscillate at room temperature in a constant temperature oscillator for 20 min, then add sodium persulfate to a concentration of 2 mM, raise the temperature to 45 ° C, and start the degradation reaction. Take 0.5 mL of the sample at 30 min after the reaction, add it to 0.5 mL of methanol, and filter it through a 0.22 μm PTFE filter. Finally, use a high performance liquid chromatograph to detect the content of bisphenol A in the sample.

[0099] The pH value of the 78 μM bisphenol A aqueous solution was adjusted to 5, 7, 9 and 11 in sequence using 0.5 M sulfuric acid solution or 0.5 M NaOH aqueous solution, and other conditions were kept consistent with the above experiment. The effects of different pH conditions on the effect of the material activation sodium persulfate system in Example 1 on the removal of bisphenol A were compared. The specific results are shown in Fig.10 .

[0100] Depend on Fig.10 It can be seen that the removal rates of bisphenol A by the composite material catalyzed sodium persulfate system prepared in Example 1 were 83.5%, 72.1%, 60.7%, 57.6% and 19.1% respectively at pH values ​​of 3, 5, 7, 9 and 11. The results show that pH significantly affects the degradation rate of BPA, and has a faster reaction effect under acidic conditions.

[0101] Test Example 4

[0102] Effects of common inorganic anions on the removal of bisphenol A by sodium persulfate activated composite materials prepared in Example 1:

[0103] Add 50 mL of 78 μM bisphenol A aqueous solution and 1 mM NaCl aqueous solution to the conical flask to ensure that the Cl - The concentration is 1 mM. Subsequently, 32 mg of the composite material prepared in Example 1 was added to the bisphenol A aqueous solution, and after oscillating at room temperature in a constant temperature oscillator for 20 minutes, sodium persulfate was added to make its concentration 2 mM, and the initial pH of the reaction solution was adjusted to 4 using a 0.5 M sulfuric acid solution, and the degradation reaction was started at room temperature; 0.5 mL of the sample was taken at 30 minutes after the degradation, added to 0.5 mL of methanol, filtered through a 0.22 μm PTFE filter head, and then the content of bisphenol A in the sample was detected by high performance liquid chromatography.

[0104] The addition concentration of NaCl was changed to 2.5mM, 5mM and 10mM respectively, and other conditions were the same as the above method. The effect of the addition amount of chloride ions on the removal of bisphenol A by the sodium persulfate system activated by the material in Example 1 was compared. The results are as follows: Fig.11 shown.

[0105] according to Fig.11 The results show that after adding sodium persulfate at a concentration of 2mM, the degradation rates of bisphenol A after 30 minutes of degradation were 80.1%, 81.6%, 81.1%, and 89.5%, respectively. These results show that when the chloride ion dosage is in the range of 1 to 10mM, the increase of chloride ions will lead to a corresponding increase in the degradation rate of bisphenol A, but the adsorption rate will decrease. This is because chloride ions are adsorbed to the surface of the material, resulting in a decrease in the adsorption rate of bisphenol A, while chloride ions and sodium persulfate generate active substances such as free chlorine, thereby promoting the degradation process of bisphenol A.

[0106] The same concentration gradient was set and the same experimental method was used to add PBS buffer (1M Na 2 HPO 4 :1MNaH 2 PO 4 ), replace the NaCl aqueous solution with PBS buffer, adjust the PBS concentration gradient with Cl - The same solution volume was controlled to be 50 mL, and the effect of the amount of PBS added on the removal of bisphenol A by the sodium persulfate system activated by the composite material of Example 1 was compared. The results are as follows Fig.12 shown.

[0107] according to Fig.12 As shown, after adding 2 mM sodium persulfate and 30 min degradation, the degradation rates of bisphenol A were 58.0%, 55.1%, 41.8% and 36.4% respectively. These results show that when the PBS dosage increases within the range of 1 to 10 mM, the degradation rate of bisphenol A is significantly inhibited.

[0108] Test Example 5

[0109] Effect of removing bisphenol A from different wastewaters by activating sodium persulfate with the composite material prepared in Example 1:

[0110] 50 mL of 78 μM bisphenol A solution was injected into a conical flask, and then 32 mg of the composite material of Example 1 was added thereto, and the mixture was placed in a constant temperature oscillator and oscillated at room temperature for 20 min. Subsequently, sodium persulfate was added to a concentration of 5 mM, and a 0.5 M sulfuric acid solution was used to adjust the pH of the reaction solution to 4, and a degradation reaction at room temperature was started; after 20 min of oscillation at room temperature and 30 min of degradation reaction, 0.5 mL of sample was taken respectively, and added to 0.5 mL of methanol, and then filtered through a 0.22 μm PTFE filter, and finally the bisphenol A content in the sample was detected by high performance liquid chromatography.

[0111] 50 mL of 78 μM bisphenol A solution was prepared using actual wastewater from the Zhejiang Xianju Pharmaceutical Chemical Park. Other conditions were the same as the above method. The effects of different water bodies on the removal of bisphenol A by the composite material activated sodium persulfate system in Example 1 were compared. The results are as follows: Fig.13 As shown, the pure water is the ultrapure water in the above method.

[0112] Fig.13The data show that the adsorption removal rate of bisphenol A in different wastewaters by the composite material prepared in Example 1 within 20 minutes is 8.4% (Shou Chuang effluent), 8.4% (Medical and Chemical Park groundwater), 8.5% (Xian Yao Park groundwater), 7.8% (4# extraction well groundwater in the factory), 7.3% (groundwater on the south side outside the factory), and 9.3% (Chailingxia groundwater). After adding sodium persulfate and degrading for 30 minutes, the removal rate of bisphenol A by the activated sodium persulfate system of the composite material prepared in Example 1 under different actual wastewater conditions is 35.7% (Shou Chuang effluent), 54.2% (Medical and Chemical Park groundwater), 55.3% (Xian Yao Park groundwater), 32.3% (4# extraction well groundwater in the factory), 42.4% (groundwater on the south side outside the factory), and 43.6% (Chailingxia groundwater). These results indicate that the composite material prepared in Example 1 can effectively catalyze the degradation of bisphenol A in actual industrial wastewater with complex components by activating the sodium persulfate system at low temperature, and has significant application potential.

[0113] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for removing bisphenol A from wastewater by catalyzing persulfate with nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material, characterized in that: The following steps are involved: The wastewater containing bisphenol A, the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material and persulfate are mixed for degradation; The method for preparing the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material comprises the following steps: An iron source, a carbon source and a nitrogen source are mixed, the obtained mixture is mixed with the helical carbon nanotubes, and the mixture is dried and calcined in sequence to obtain a nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material; The usage ratio of the bisphenol A-containing wastewater to the nitrogen-doped helical carbon nanotube-wrapped iron carbide composite material is 47-53 mL: 32-80 mg.

2. The method according to claim 1, characterized in that The persulfate includes sodium persulfate, potassium persulfate, sodium monopersulfate or potassium monopersulfate; the concentration of the persulfate in the bisphenol A-containing wastewater is 0.2-3.5 mM, the degradation temperature is 20-50° C., the pH value is 3-11, and the degradation time is 20-40 min.

3. The method according to claim 1, characterized in that The iron source comprises a ferric chloride solution; the carbon source comprises a glucose solution; the nitrogen source comprises a melamine solution; and the volume ratio of the ferric chloride solution, the glucose solution and the melamine solution is 30-50:50-70:80-120.

4. The method according to claim 3, characterized in that The solvents used in the ferric chloride solution are anhydrous ethanol and water, and the volume ratio of the anhydrous ethanol to water is 1-2:1-2; the dosage ratio of anhydrous ferric chloride to the solvent in the ferric chloride solution is 2-4g:30-50mL.

5. The method according to claim 3, characterized in that: The glucose solution comprises glucose, water and anhydrous ethanol, and the usage ratio of the glucose, water and anhydrous ethanol is 2-4 g: 15-25 mL: 35-45 mL.

6. The method according to claim 3, characterized in that The solvents used in the melamine solution are anhydrous ethanol and water, and the volume ratio of the anhydrous ethanol to water is 1-2:1-2; the amount ratio of melamine to the solvent in the melamine solution is 1-3g:80-120mL.

7. The method according to claim 4, characterized in that The mass ratio of the helical carbon nanotubes to anhydrous ferric chloride is 0.4-0.6:2-4.

8. The method according to claim 1, characterized in that The temperature for mixing the mixture with the helical carbon nanotubes is 50-70° C. and the time is 1-3 hours; the temperature for drying is 160-200° C. and the time is 10-14 hours.

9. The method according to claim 1, characterized in that: The calcination is carried out in a protective atmosphere. The protective atmosphere includes nitrogen and / or argon; the calcination temperature is 700-900°C and the calcination time is 2-4h; The heating rate to the calcination temperature is 4-6°C / min.