Colossal magnetoresistance sensor and preparation method thereof, and current sensor

By using giant magnetoresistive sensors in the power system and using serpentine manganese oxide films and electrodes to convert the external magnetic field into voltage signals, the problem of incomplete measurement of existing current sensors is solved, and current measurement with a wide range is achieved in a small size. , simple structure and low cost, meeting the needs of the power system and improving the convenience of measurement.

CN118317683BActive Publication Date: 2024-10-25SOUTHERN POWER GRID DIGITAL GRID RESEARCH INSTITUTE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410743515.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-25
Estimated Expiration
2044-06-11

AI Technical Summary

Technical Problem

Existing current sensors in power systems have problems such as incomplete measurement, large size, high price, weak anti-electromagnetic interference capability, and low sensitivity, and cannot fully meet current measurement needs.

Method used

The giant magnetoresistive sensor is used, including forming a serpentine manganese oxide film and electrode with a perovskite structure on the substrate, using an external magnetic field to convert it into a voltage signal, and preparing it through pulsed laser deposition and mask-less photolithography processes to achieve current flow. Measurement.

Benefits of technology

It realizes current measurement with a wide range, has small size, simple structure and low cost, can meet the needs of current measurement in power systems, and improves the convenience of measurement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118317683B_ABST
    Figure CN118317683B_ABST
Patent Text Reader

Abstract

The present application relates to a colossal magnetoresistance sensor and a preparation method thereof, and a current sensor. The colossal magnetoresistance sensor comprises: a substrate; a serpentine manganese oxide film formed on the substrate, the manganese oxide film comprising a manganese oxide having a perovskite structure and a colossal magnetoresistance effect; two electrodes formed on the substrate, the two electrodes are respectively connected to the two ends of the serpentine manganese oxide film to convert the magnetic field strength of the external magnetic field excited by the current of the conductor to be measured into a voltage signal for output. The current sensor equipped with the colossal magnetoresistance sensor has a large range, and there is no precise requirement for the placement of the colossal magnetoresistance sensor, which improves the convenience of measurement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of integrated circuits, and in particular to a colossal magnetoresistive sensor and a preparation method thereof, and a current sensor. Background Art

[0002] With the development of smart grids, power systems have put forward higher requirements for current sensor technology. The current amplitude ranges from μA to kA, and the frequency range covers DC to MHz level. According to the size of the current amplitude, the types of currents that need to be measured in the power system mainly include small and medium currents (small amplitude and frequency, long duration), normal working currents (moderate amplitude, long duration) and transient currents (large amplitude, high frequency, short duration).

[0003] At present, there are mainly the following ways to detect current in power systems: current transformer, Rogowski coil, shunt, fiber optic current transformer, fluxgate current transformer and Hall current sensor. Among them, the current transformer based on the law of electromagnetic induction is only used in substations and power stations because it cannot measure DC current, and has the disadvantages of being bulky, expensive, and having limited bandwidth; Rogowski coil is mainly used to detect transient current due to its high bandwidth and large current measurement capability; the use of shunt will affect the normal operation of the circuit, and overcurrent may also damage the shunt; although the fiber optic current sensor has strong anti-electromagnetic interference ability, its structure is complex and expensive; the Hall current sensor has low sensitivity, is sensitive to temperature, and has low breakdown voltage, which limits its application in power systems; fluxgate current sensors are currently usually only used in calibration systems for laboratory equipment. Based on this, it is urgent to provide a current sensor that can fully meet the current measurement requirements in power systems. Summary of the invention

[0004] Based on this, it is necessary to provide a colossal magnetoresistance sensor with a wide measuring range, a preparation method thereof, and a current sensor.

[0005] In order to achieve the above object, the present invention provides a colossal magnetoresistive sensor, the colossal magnetoresistive sensor comprising:

[0006] substrate;

[0007] A serpentine manganese oxide film is formed on a substrate, wherein the manganese oxide film includes a manganese oxide having a perovskite structure and a colossal magnetoresistance effect;

[0008] Two electrodes are formed on the substrate and are respectively connected to the two ends of the serpentine manganese oxide film to convert the magnetic field intensity of the external magnetic field excited by the current of the wire to be tested into a voltage signal for output.

[0009] In one embodiment, the substrate includes at least one of a single crystal strontium titanium oxide substrate, a lanthanum aluminum oxide substrate and a single crystal aluminum oxide substrate, and / or the manganese oxide film includes at least one of lanthanum praseodymium calcium manganese oxide, lanthanum strontium manganese oxide, neodymium strontium manganese oxide and lanthanum barium manganese oxide, and / or the electrode includes tantalum and copper.

[0010] In one embodiment, the single crystal strontium titanium oxide substrate has an orientation of (100), the lanthanum aluminum oxide substrate has an orientation of (100), and the single crystal aluminum oxide substrate has an orientation of (0001).

[0011] In one embodiment, a current sensor is provided, comprising the above-mentioned giant magnetoresistive sensor, a coaxial line and a back-end processing circuit;

[0012] The coaxial line is perpendicular to the surface of the colossal magnetoresistance sensor and is welded to the colossal magnetoresistance sensor;

[0013] The back-end processing circuit is connected to the coaxial line to receive the electrical signal output by the giant magnetoresistive sensor through the coaxial line and convert the electrical signal into an electrical signal that meets the measurement requirements.

[0014] In one embodiment, the coaxial line comprises:

[0015] A central conductor, one end of the central conductor is connected to an output connection point on the substrate, and the other end of the central conductor is connected to a back-end processing circuit;

[0016] An insulating dielectric layer covering the outer circumference of the center conductor;

[0017] A shielding layer covers the outer periphery of the insulating dielectric layer, and the shielding layer is connected to another output connection point on the substrate to shield high-frequency noise;

[0018] The protective layer covers the outer periphery of the shielding layer.

[0019] In one embodiment, the current sensor further includes:

[0020] The functional protective layer covers the serpentine manganese oxide film and the electrode area.

[0021] In one embodiment, the back-end processing circuit includes a signal filtering and amplifying circuit, the input end of the signal filtering and amplifying circuit is connected to the coaxial line, and the signal filtering and amplifying circuit is used to filter and amplify the electrical signal output by the giant magnetoresistive sensor and then output it through the output end.

[0022] In one embodiment, a method for preparing a giant magnetoresistive sensor is provided, comprising the following steps:

[0023] obtaining a substrate;

[0024] In a vacuum environment of a deposition chamber, a pulsed laser deposition process is used to deposit a manganese oxide thin film on a substrate;

[0025] The manganese oxide film was patterned into a serpentine pattern using maskless photolithography and argon plasma etching;

[0026] Electrode regions are formed at both ends of the formed manganese oxide film by using maskless photolithography and lift-off methods, and electrodes are grown in the electrode regions by using magnetron sputtering.

[0027] In one embodiment, a pulsed laser deposition process is used to deposit a manganese oxide thin film on a substrate, and the process also includes:

[0028] ultrasonically cleaning the substrate for a first time period using acetone, alcohol and deionized water in sequence;

[0029] The residual liquid on the surface of the substrate is blown dry with nitrogen, and then dried in an oven at a first temperature for a second period of time.

[0030] In one embodiment, the preparation method further comprises the steps of:

[0031] The mechanical pump, the electromagnetic valve and the bypass valve are opened in sequence until the vacuum degree of the deposition chamber is drawn below a preset vacuum value, and then the bypass valve is closed;

[0032] Open the molecular pump and gate valve until the vacuum degree of the chamber is drawn to the preset value.

[0033] The giant magnetoresistance sensor and its preparation method, and current sensor provided by the present application, the serpentine manganese oxide film on the substrate is connected to the electrode, and as the external magnetic field increases, the magnetoresistance change rate of the serpentine manganese oxide film increases proportionally, and the increase of the external magnetic field is correlated with the change of the current of the conductor to be measured, so the size of the external magnetic field can be determined based on the size of the voltage signal output by the giant magnetoresistance sensor, and then the current of the conductor to be measured can be determined. The giant magnetoresistance sensor provided in the embodiment of the present application has a large range of magnetic field strength sensing, so when it is applied to the current measurement scenario, it can fully meet the current measurement needs of the power system, and there is no precise requirement for the placement of the giant magnetoresistance sensor, which improves the convenience of measurement. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 is a flow chart of a method for preparing a giant magnetoresistive sensor provided in an embodiment;

[0036] Figure 2 is an X-ray diffraction diagram of an LSMO film epitaxially grown on an STO substrate in one embodiment;

[0037] Figure 3 This is a schematic diagram of the connection between a giant magnetoresistive sensor and a coaxial cable in one embodiment;

[0038] Figure 4 A schematic diagram of the structure of a serpentine manganese oxide film and electrodes at both ends of the film in a colossal magnetoresistive sensor in one embodiment;

[0039] Figure 5 is a schematic diagram of the electrical structure of a current sensor in one embodiment;

[0040] Figure 6 1 is a magnetoresistance test result of a giant magnetoresistance sensor in different directions of an external magnetic field in one embodiment. DETAILED DESCRIPTION

[0041] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. Embodiments of the present application are provided in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.

[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0043] It should be understood that when an element or layer is referred to as being "on," "adjacent to," "connected to," or "coupled to" another element or layer, it can be directly on, adjacent to, connected to, or coupled to the other element or layer, or there may be intervening elements or layers. In contrast, when an element is referred to as being "directly on," "directly adjacent to," "directly connected to," or "directly coupled to" another element or layer, there are no intervening elements or layers.

[0044] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that, in addition to the orientations shown in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, an element or feature described as "under other elements" or "under it" or "under it" will be oriented as being "above" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include additional orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.

[0045] When used herein, the singular forms "a", "an", and "said / the" may also include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "include / comprise" or "have" and the like specify the presence of stated features, wholes, steps, operations, components, parts, or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, wholes, steps, operations, components, parts, or combinations thereof. At the same time, in this specification, the term "and / or" includes any and all combinations of the relevant listed items.

[0046] Embodiments of the invention are described herein with reference to cross-sectional views which are schematic representations of idealized embodiments (and intermediate structures) of the invention, such that variations in the shapes shown due to, for example, manufacturing techniques and / or tolerances are anticipated. Thus, embodiments of the invention should not be limited to the particular shapes of the regions shown herein, but rather include deviations in shapes due to, for example, manufacturing techniques. Thus, the regions shown in the figures are schematic in nature, their shapes do not represent the actual shapes of the regions of the device, and do not limit the scope of the invention.

[0047] Magnetoresistive current sensor is a new type of current sensor that uses magnetoresistive effect to measure current. It includes giant magnetoresistive current sensor, tunnel resistance current sensor and colossal magnetoresistive current sensor. Current sensor based on magnetoresistive effect can measure current signals from DC to high frequency, and has the advantages of high sensitivity, small size, simple structure and low cost. It is a product with great potential for current measurement in power systems. Among them, current sensor based on colossal magnetoresistive effect only requires a single layer of magnetic material, with a very simple structure and a wide linear response range.

[0048] See also Figure 1 The present invention provides a method for preparing a giant magnetoresistive sensor, comprising the following steps:

[0049] S120, obtaining a substrate. After obtaining the substrate, the substrate may be cleaned. The cleaning process may be implemented in a variety of ways, aiming to clean the surface of the substrate and keep it dry. The substrate may include a variety of manganese oxides, for example, may include a single crystal strontium titanium oxide substrate oriented (100), and a lanthanum strontium manganese oxide (LSMO) film epitaxially grown on the single crystal strontium titanium oxide substrate.

[0050] To ensure that the substrate does not move during the thin film growth process, the cleaned substrate can be glued to the sample holder. For example, the substrate can be glued to the sample holder using silver paste. The glue operation can prevent the sample from falling off during the growth process.

[0051] Then, the sample holder with the substrate attached is placed in the deposition chamber, and the chamber door is closed to evacuate the chamber. The evacuation operation can be achieved by a vacuum pump, etc., depending on the deposition chamber structure selected in the manufacturing process.

[0052] S140, in the vacuum environment of the deposition chamber, a pulsed laser deposition process is used to deposit a manganese oxide thin film on the substrate. A vacuum environment refers to an environment close to a vacuum. For example, the vacuum degree of the cavity can be evacuated to a preset value by a vacuum pumping operation. When the preset value is reached, it is considered that the vacuum environment required for thin film growth is satisfied. That is, the preset value refers to a value that can characterize that the vacuum value in the cavity reaches the vacuum condition required for thin film growth. The deposition of a manganese oxide thin film on the substrate using a pulsed laser deposition process can be performed by using manganese oxide as a target material and using pulsed laser deposition technology to deposit a thin film on a selected single crystal strontium titanium oxide substrate with an orientation of (100).

[0053] X-ray diffraction analysis can be performed on the deposited manganese oxide film. After analysis, it can be found that the deposited manganese oxide film is a high-quality single-crystal epitaxial film, which is the key factor in the generation of the giant magnetoresistance effect. Therefore, during the preparation process, X-ray diffraction analysis can be performed on the deposited manganese oxide film. If it does not meet the requirements, the film deposition operation can be continued or the film can be grown again on a new substrate (based on Figure 2 The X-ray diffraction analysis results are shown).

[0054] S160, a manganese oxide film is formed into a serpentine pattern by maskless lithography and argon plasma etching.

[0055] S180, using maskless photolithography and lift-off methods, electrode regions are formed at both ends of the formed manganese oxide film, and magnetron sputtering is used to grow electrodes in the electrode regions.

[0056] The giant magnetoresistive sensor formed by the preparation method provided in the embodiment of the present application has a structure as follows: Figure 3-Figure 4As shown, the electrodes are connected to the power supply of the Colossal Magnetoresistive Sensor. When the power is supplied, the Colossal Magnetoresistive Sensor is subjected to an external magnetic field. When the electrons move in the lattice of the substrate, they are scattered by the lattice ions, which results in a decrease in the mean free path of the electrons. When the mean free path of the electrons is smaller than the specific size, they will be bound by the lattice and unable to move. At this time, the resistivity of the serpentine manganese oxide thin film material will increase with the increase of the external magnetic field. This phenomenon is the Colossal Magnetoresistive Effect. Its Colossal Magnetoresistive Magnetoresistive Change Rate MR can be expressed as:

[0057]

[0058] in, It represents the resistance of the magnetoresistive sensor when the external magnetic field is H. It represents the resistance of the Colossal Magnetoresistive Sensor when the external magnetic field is 0. As the external magnetic field increases, it can be seen that the magnetoresistance change rate of the serpentine manganese oxide film increases proportionally, and the increase of the external magnetic field is correlated with the change of the current of the conductor to be measured. Therefore, the size of the external magnetic field can be determined based on the size of the voltage signal output by the Colossal Magnetoresistive Sensor, and then the current of the conductor to be measured can be determined.

[0059] The giant magnetoresistive sensor formed by the preparation method provided in the embodiment of the present application can be applied to a current sensor. When it is applied to a current sensor, for example, it can be applied to Figure 5 In the current sensor shown, the coaxial line connects the giant magnetoresistance sensor and the back-end processing circuit to transmit the voltage signal output by the giant magnetoresistance sensor that can represent the strength of the external magnetic field to the back-end processing circuit for processing to achieve current measurement. In a test example, the magnetic field detection of the current sensor is tested, and the results are as follows: Figure 6 As shown. Under the action of a 1T external magnetic field, no matter how the orientation of the giant magnetoresistance sensor and the external magnetic field changes, the MR value of the giant magnetoresistance change rate is basically stable at 8.5%. And the MR value increases basically linearly with the increase of the external magnetic field, which shows that the magnetic field test range of the magnetoresistance sensor is very wide, that is, the current test range of the current sensor is very wide, that is to say, the working range of the sensor is wide. In summary, the giant magnetoresistance sensor formed by the preparation method provided in the embodiment of the present application has a large range when used in current measurement. And only a single layer of manganese oxide film is required, the structure is simple, and the volume is small.

[0060] In one embodiment, the step of obtaining a substrate comprises:

[0061] Using a selected manganese oxide (for example, lanthanum strontium manganese oxide) as a target, a pulsed laser deposition technique is used to perform thin film deposition on a selected single crystal substrate (for example, a single crystal strontium titanium oxide substrate with a (100) orientation);

[0062] ARP-3510T photoresist is spin-coated on the selected manganese oxide film using a coating machine; wherein the coating parameters of the coating machine can be a low speed of 600 rpm, a spin coating of 1 minute, a high speed of 4000 rpm, a spin coating of 2 minutes, and the photoresist thickness is about 2 microns.

[0063] After the sample material is spin-coated with the photoresist, it is dried in an oven; for example, it can be dried at 150 degrees Celsius for 20 minutes to form a substrate.

[0064] In one embodiment, cleaning the substrate comprises the following steps:

[0065] The substrate is ultrasonically cleaned with acetone, alcohol and deionized water in sequence for a first duration; for example, the first duration may be 5 minutes.

[0066] The liquid remaining on the surface of the substrate is blown dry with nitrogen, and then dried in an oven at a first temperature for a second time. Nitrogen is an inert gas and can dry the substrate without reacting with the substrate material. Oven drying can further ensure the dryness of the substrate. For example, the substrate can be dried in an oven at 115°C for 20 minutes to fully dry it.

[0067] By cleaning and drying the substrate, it can be ensured that no impurities are introduced during the growth of the manganese oxide film, thereby avoiding affecting the quality of the single crystal epitaxial film and the effect of the colossal magnetoresistance effect.

[0068] In one embodiment, the deposition chamber device is provided with a mechanical pump, a solenoid valve, a bypass valve, a molecular pump and a gate valve, and the vacuuming operation of the chamber includes the following steps:

[0069] Open the mechanical pump, solenoid valve and bypass valve in sequence until the vacuum of the chamber is pumped below the preset vacuum value and then close the bypass valve; the preset vacuum value can be 5 Pa. At this point, it is close to a vacuum environment and the bypass valve needs to be closed for further vacuuming operations.

[0070] Open the molecular pump and gate valve until the vacuum degree of the chamber is drawn to the preset value.

[0071] In one embodiment, the preset value is 2.0*10 -4 Pa.

[0072] By adopting the above-mentioned staged vacuum operation, the chamber can be evacuated to 2.0*10 -4 The vacuum degree of Pa, which is infinitely close to the vacuum environment, prevents the gas in the cavity from reacting with the substrate beyond the user's expectations during the subsequent film growth process, thereby ensuring the subsequent deposition effect of the manganese oxide film.

[0073] In one embodiment, the step of depositing a manganese oxide thin film using a pulsed laser deposition process comprises the following steps:

[0074] Raise the temperature in the deposition chamber to the preset growth temperature. When the preset growth temperature is below 500°C, the set temperature rise rate should be no greater than 10°C / min; when the preset growth temperature is above 500°C, the set temperature rise rate should be no greater than 5°C / min. Optionally, the preset growth temperature can be 700°C.

[0075] The oxygen flow rate and the gate valve are adjusted to balance the oxygen pressure in the chamber, so that the oxygen pressure in the chamber is stabilized at a first preset oxygen pressure and the oxygen flow rate is stabilized at a preset flow rate. Optionally, the preset flow rate may be 50 sccm.

[0076] The manganese oxide film is deposited by a pulsed laser deposition process until the thickness of the manganese oxide film reaches a preset thickness value; for example, it may be 60 nm, which may be specifically set based on sensitivity requirements.

[0077] After the deposition is completed, in-situ annealing is performed at a second preset oxygen pressure until it cools to room temperature; the annealing treatment can repair the lattice loss caused to the substrate during the manganese oxide implantation process and activate the ions in the manganese oxide; specifically, the substrate after the film deposition can be annealed by a rapid thermal annealing (RTA) process. Compared with the ordinary annealing process, the rapid thermal annealing process has a shorter annealing time, which can avoid long-term high temperature causing ion diffusion and reduce the instantaneous enhanced diffusion of ions. For example, in-situ annealing can be performed at an oxygen pressure of 100 Pa for 10 minutes, and then cooled to room temperature at a cooling rate of 5°C / min.

[0078] The second preset oxygen pressure is greater than the first preset oxygen pressure. For example, the first preset oxygen pressure may be 20Pa, and the second preset oxygen pressure may be 100Pa.

[0079] In order to better illustrate the implementation process of the preparation method provided in the embodiment of the present application, a specific example is used here for illustration:

[0080] A substrate can be obtained, wherein the substrate adopts a single crystal strontium titanium oxide (SrTiO3, hereinafter abbreviated as STO) with an orientation of (100), and the epitaxial film used for the substrate is a lanthanum strontium manganese oxide (LSMO) film, and its growth process adopts pulsed laser deposition.

[0081] Before depositing the thin film, the substrate was cleaned by ultrasonic cleaning with acetone, alcohol and deionized water for 5 minutes respectively, then dried with nitrogen and kept at 115°C in an oven for 20 minutes.

[0082] After taking it out, use silver paste to stick the STO substrate to the sample holder of pulsed laser deposition, and bake it on a hot plate at 115°C for 5 minutes to completely solidify the silver paste and stick the sample firmly to the sample holder to prevent the sample from falling off during the growth process.

[0083] After the sample holder cools to room temperature, place the sample holder with the substrate in the deposition chamber, then close the chamber door and evacuate the chamber. The specific steps are as follows: first open the mechanical pump, solenoid valve and bypass valve in sequence, wait for the chamber vacuum to be pumped below 5Pa, close the bypass valve, open the molecular pump and gate valve, wait for about 1 hour, and pump the chamber vacuum to 2.0*10 - 4 Pa.

[0084] When the vacuum reaches 2.0*10 -4 Pa, perform the following heating operations: when the growth temperature is below 500°C, set the temperature rise rate to no more than 10°C / min; when the growth temperature is above 500°C, set the temperature rise rate to no more than 5°C / min. Taking the growth temperature of 700°C as an example, when the temperature rises to 700°C, the oxygen pressure in the chamber is balanced by adjusting the oxygen flow rate and the gate valve. Here, the oxygen pressure is set to 20 Pa, and the oxygen flow rate needs to be set to 50sccm. After all parameters are adjusted, manganese oxide film deposition is performed with a film thickness of 60nm. After deposition is completed, in-situ annealing is performed at an oxygen pressure of 100 Pa for 10 minutes, and then cooled to room temperature at a cooling rate of 5°C / min. X-ray diffraction analysis is performed on the deposited manganese oxide film, as shown Figure 2 As shown, it was found that the deposited manganese oxide film was a high-quality single-crystal epitaxial film, which is the key factor in the generation of the giant magnetoresistance effect. Then, the manganese oxide film was made into a serpentine pattern by maskless lithography and argon plasma etching, and then tantalum / copper / tantalum metal electrodes were grown by magnetron sputtering using maskless lithography and lift-off.

[0085] In one embodiment, the preparation method steps may include:

[0086] Step 1, using the selected manganese oxide as the target material, here lanthanum strontium manganese oxide is selected, and using pulsed laser deposition technology to deposit a thin film with a thickness of about 60nm on the selected single crystal substrate, here a single crystal strontium titanium oxide substrate with an orientation of (100) is selected.

[0087] Step 2, on the grown lanthanum strontium manganese oxide film, use a coating machine to spin-coat ARP-3510T photoresist, the coating parameters are low speed 600 rpm, spinning for 1 minute, high speed 4000 rpm, spinning for 2 minutes, and the photoresist thickness is about 2 microns.

[0088] Step 3, drying the sample processed in step 2 in an oven at 150 degrees for 20 minutes.

[0089] Step 4: Use maskless lithography to expose the required serpentine pattern. A DS-2000 / 14K maskless single-sided laser lithography machine can be used.

[0090] Step 5, developing the sample processed in step 4 to obtain the desired pattern. In this step, the sample is developed for 30 seconds using developer AR300-26 and deionized water in a ratio of 1:2, and then the developer on the sample surface is rinsed with distilled water, and then the sample surface is dried with nitrogen.

[0091] Step 6, fix the sample processed in step 5 to the loading position of DISC-IBE-150C ion etcher with silicone grease. The preferred parameters of the etcher are as follows: the sample stage speed is 8 rpm, the angle is -20 °, the voltage of the neutralizer is set to 20V, the cathode voltage of the ion source is set to 13.5V, the anode voltage is set to 50V, the screen voltage is 500V, the acceleration voltage is 200V, the neutralization current is 9A, the reaction gas is argon, and the etching time is 10 minutes. Here, the etching time should not be too long or too short. Too long a time will cause the serpentine pattern protected by the photoresist to be damaged, and too short a time will cause the thin films in other areas that need to be removed to not be completely etched.

[0092] Step 7, de-resist the sample processed in step 6 by soaking the sample in acetone for 3-5 hours to remove the photoresist, then clean the sample with alcohol and deionized water, and then blow dry with nitrogen.

[0093] Step 8, spin-coating the sample processed in step 7 with photoresist and drying it. For specific parameters, refer to steps 2 and 3.

[0094] Step 9, using maskless photolithography technology to expose the required square electrode structure, the electrode structure is located on both sides of the serpentine sample. The specific parameters refer to step 4. The difference here is that the photoresist in the square electrode area is removed, and the photoresist in other areas is retained.

[0095] Step 10, developing the sample processed in step 9 to obtain the desired pattern. For specific parameters, refer to step 5.

[0096] Step 11, the sample processed in step 10 is placed in a magnetron sputtering apparatus for tantalum / copper / tantalum electrode growth, the thickness of tantalum is 10nm, and the thickness of copper is 100nm. The vacuum in the sample chamber is evacuated to below 8×10-6Torr, and then the sample is sent to the growth chamber for electrode growth, the argon flow rate is 28.7sccm, the pressure is 3mTorr, and the DC sputtering power is 30W at room temperature.

[0097] Step 12, degumming the sample processed in step 11, with reference to step 7 for the specific process, to obtain a colossal magnetoresistive sensor.

[0098] By growing a lanthanum strontium manganese oxide thin film on a (100) oriented single crystal strontium titanium oxide (STO) substrate and etching it into a serpentine magnetoresistive strip, when it is applied to a current sensor, the magnetic field strength is measured by detecting the change in magnetoresistiveness when an external magnetic field exists. According to the Biotsafar law, the magnetic field generated by the current-carrying wire can be measured to determine the magnitude of the current. The present application utilizes the Biotsafar law and the colossal magnetoresistive effect. The current sensor equipped with the colossal magnetoresistive sensor obtained by the above preparation method has the advantage of ultra-large range (greater than 1 Tesla).

[0099] It should be understood that, although the various steps in the flow chart are shown in sequence according to the indication of the arrows, these steps are not necessarily executed in sequence according to the order indicated by the arrows. Unless there is a clear description in this article, there is no strict order restriction on the execution of these steps, and these steps can be executed in other orders. Moreover, at least a part of the steps in the figure may include multiple steps or multiple stages, and these steps or stages are not necessarily executed at the same time, but can be executed at different times, and the execution order of these steps or stages is not necessarily to be carried out in sequence, but can be executed in turn or alternately with other steps or at least a part of the steps or stages in other steps.

[0100] Please continue reading Figure 3 and Figure 4 As shown, the present invention further provides a giant magnetoresistive sensor 20, and the giant magnetoresistive sensor 20 includes:

[0101] Substrate 21;

[0102] A serpentine manganese oxide film 22 is formed on a substrate 21, wherein the manganese oxide film 22 includes a manganese oxide having a perovskite structure and a colossal magnetoresistance effect;

[0103] Two electrodes 23 are formed on the substrate 21 and are respectively connected to two ends of the serpentine manganese oxide film 22 to convert the magnetic field intensity B of the external magnetic field excited by the current I of the wire 10 to be tested into a voltage signal for output.

[0104] The functions of the giant magnetoresistive sensor 20 provided in the embodiment of the present application can be realized based on the introduction in the above embodiment and will not be elaborated here.

[0105] In one embodiment, the substrate 21 includes at least one of a single crystal strontium titanium oxide substrate, a lanthanum aluminum oxide substrate, and a single crystal aluminum oxide substrate, and / or the manganese oxide film 22 includes at least one of lanthanum praseodymium calcium manganese oxide, lanthanum strontium manganese oxide, neodymium strontium manganese oxide, and lanthanum barium manganese oxide, and / or the electrode 23 includes tantalum and copper. The electrode 23 may be a tantalum / copper / tantalum multilayer structure.

[0106] In one embodiment, the single crystal strontium titanium oxide substrate has an orientation of (100), the lanthanum aluminum oxide substrate has an orientation of (100), and the single crystal aluminum oxide substrate has an orientation of (0001).

[0107] The giant magnetoresistance sensor 20 provided in the embodiment of the present application can measure a magnetic field strength of up to 1T, and in a test, no matter how the angle between the giant magnetoresistance sensor 20 and the external magnetic field changes, its magnetoresistance change rate is basically stable at 8.5%. Compared with traditional giant magnetoresistance sensors and tunnel magnetoresistance sensors, the giant magnetoresistance sensor 20 provided in the embodiment of the present application has no precise requirements for the placement when testing the magnetic field generated by the energized wire. On the basis of meeting the large-scale test in application scenarios such as electricity, it also greatly improves the convenience of measurement, which is conducive to improving the work efficiency of the power system monitoring link.

[0108] In one embodiment, if Figure 5 As shown, a current sensor is provided, comprising the above-mentioned giant magnetoresistive sensor 20, a coaxial line 30 and a back-end processing circuit 40;

[0109] The coaxial line 30 is perpendicular to the surface of the giant magnetoresistive sensor 20 and is welded to the giant magnetoresistive sensor 20;

[0110] The back-end processing circuit 40 is connected to the coaxial line 30 to receive the electrical signal output by the giant magnetoresistive sensor 20 via the coaxial line 30 and convert the electrical signal into an electrical signal that meets the measurement requirements.

[0111] The coaxial line 30 is connected to the back-end processing circuit 40, which can adopt a typical open-loop structure. The giant magnetoresistive sensor 20 converts the magnetic field strength into a voltage signal, and the output voltage signal can be amplified to a suitable level by the back-end processing circuit 40 such as a typical signal filtering and amplification circuit, so as to facilitate subsequent measurement.

[0112] In one embodiment, if Figure 3 As shown, the coaxial line 30 comprises:

[0113] A central conductor 31, one end of the central conductor 31 is connected to an output connection point on the substrate, and the other end of the central conductor 31 is connected to a back-end processing circuit;

[0114] A layer of insulating medium 32 covering the outer periphery of the central conductor 31;

[0115] A shielding layer 33 covers the outer periphery of the insulating medium 32 layer, and the shielding layer 33 is connected to another output connection point on the substrate to shield high-frequency noise;

[0116] The protection layer 34 covers the outer periphery of the shielding layer 33 .

[0117] In one embodiment, the current sensor further includes:

[0118] The functional protection layer (not shown) covers the serpentine manganese oxide film and the electrode area. The coaxial line 30 is welded perpendicular to the film surface of the giant magnetoresistive sensor 20, and then the functional layer area of ​​the giant magnetoresistive sensor 20 is covered with a material such as hot melt adhesive to form a functional protection layer to protect the functional layer of the giant magnetoresistive sensor 20 from atmospheric conditions and strengthen the welded joint.

[0119] In one embodiment, the back-end processing circuit 40 includes a signal filtering and amplifying circuit, the input end of which is connected to the coaxial line 30, and the signal filtering and amplifying circuit is used to filter and amplify the electrical signal output by the giant magnetoresistive sensor 20 and then output it through the output end. The signal filtering and amplifying circuit may specifically include a filtering circuit and an amplifying circuit, and the filtering circuit is connected in series with the coaxial line 30 cable and then connected to the amplifying circuit to amplify the filtered voltage signal into a voltage signal of a suitable magnitude that meets the measurement requirements, and the voltage signal is used to characterize the current magnitude of the conductor 10 to be measured.

[0120] In the description of this specification, the description with reference to the terms "some embodiments", "other embodiments", "ideal embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic descriptions of the above terms do not necessarily refer to the same embodiment or example.

[0121] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features of the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0122] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A giant magnetoresistive sensor, characterized in that: The colossal magnetoresistive sensor comprises: substrate; A serpentine manganese oxide film is formed on the substrate, wherein the manganese oxide film comprises a manganese oxide having a perovskite structure and a colossal magnetoresistance effect; the manganese oxide film is a single crystal manganese oxide film; the manganese oxide film comprises at least one of lanthanum praseodymium calcium manganese oxide, lanthanum strontium manganese oxide, neodymium strontium manganese oxide and lanthanum barium manganese oxide; Two electrodes are formed on the substrate, and the two electrodes are respectively connected to the two ends of the serpentine manganese oxide film to convert the magnetic field intensity of the external magnetic field excited by the current of the wire to be tested into a voltage signal for output.

2. The giant magnetoresistive sensor according to claim 1, characterized in that: The substrate includes at least one of a single crystal strontium titanium oxide substrate, a lanthanum aluminum oxide substrate and a single crystal aluminum oxide substrate, and / or the electrode includes tantalum and copper.

3. The giant magnetoresistive sensor according to claim 2, characterized in that: The single crystal strontium titanium oxide substrate has an orientation of (100), the lanthanum aluminum oxide substrate has an orientation of (100), and the single crystal aluminum oxide substrate has an orientation of (0001).

4. A current sensor, characterized in that: It comprises a giant magnetoresistive sensor, a coaxial line and a back-end processing circuit as described in any one of claims 1 to 3; The coaxial line is perpendicular to the surface of the colossal magnetoresistive sensor and is welded to the colossal magnetoresistive sensor; The back-end processing circuit is connected to the coaxial line to receive the electrical signal output by the giant magnetoresistive sensor via the coaxial line and convert the electrical signal into an electrical signal that meets measurement requirements.

5. The current sensor according to claim 4, characterized in that: The coaxial line comprises: A central conductor, one end of which is connected to an output connection point on the substrate, and the other end of which is connected to the back-end processing circuit; An insulating dielectric layer covering the outer periphery of the central conductor; A shielding layer, covering the outer periphery of the insulating dielectric layer, and the shielding layer is connected to another output connection point on the substrate to shield high-frequency noise; The protective layer covers the outer periphery of the shielding layer.

6. The current sensor according to claim 4, characterized in that: Also includes: The functional protection layer covers the serpentine manganese oxide film and the electrode area.

7. The current sensor according to claim 4, characterized in that: The back-end processing circuit includes a signal filtering and amplifying circuit, the input end of which is connected to the coaxial line, and the signal filtering and amplifying circuit is used to filter and amplify the electrical signal output by the giant magnetoresistive sensor and then output it through the output end.

8. A method for preparing a colossal magnetoresistive sensor according to any one of claims 1 to 3, characterized in that: The steps include: obtaining a substrate; Depositing a manganese oxide thin film on the substrate using a pulsed laser deposition process in a vacuum environment of a deposition chamber; The manganese oxide film is formed into a serpentine pattern by maskless photolithography and argon plasma etching; Electrode regions are formed at both ends of the formed manganese oxide film by using maskless photolithography and lift-off methods, and electrodes are grown in the electrode regions by using magnetron sputtering.

9. The method for preparing a colossal magnetoresistive sensor according to claim 8, characterized in that: The method of depositing a manganese oxide thin film on the substrate by using a pulsed laser deposition process also includes: ultrasonically cleaning the substrate for a first time period using acetone, alcohol and deionized water in sequence; The residual liquid on the surface of the substrate is blown dry with nitrogen, and then dried in an oven at a first temperature for a second period of time.

10. The method for preparing a colossal magnetoresistive sensor according to claim 9, characterized in that: The method further comprises the steps of: The mechanical pump, the electromagnetic valve and the bypass valve are opened in sequence until the vacuum degree of the deposition chamber is drawn below a preset vacuum value, and then the bypass valve is closed; Open the molecular pump and gate valve until the vacuum degree of the chamber is drawn to the preset value.