A method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials

Through the production of preset precursor embryo body and buffer layer, the melt texture method and cleavage and grinding technology of the top seed crystals were successfully realized, and the recycling and reuse of REBCO block seed crystals was solved, solving the problem of waste and inconsistent performance in block preparation. , realizes high-quality and low-cost batch preparation.

CN118326491BActive Publication Date: 2024-12-06SOUTHWEST JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410307195.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-18
Publication Date
2024-12-06
Estimated Expiration
2044-03-18

AI Technical Summary

Technical Problem

During the preparation of REBCO high-temperature superconducting block materials, the waste and inconsistent performance of bulk seed crystals lead to high costs and difficult to control quality. The existing recycling technology is insufficient, which affects batch preparation.

Method used

By making preset precursor embryos and buffer layers, the seeds are processed by melt texture method of the top seed crystals, cleavage and grinding, and reused to grow high-quality REBCO high-temperature superconducting blocks.

Benefits of technology

Lossless seed crystal recovery is achieved, and multiple repeated growth of blocks with good morphology is successfully achieved, ensuring the consistency of magnetic levitation performance, reducing preparation costs, and improving resource utilization efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118326491B_ABST
    Figure CN118326491B_ABST
Patent Text Reader

Abstract

The present invention provides a method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials, which relates to the technical field of superconducting material recycling, including preparing a first precursor embryo and a first buffer layer, processing the original REBCO seed crystal and the first precursor embryo based on the top seed crystal melt texturing method, and obtaining the original REBCO high-temperature superconducting bulk material. Subsequently, the original bulk material is cleaved in a specific manner, and the REBCO seed crystal is recovered, and the REBCO seed crystal is polished. By repeated production, a second precursor embryo and a second buffer layer are obtained, and the recovered seed crystal is inserted into the second precursor embryo and assembled. Finally, the assembled second precursor embryo is treated again using exactly the same top seed crystal melt texturing method to obtain a REBCO high-temperature superconducting bulk material grown using the recovered seed crystal. The present invention can realize a lossless seed crystal recovery process, and can successfully grow a block with good morphology and consistent magnetic properties each time, and can achieve as many times of seed crystal recovery as possible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of superconducting material recycling, and in particular to a method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials. Background Art

[0002] The second major difficulty in mass production of high-temperature superconducting bulk materials is cost control and quality control. Due to the complex preparation process, long preparation cycle and low yield rate of REBCO high-temperature superconducting bulk materials, a batch of qualified samples will usually produce a large number of failed samples at the same time, and the expensive light rare earth elements contained in them can only be wasted as waste. The recycling technology of REBCO bulk materials has always been a hot research topic in this field.

[0003] In conventional processes, bulk seed crystals are usually peeled off from the top of the sample and discarded after the sample growth is completed, regardless of its expensive cost and complex preparation process. In addition to the cost issue, since the crystallinity of each seed crystal is not exactly the same, different seed crystals may require different temperature programs to prepare bulk materials, and the properties of the superconducting bulk materials induced by them may also vary greatly, which increases the trial and error cost and quality control cost of growing bulk materials. Therefore, in order to ensure that the superconducting properties of the samples are as consistent as possible to meet the needs of batch preparation, and to avoid the waste of bulk seed crystals containing expensive light rare earth elements in the preparation process of REBCO high-temperature superconducting bulk materials and thus reduce the preparation cost of REBCO bulk materials, a method for recycling and reusing REBCO bulk seed crystals is now needed. Summary of the invention

[0004] The purpose of the present invention is to provide a method for recycling and reusing REBCO bulk seed crystals for growing superconducting bulk materials, so as to improve the above problems. In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0005] The present application provides a method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials, comprising:

[0006] Prepare a first precursor body and a first buffer layer based on a preset REBCO high-temperature superconducting bulk material precursor body preparation method and a buffer layer preparation method;

[0007] The original REBCO seed crystal, the first precursor embryo and the first buffer layer are processed based on the top seed crystal melt texturing method to obtain the original REBCO high temperature superconducting bulk material;

[0008] Cleaving the original REBCO high temperature superconducting bulk material along a preset cleavage plane, and grinding and polishing the structure consisting of the first buffer layer and the REBCO seed crystal obtained by cleavage to obtain a recycled seed crystal;

[0009] Repeat the process to obtain a second precursor embryo and a second buffer layer, place the recycled seed crystal in the top center of the second precursor embryo, and coaxially insert the second buffer layer between the recycled seed crystal and the second precursor embryo to obtain an assembled second precursor embryo;

[0010] The assembled second precursor embryo body is subjected to the same heat treatment as the first precursor embryo body based on the top seed crystal melt texturing method to obtain a REBCO high temperature superconducting bulk material grown by using recycled seed crystals.

[0011] Preferably, the step of preparing the first precursor embryo and the first buffer layer based on the preset precursor embryo preparation method and the buffer layer preparation method comprises:

[0012] The original drugs were weighed according to the molar ratio of RE2O3:BaCO3:CuO=1:4:6 and 1:1:1, and were mixed to prepare RE123 original powder and RE211 original powder respectively;

[0013] The RE123 original powder and the RE211 original powder were prepared by solid phase sintering method to obtain purified RE123 powder and RE211 powder;

[0014] The purified RE123 powder and RE211 powder were weighed and mixed in a molar ratio of 1:0.35 to obtain a precursor powder, and 1 wt % of CeO2 powder was added to the precursor powder for mixing to obtain a precursor powder;

[0015] Weighing the precursor powder, putting it into a mold for pressing, and obtaining a first precursor embryo;

[0016] The purified RE123 powder, RE211 powder and CeO2 powder are weighed according to a preset ratio, put into a mold for pressing, and obtain a first buffer layer.

[0017] Preferably, the RE123 original powder and the RE211 original powder are prepared by a solid phase sintering method, comprising:

[0018] The RE123 raw powder was sintered in an air environment at 920° C. for 48 hours, and the RE211 raw powder was sintered in an air environment at 930° C. for 48 hours to obtain sintered RE123 powder blocks and RE211 powder blocks;

[0019] The sintered RE123 powder block and RE211 powder block are ground and sintered three times to obtain purified RE123 powder and RE211 powder.

[0020] Preferably, the purified RE123 powder, RE211 powder and CeO2 powder are weighed according to a preset ratio, and put into a mold for pressing to obtain a first buffer layer, comprising:

[0021] The purified RE123 powder and the purified RE211 powder are mixed in a molar ratio of 5:2, and the mixed RE123 powder, RE211 powder and 1 wt % of CeO2 are mixed again to obtain a mixed powder;

[0022] The mixed powder is placed in a cylindrical mold with a diameter of 6 mm and subjected to pressure pressing to obtain a cylindrical first buffer layer.

[0023] Preferably, the preset REBCO original seed crystal, the first precursor embryo and the first buffer layer are processed based on the top seed crystal melt texturing method to obtain the original REBCO high temperature superconducting bulk material, including:

[0024] Inserting the first buffer layer between the REBCO original seed crystal and the first precursor embryo to form a coaxial combined structure from top to bottom;

[0025] The combined structure is placed on an alumina ceramic plate and placed in a high-temperature furnace in an air atmosphere for texture growth, thereby obtaining an original YBCO high-temperature superconducting bulk material induced by REBCO original seed crystal growth.

[0026] Preferably, the first buffer layer is inserted between the REBCO original seed crystal and the first precursor embryo to form a coaxial combined structure from top to bottom, including:

[0027] A REBCO original seed crystal of 3 mm×3 mm×3 mm with a smooth cross section is selected, and the ab surface of the bottom of the REBCO original seed crystal is polished to obtain a processed REBCO original seed crystal;

[0028] The center axis of the processed REBCO original seed crystal perpendicular to the ground is aligned with the center axis of the first buffer layer and the center axis of the first precursor embryo respectively, and the REBCO original seed crystal is placed between the first buffer layer and the first precursor embryo to obtain a coaxial combined structure.

[0029] Preferably, placing the combined structure on an alumina ceramic plate and placing it in a high-temperature furnace in an air atmosphere for texture growth comprises:

[0030] The temperature in the high-temperature furnace starts from room temperature and rises to 900°C after 1 hour and is kept at this temperature for 3 hours. Then, the heating is continued for 1 hour, and the temperature in the high-temperature furnace is raised to 1055°C and is kept at this temperature for 1 hour.

[0031] The furnace temperature was lowered to 1005° C. within 30 minutes, and then the furnace temperature was lowered at a cooling rate of 0.2 K / h to 0.4 K / h, so that the REBCO original seed crystal in the furnace induced the growth of the first precursor embryo for 100 hours;

[0032] After the sample growth was completed, the temperature of the high-temperature furnace was lowered to room temperature within 3 h.

[0033] Preferably, RE in the REBCO bulk seed crystal is selected from Y, Gd, Sm and Nd.

[0034] Preferably, the cleaving of the original REBCO high temperature superconducting bulk material along a preset cleavage plane comprises:

[0035] Using a cutting device to cleave the original REBCO high-temperature superconducting bulk material along the crystal ab plane direction to obtain a REBCO bulk seed crystal with a first buffer layer with a thickness of 0.5 mm, wherein the crystal ab plane direction is a layered cross section of the layered structure on the original REBCO high-temperature superconducting bulk material;

[0036] The cleavage surface of the REBCO bulk seed crystal was ground and polished with 1000-grit sandpaper to obtain a REBCO recovery seed crystal.

[0037] Preferably, after obtaining the REBCO high temperature superconducting bulk material grown by using the recycled seed crystal, the method further comprises:

[0038] Recovering the seed crystals on the REBCO high-temperature superconducting bulk material grown using the recycled seed crystals, and performing grinding and polishing treatments on the REBCO high-temperature superconducting bulk material grown using the recycled seed crystals and the original REBCO high-temperature superconducting bulk material to obtain two completed growth bulk materials;

[0039] The two grown blocks were sent to a high temperature furnace with a flowing oxygen atmosphere for annealing, wherein the annealing temperature was 450° C. and the annealing time was 200 h, to obtain two REBCO high temperature superconducting blocks that had completed the annealing process;

[0040] The magnetic levitation force test was performed on two REBCO high temperature superconducting bulk materials that had completed the annealing process, and the magnetic levitation force test results of the two REBCO high temperature superconducting bulk materials that had completed the annealing process were obtained.

[0041] The beneficial effects of the present invention are:

[0042] The method of the present invention can realize a lossless seed crystal recovery process, and can successfully grow a block material with good morphology each time, and can realize as many seed crystal recovery times as possible. Through the present invention, REBCO high-temperature superconducting block materials can be repeatedly prepared from two aspects of growth morphology and magnetic levitation performance. In addition, the present invention ensures the relative position between the seed crystal and the solid solution by virtue of the property that the solid solution can maintain its own shape in the molten state, and reliably realizes the effect of repeatedly guiding the growth of the precursor embryo below.

[0043] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or be understood by implementing the embodiments of the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures particularly pointed out in the written description, claims, and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0045] Figure 1 It is a schematic flow chart of a method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials according to an embodiment of the present invention;

[0046] Figure 2 It is a schematic diagram of the magnetic levitation force test results of the superconducting bulk material grown by recycling and reusing REBCO bulk seed crystals described in an embodiment of the present invention. DETAILED DESCRIPTION

[0047] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention generally described and shown in the drawings here can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0048] It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings. At the same time, in the description of the present invention, the terms "first", "second", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.

[0049] Embodiment 1:

[0050] This embodiment provides a method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials.

[0051] See also Figure 1 and Figure 2 , the figure shows that the method includes step S1, step S2, step S3, step S4 and step S5.

[0052] Step S1, preparing a first precursor body and a first buffer layer based on a preset REBCO high-temperature superconducting bulk material precursor body manufacturing method and a buffer layer manufacturing method;

[0053] It can be understood that in this step, a precursor embryo and a buffer layer with good crystallinity and density are provided, which provide an ideal base material and substrate for the subsequent superconductor growth. This helps to improve the crystallization quality and performance of the superconductor material, thereby improving the performance and stability of the overall superconducting bulk material. In this step, step S1 includes step S11, step S12, step S13, step S14 and step S15.

[0054] Step S11, weighing the original drugs according to the molar ratio of RE2O3:BaCO3:CuO=1:4:6 and 1:1:1, and mixing them respectively to prepare RE123 original powder and RE211 original powder;

[0055] Step S12, preparing RE123 original powder and RE211 original powder by solid phase sintering method to obtain purified RE123 powder and RE211 powder;

[0056] It can be understood that step S12 also includes step S121 and step S122.

[0057] Step S121, sintering the RE123 raw powder in an air environment at 920° C. for 48 hours, and sintering the RE211 raw powder in an air environment at 930° C. for 48 hours, to obtain sintered RE123 powder blocks and RE211 powder blocks;

[0058] Step S122, grinding and sintering the sintered RE123 powder block and RE211 powder block, repeating the process three times to obtain purified RE123 powder and RE211 powder.

[0059] It can be understood that in this step, the original powder is sintered for a long time under specific temperature and environmental conditions to promote the bonding between powder particles and the growth of crystals, and finally sintered RE123 powder blocks and RE211 powder blocks are obtained. Through sintering and grinding treatment, the purity and crystal structure of the powder are improved, providing high-quality raw materials for the subsequent superconductor preparation process.

[0060] Step S13, weighing and mixing the purified RE123 powder and RE211 powder in a molar ratio of 1:0.35 to obtain a precursor powder, and adding 1wt% of CeO2 powder to the precursor powder for mixing to obtain a precursor powder;

[0061] Step S14, weighing the precursor powder, putting it into a mold for pressing, and obtaining a first precursor embryo;

[0062] Step S15, weighing the purified RE123 powder, RE211 powder and CeO2 powder according to a preset ratio, and putting them into a mold for pressing to obtain a first buffer layer.

[0063] It can be understood that in this step, step S15 includes step S151 and step S152.

[0064] Step S151, mixing the purified RE123 powder and the purified RE211 powder in a molar ratio of 5:2, and mixing the mixed RE123 powder, RE211 powder and 1 wt % CeO2 again to obtain a mixed powder;

[0065] Step S152: placing the mixed powder into a cylindrical mold with a diameter of 6 mm for pressurization to obtain a cylindrical first buffer layer.

[0066] It can be understood that the above steps adopt the solid phase sintering method and powder metallurgy technology, and accurately control the molar ratio and process conditions of the original drugs to prepare the precursor powder with the required composition and structure, and form the first precursor embryo and the first buffer layer through the pressing process. This step accurately controls the molar ratio and process conditions of the original drugs, prepares the precursor powder with the required composition and structure, and forms the first precursor embryo and the first buffer layer through the pressing process, which provides a good basic material and support structure for the subsequent superconductor growth process.

[0067] Step S2, processing the REBCO original seed crystal, the first precursor embryo and the first buffer layer based on the top seed crystal melt texturing method to obtain an original REBCO high temperature superconducting bulk material;

[0068] It can be understood that this step utilizes the guiding effect of the top seed crystal to grow a single crystal superconductor layer on its surface by melt texturing, thereby forming an original REBCO high-temperature superconducting bulk material. This method can effectively control the growth quality and thickness of the superconductor layer and improve the crystallization performance and uniformity of the material. In this step, step S2 includes step S21 and step S22.

[0069] Step S21, inserting the first buffer layer between the REBCO original seed crystal and the first precursor embryo to form a coaxial combination structure from top to bottom;

[0070] It can be understood that in this step, step S21 includes step S211 and step S212.

[0071] Step S211, selecting a 3mm×3mm×3mm REBCO original seed crystal with a smooth cross section, and polishing the ab surface of the bottom of the REBCO original seed crystal to obtain a processed REBCO original seed crystal;

[0072] Step S212, align the central axis of the processed REBCO original seed crystal perpendicular to the ground with the central axis of the first buffer layer and the central axis of the first precursor embryo respectively, and place the REBCO original seed crystal between the first buffer layer and the first precursor embryo to obtain a coaxial combined structure.

[0073] It is understood that the purpose of polishing the original REBCO seed crystal in this step is to eliminate possible surface defects and roughness, so as to ensure that the original REBCO seed crystal can be tightly combined with other components in the subsequent assembly and growth process and provide a good growth surface. Through the polishing process, the surface unevenness can be reduced, and the crystal orientation can be further ensured, and the uniformity and stability in the growth process can be improved. The surface treatment of the original REBCO seed crystal and the formation of the coaxial combination structure lay the foundation for the subsequent texture growth process. The smooth surface after treatment is conducive to the crystal growth and quality improvement in the growth process, and the coaxial combination structure ensures the close combination and stability between the components, which is conducive to the progress and control of the growth process.

[0074] Step S22, placing the combined structure on an alumina ceramic plate, and placing it in a high-temperature furnace in an air atmosphere for texture growth, to obtain an original YBCO high-temperature superconducting bulk material induced by REBCO original seed crystal growth.

[0075] It can be understood that this step realizes the induced growth of the original seed crystal on the REBCO superconducting bulk material through the crystal texture growth technology, thereby obtaining a REBCO high-temperature superconducting bulk material with excellent superconducting properties. This method can control the crystal orientation and superconducting properties of the superconductor during the preparation process, thereby improving the application value of the material. In this step, step S22 includes step S221, step S222 and step S223.

[0076] Step S221, the temperature in the high temperature furnace starts from room temperature, rises to 900°C after 1 hour, and is kept at this temperature for 3 hours, and then continues to be heated for 1 hour, the temperature in the high temperature furnace rises to 1055°C, and is kept at this temperature for 1 hour;

[0077] Step S222, lowering the furnace temperature to 1005° C. within 30 minutes, and then lowering the furnace temperature at a cooling rate of 0.2 K / h to 0.4 K / h, so that the REBCO original seed crystal in the furnace induces the growth of the first precursor embryo for 100 hours;

[0078] Step S223: After the sample growth is completed, the temperature of the high temperature furnace is lowered to room temperature within 3 hours.

[0079] It can be understood that this step promotes the growth of the REBCO original seed crystal by controlling the temperature and time, and finally obtains the desired superconducting bulk material. Through the control of these steps, the precise control and stability of the growth process of the REBCO original seed crystal are achieved. Through appropriate temperature and time control, the formation and growth of the crystal can be promoted, thereby obtaining a superconducting bulk material with good crystal quality and performance. At the same time, by controlling the cooling rate and temperature change, the non-uniformity and deformation of the crystal during the growth process can be avoided, ensuring that the superconducting bulk material finally grown has excellent uniformity and stability.

[0080] Step S3, cleaving the original REBCO high temperature superconducting bulk material along a preset cleavage plane, and grinding and polishing the structure consisting of the first buffer layer and the REBCO seed crystal obtained by cleavage to obtain a recycled seed crystal;

[0081] This step can effectively recycle the seed crystals in the original REBCO block, providing high-quality seed crystals for the subsequent growth process, thereby helping to improve the quality and uniformity of the newly grown superconductor material. The REBCO seed crystal recovery method of the present invention is based on the TSMG method. During the cleavage process, it is necessary to carefully determine the crystal orientation and use a suitable method to accurately cleave the seed crystal-buffer layer structure, and polish the cleavage surface of the structure composed of the first buffer layer and the REBCO seed crystal obtained by cleavage to ensure that the REBCO recycled seed crystal has a natural crystal orientation each time it is reused, and correctly guide the texture of the precursor embryo during the growth process. Step S3 includes step S31 and step S32.

[0082] Step S31, using a cutting device to cleave the original REBCO high temperature superconducting bulk material along the crystal ab plane direction to obtain a REBCO bulk seed crystal with a first buffer layer with a thickness of 0.5 mm, wherein the crystal ab plane direction is a layered cross section of the layered structure on the original REBCO high temperature superconducting bulk material;

[0083] Step S32: grinding and polishing the cleavage surface of the REBCO bulk seed crystal with 1000-grit sandpaper to obtain a REBCO recovery seed crystal.

[0084] It can be understood that in this step, the original REBCO high-temperature superconducting block is cleaved along the ab plane direction of the crystal, that is, the layered cross section of the crystal layering structure, by using a cutting device to obtain a REBCO bulk seed crystal with a first buffer layer of 0.5 mm thickness. The purpose of this step is to separate a bulk seed crystal with a certain buffer layer thickness from the original bulk material for subsequent recycling and reuse. It can be understood that in this step, a bulk seed crystal with a certain buffer layer thickness is obtained by effectively separating and treating the original REBCO high-temperature superconducting block material, and its cleavage surface is smoothed and uniformly treated. Such treatment can ensure that the recovered seed crystal has good surface quality and morphology, and can effectively participate in the subsequent growth process, thereby realizing the effective reuse of the REBCO bulk seed crystal.

[0085] Step S4, repeating the process to obtain a second precursor embryo and a second buffer layer, placing the recycled seed crystal at the top center of the second precursor embryo, and coaxially inserting the second buffer layer between the recycled seed crystal and the second precursor embryo to obtain an assembled second precursor embryo;

[0086] It can be understood that this step provides an ideal base material and substrate for the next step of superconductor growth. At the same time, by using the recycled seed crystals, the production cost is also reduced and the resource utilization efficiency is improved.

[0087] Step S5: Based on the top seed crystal melt texturing method, the assembled second precursor embryo body is subjected to the same heat treatment as the first precursor embryo body to obtain a REBCO high temperature superconducting bulk material grown by using recycled seed crystals.

[0088] It can be understood that the RE in the REBCO bulk seed crystal in this step is selected from Y, Gd, Sm, and Nd, and step S5 also includes step S6 and step S7.

[0089] Step S6, sending the two grown blocks into a high temperature furnace with a flowing oxygen atmosphere for annealing, wherein the annealing temperature is 450° C. and the annealing time is 200 h, to obtain two REBCO high temperature superconducting blocks that have completed the annealing process;

[0090] Step S7: Perform a magnetic levitation force test on the two REBCO high temperature superconducting bulk materials that have completed the annealing process, and obtain the magnetic levitation force test results of the two REBCO high temperature superconducting bulk materials that have completed the annealing process.

[0091] It can be understood that this step is to place the block in a high temperature furnace, anneal it in a flowing oxygen atmosphere at a temperature of 450°C for 200 hours. The purpose of the annealing treatment is to achieve the transformation of the crystal structure of the block so that it can obtain superconductivity. The annealing treatment can achieve the transformation of the crystal structure of the block so that it can obtain superconductivity and improve its superconducting performance and stability. The magnetic levitation force test can accurately evaluate the superconducting performance of the block, ensure that it meets the design requirements, and judge the changes in its magnetic levitation force, such as Figure 2 As shown, the magnetic levitation performance of the original REBCO high-temperature superconducting bulk material and the REBCO high-temperature superconducting bulk material grown using recycled seed crystals are highly consistent. It can be further known that the present invention can repeatedly prepare REBCO high-temperature superconducting bulk materials from two aspects of growth morphology and magnetic levitation force performance.

[0092] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

[0093] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for recycling and reusing REBCO bulk seed crystals for growing superconducting bulk materials, characterized in that: include: Prepare a first precursor body and a first buffer layer based on a preset REBCO high-temperature superconducting bulk material precursor body preparation method and a buffer layer preparation method; The original REBCO seed crystal, the first precursor embryo and the first buffer layer are processed based on the top seed crystal melt texturing method to obtain the original REBCO high temperature superconducting bulk material; Cleavage the original REBCO high temperature superconducting bulk material along a preset cleavage plane, and grind and polish the structure consisting of the first buffer layer and the REBCO seed crystal obtained by cleavage to obtain a recycled seed crystal; Repeat the process to obtain a second precursor embryo and a second buffer layer, place the recycled seed crystal in the top center of the second precursor embryo, and coaxially insert the second buffer layer between the recycled seed crystal and the second precursor embryo to obtain an assembled second precursor embryo; Based on the top seed crystal melt texturing method, the assembled second precursor embryo body is subjected to the same heat treatment as the first precursor embryo body to obtain a REBCO high temperature superconducting bulk material grown by using recycled seed crystals; The method comprises: processing the preset REBCO original seed crystal, the first precursor embryo and the first buffer layer based on the top seed crystal melt texturing method to obtain the original REBCO high temperature superconducting bulk material, including: Inserting the first buffer layer between the REBCO original seed crystal and the first precursor embryo to form a coaxial combined structure from top to bottom; Placing the combined structure on an alumina ceramic plate, and placing it in a high-temperature furnace in an air atmosphere for texture growth, to obtain an original YBCO high-temperature superconducting bulk material induced by REBCO original seed crystal growth; The first buffer layer is inserted between the REBCO original seed crystal and the first precursor embryo to form a coaxial combination structure from top to bottom, including: A REBCO original seed crystal of 3 mm×3 mm×3 mm with a smooth cross section is selected, and the ab surface of the bottom of the REBCO original seed crystal is polished to obtain a processed REBCO original seed crystal; Aligning the central axis of the processed REBCO original seed crystal perpendicular to the ground with the central axis of the first buffer layer and the central axis of the first precursor embryo body, respectively, and placing the REBCO original seed crystal between the first buffer layer and the first precursor embryo body to obtain a coaxial combined structure; Wherein, the cleaving of the original REBCO high temperature superconducting bulk material along a preset cleavage plane comprises: Using a cutting device to cleave the original REBCO high-temperature superconducting bulk material along the crystal ab plane direction to obtain a REBCO bulk seed crystal with a first buffer layer with a thickness of 0.5 mm, wherein the crystal ab plane direction is a layered cross section of the layered structure on the original REBCO high-temperature superconducting bulk material; The cleavage surface of the REBCO bulk seed crystal was ground and polished with 1000-grit sandpaper to obtain a REBCO recovery seed crystal.

2. The method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials according to claim 1, characterized in that The method of preparing the first precursor embryo and the first buffer layer based on the preset precursor embryo preparation method and the buffer layer preparation method includes: The original drugs were weighed according to the molar ratio of RE2O3:BaCO3:CuO=1:4:6 and 1:1:1, and were mixed to prepare RE123 original powder and RE211 original powder respectively; The RE123 original powder and the RE211 original powder were prepared by solid phase sintering method to obtain purified RE123 powder and RE211 powder; The purified RE123 powder and RE211 powder were weighed and mixed in a molar ratio of 1:0.35 to obtain a precursor powder, and 1 wt % of CeO2 powder was added to the precursor powder for mixing to obtain a precursor powder; Weighing the precursor powder, putting it into a mold for pressing, and obtaining a first precursor embryo; The purified RE123 powder, RE211 powder and CeO2 powder are weighed according to a preset ratio, put into a mold for pressing, and obtain a first buffer layer.

3. The method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials according to claim 2, characterized in that , the RE123 original powder and the RE211 original powder are prepared by solid phase sintering method, including: The RE123 raw powder was sintered in an air environment at 920° C. for 48 hours, and the RE211 raw powder was sintered in an air environment at 930° C. for 48 hours to obtain sintered RE123 powder blocks and RE211 powder blocks; The sintered RE123 powder block and RE211 powder block are ground and sintered three times to obtain purified RE123 powder and RE211 powder.

4. The method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials according to claim 2, characterized in that The purified RE123 powder, RE211 powder and CeO2 powder are weighed according to a preset ratio, and put into a mold for pressing to obtain a first buffer layer, including: The purified RE123 powder and the purified RE211 powder are mixed in a molar ratio of 5:2, and the mixed RE123 powder, RE211 powder and 1 wt % CeO2 powder are mixed again to obtain a mixed powder; The mixed powder is placed in a cylindrical mold with a diameter of 6 mm and subjected to pressure pressing to obtain a cylindrical first buffer layer.

5. The method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials according to claim 1, characterized in that: The step of placing the combined structure on an alumina ceramic plate and placing the combined structure in a high temperature furnace in an air atmosphere for texture growth comprises: The temperature in the high-temperature furnace starts from room temperature and rises to 900°C after 1 hour and is kept at this temperature for 3 hours. Then, the heating is continued for 1 hour, and the temperature in the high-temperature furnace is raised to 1055°C and is kept at this temperature for 1 hour. The furnace temperature was lowered to 1005° C. within 30 minutes, and then the furnace temperature was lowered at a cooling rate of 0.2 K / h to 0.4 K / h, so that the REBCO original seed crystal in the furnace induced the growth of the first precursor embryo for 100 hours; After the sample growth was completed, the temperature of the high-temperature furnace was lowered to room temperature within 3 h.

6. The method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials according to claim 1, characterized in that: The RE in the REBCO bulk seed crystal is selected from Y, Gd, Sm, and Nd.

7. The method for recycling and reusing REBCO bulk seed crystals to grow superconducting bulk materials according to claim 1, characterized in that: After obtaining the REBCO high temperature superconducting bulk material grown by using the recycled seed crystal, the method further includes: Recovering the seed crystals on the REBCO high-temperature superconducting bulk material grown using the recycled seed crystals, and performing grinding and polishing treatments on the REBCO high-temperature superconducting bulk material grown using the recycled seed crystals and the original REBCO high-temperature superconducting bulk material to obtain two completed growth bulk materials; The two grown blocks were sent to a high temperature furnace with a flowing oxygen atmosphere for annealing, wherein the annealing temperature was 450° C. and the annealing time was 200 h, to obtain two REBCO high temperature superconducting blocks that had completed the annealing process; The magnetic levitation force test was performed on two REBCO high temperature superconducting bulk materials that had completed the annealing process, and the magnetic levitation force test results of the two REBCO high temperature superconducting bulk materials that had completed the annealing process were obtained.