Perovskite ink and preparation method thereof, perovskite film and preparation method thereof, perovskite solar cell
By repeating the mixing steps at different temperatures to adjust the dissolution and colloid formation of the perovskite precursor composition, the stability of perovskite ink is solved, the efficiency of perovskite films and solar cells is improved, and the efficient perovskite films and solar cells are achieved. Preparation of mineral ink.
Patent Information
- Application Number
- CN202410763873.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-06-14
AI Technical Summary
There are stability problems in the aging process of traditional perovskite ink formulations, which affects the efficiency and film quality of perovskite solar cells.
By repeating the mixing steps at different temperatures, the component dissolution of the perovskite precursor composition and the formation of colloid particles are adjusted, and the stability of the dispersed colloids in the solution is improved, thereby ensuring the uniformity of the perovskite ink and the stability of the film.
It achieves high stability and uniformity of perovskite ink, improves the photoelectric conversion efficiency of perovskite films and solar cells, and is suitable for mass production control and performance improvement.
Smart Images

Figure CN118338752B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photovoltaic technology, and in particular to a perovskite ink and a preparation method thereof, a perovskite film and a preparation method thereof, and a perovskite solar cell. Background Art
[0002] The development of semiconductor technology plays a vital role in the progress of the electronics industry. As a new type of semiconductor, perovskite has many advantages such as long carrier diffusion length, high defect tolerance, adjustable band gap, and large absorption coefficient. Compared with traditional organic and inorganic semiconductors, perovskite has a simple preparation process and low cost, which has great advantages in the semiconductor field. Up to now, the efficiency of perovskite solar cells has exceeded 26%, and T95 has exceeded thousands of hours. In addition, it has been studied and applied in light-emitting diodes, detectors, lasers, etc. As an emerging semiconductor material, perovskite shows great potential.
[0003] Perovskite solar cells have attracted much attention as the third generation of photovoltaic technology due to their potential high efficiency and low cost advantages. Among them, the solution method for preparing perovskite thin films has significant advantages of high production efficiency and low cost in large-area processes, and the efficiency of perovskite solar cells depends largely on the crystallization quality of the perovskite photoactive layer. There are still some problems in the aging process of traditional perovskite ink formulations that need to be solved urgently. Summary of the invention
[0004] Based on this, it is necessary to provide a perovskite ink and a preparation method thereof, a perovskite film and a preparation method thereof, and a perovskite solar cell to address the problem of how to improve the stability of dispersed colloids in solutions, wherein the perovskite ink of the present invention is a perovskite photovoltaic cell material.
[0005] A method for preparing perovskite ink comprises the following steps:
[0006] Step 1: fully mixing the perovskite precursor composition at a first temperature to obtain a first mixed solution;
[0007] Step 2: fully mixing the first mixed solution at a second temperature to obtain a second mixed solution, wherein the second temperature is lower than the first temperature; and
[0008] Step 3: Repeat steps 1 and 2, with the number of repetitions being ≥ 1, to obtain perovskite ink.
[0009] The preparation method of perovskite ink using the technical solution of the present invention is conducive to the dissolution of components in the perovskite precursor composition at the first temperature, accelerates the diffusion of components, and can cause the dispersed colloid in the solution to begin to dissolve. Large-particle colloids absorb heat energy and dissolve and become smaller due to interfacial energy reasons; while at the second temperature, it is conducive to the formation of dispersed colloids. By repeating steps one and two, the size and morphology of the colloid particles can be adjusted to be more uniform, thereby improving the stability of the dispersed colloid in the solution, which is conducive to the subsequent formation of a uniform and stable perovskite crystal phase. The above-mentioned preparation method can be used to quickly and efficiently prepare high-quality perovskite inks, which is conducive to mass production control and improving product performance.
[0010] In a feasible implementation, the difference between the first temperature and the second temperature is 10° C. to 90° C.; or
[0011] The difference between the first temperature and the second temperature is 20°C to 60°C; or
[0012] The difference between the first temperature and the second temperature is 40°C to 60°C.
[0013] In a feasible implementation, the first temperature is 60°C to 90°C, and the second temperature is 0°C to 30°C.
[0014] In a feasible implementation, the perovskite precursor composition includes a perovskite precursor, an organic solvent and an auxiliary agent;
[0015] The perovskite precursor is a precursor of perovskite, and the perovskite is an ABX3 structure, wherein A represents an organic cation selected from MA + , FA + With Cs + At least one of; B represents a metal cation Pb 2+ ; X represents a halogen anion selected from I - Br - With Cl - At least one of;
[0016] The organic solvent is selected from at least one of dimethylformamide, N-methylpyrrolidone and dimethyl sulfoxide;
[0017] The auxiliary agent is selected from at least one of γ-butyrolactone, methylamine chloride and 1-butyl-3-methylimidazolium tetrafluoroborate.
[0018] In a feasible implementation, the time for sufficient mixing in step one is greater than the time for sufficient mixing when step one is repeated in step three, and the time for sufficient mixing in step two is equal to, greater than or less than the time for sufficient mixing when step two is repeated in step three.
[0019] In a feasible implementation, in step one, the time for sufficient mixing is 30 min to 120 min; in step two, the time for sufficient mixing is 10 min to 30 min; in step three, the time for sufficient mixing when repeating step one is 30 min to 60 min, and the time for sufficient mixing when repeating step two is 10 min to 30 min.
[0020] In a feasible implementation, in step three, the number of times of repeating step one and step two is 1 to 100.
[0021] In a feasible implementation, the first temperature in step one is equal to the first temperature in step one repeated in step three, and the second temperature in step two is equal to the second temperature in step two repeated in step three; or
[0022] The first temperature in step one is equal to the first temperature in step one repeated in step three, and the second temperature in step two is not equal to the second temperature in step two repeated in step three; or
[0023] The first temperature in step one is not equal to the first temperature in step one repeated in step three, and the second temperature in step two is not equal to the second temperature in step two repeated in step three; or
[0024] The first temperature in step one is not equal to the first temperature in step one repeated in step three, and the second temperature in step two is equal to the second temperature in step two repeated in step three.
[0025] In a feasible implementation, the interval from obtaining the first mixed solution to fully mixing the first mixed solution at the second temperature is less than 120 seconds.
[0026] In a feasible implementation, a first temperature control device is used to control the first temperature, and a second temperature control device is used to control the second temperature; or
[0027] The first temperature and the second temperature are adjusted by a temperature control device, and the temperature adjustment speed is 1°C / min~25°C / min.
[0028] A perovskite ink is prepared by any of the above-mentioned methods for preparing the perovskite ink.
[0029] The size and shape of the colloidal particles in the perovskite ink of the technical solution of the present invention are more uniform and consistent, and the stability of the dispersed colloid is better, which is conducive to the subsequent formation of a uniform and stable perovskite crystal phase.
[0030] A method for preparing a perovskite film comprises the following steps:
[0031] providing a substrate; and
[0032] The perovskite ink is coated on the surface of the substrate, and the perovskite film is obtained after removing the solvent.
[0033] The method for preparing a perovskite film using the technical solution of the present invention is beneficial for obtaining a stable perovskite film and forming a uniform and stable perovskite crystal phase because the size and morphology of the colloid particles in the above-mentioned perovskite ink are more uniform and consistent, and the stability of the dispersed colloid is better.
[0034] A perovskite film is prepared by using the above-mentioned method for preparing perovskite ink.
[0035] The size and shape of the colloidal particles in the perovskite film of the technical solution of the present invention are more uniform and consistent, and the stability of the dispersed colloid is better, which is conducive to the subsequent formation of a uniform and stable perovskite crystal phase.
[0036] A perovskite solar cell comprises the perovskite film mentioned above.
[0037] The perovskite solar cell of the technical solution of the present invention includes the above-mentioned perovskite film. Since the size and morphology of the colloidal particles in the perovskite film are more uniform and consistent, and the stability of the dispersed colloid is better, the perovskite solar cell of the technical solution of the present invention has a uniform and stable perovskite crystal phase. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Flow chart of a method for preparing perovskite ink according to one embodiment of the present invention.
[0039] Figure 2 FIG. 4 is a temperature curve of a method for preparing perovskite ink according to an embodiment of the present invention.
[0040] Figure 3 This is a schematic diagram of the particle size change in the preparation method of perovskite ink according to one embodiment of the present invention.
[0041] Figure 4 The present invention is a flowchart of a method for preparing a perovskite film according to an embodiment of the present invention.
[0042] Figure 5 This is a scanning electron microscope (SEM) image of the perovskite film prepared in Example 1.
[0043] Figure 6 This is a scanning electron microscope (SEM) image of the perovskite film prepared in Comparative Example 1.
[0044] Figure 7 This is a scanning electron microscope (SEM) image of the perovskite film prepared in Example 4.
[0045] Figure 8This is a scanning electron microscope (SEM) image of the perovskite film prepared in Example 2.
[0046] Fig. 9 This is a scanning electron microscope (SEM) image of the perovskite film prepared in Comparative Example 2.
[0047] Fig.10 This is a scanning electron microscope (SEM) image of the perovskite film prepared in Example 3.
[0048] Fig.11 This is a scanning electron microscope (SEM) image of the perovskite film prepared in Comparative Example 3. DETAILED DESCRIPTION
[0049] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0051] See also Figure 1 and Figure 2 ( Figure 2 The time on the horizontal axis is only the duration of the first temperature T1 and the second temperature T2, and does not include the interval time of switching between the first temperature T1 and the second temperature T2). The method for preparing the perovskite ink according to one embodiment of the present invention comprises the following steps:
[0052] S10: Step 1, fully mixing the perovskite precursor composition at a first temperature T1 to obtain a first mixed solution.
[0053] In a feasible implementation, the perovskite precursor composition includes a perovskite precursor, an organic solvent and an additive. The perovskite precursor is a precursor of perovskite, and the perovskite is an ABX3 structure, wherein A represents an organic cation selected from MA + , FA + With Cs + At least one of; B represents a metal cation Pb 2+ ; X represents a halogen anion selected from I- Br - With Cl - At least one of the following. The perovskite includes but is not limited to organic-inorganic hybrid perovskite or inorganic perovskite, wherein the organic-inorganic hybrid perovskite includes but is not limited to MAPbI3, FAPbI3, CsPb(I x Br (1-x) )3. Cs n FA (1-n) Pb(I x Br (1-x) )3. Cs n FA (1-n) PbI3、Cs n FA (1-n-m) MA m Pb(I x Br (1-x) )3 or tin-based perovskite, etc., where n=0~1, x=0~1.
[0054] Furthermore, the organic solvent is selected from at least one of dimethylformamide (DMF), N-methylpyrrolidone (NMP) and dimethyl sulfoxide (DMSO). The auxiliary agent is selected from at least one of γ-butyrolactone, methylamine chloride and 1-butyl-3-methylimidazolium tetrafluoroborate (BMIMBF4, an ionic liquid). It should be noted that the types of organic solvents and auxiliary agents are not limited thereto.
[0055] In step 1, the perovskite precursor composition can be fully mixed at the first temperature T1 by stirring.
[0056] After step 1, at the first temperature T1, it is beneficial for the components in the perovskite precursor composition to dissolve, accelerate the diffusion of the components, and at the same time, the dispersed colloids in the solution begin to dissolve. The large-particle colloids absorb heat energy and dissolve and become smaller due to interfacial energy.
[0057] S20: Step 2, fully mixing the first mixed solution at a second temperature T2 to obtain a second mixed solution, wherein the second temperature T2 is lower than the first temperature T1.
[0058] In step 2, the first mixed solution can be fully mixed at the second temperature T2 by stirring.
[0059] In step 2, the first mixed solution is fully mixed at a relatively low second temperature T2, which can reduce molecular thermal motion, strengthen the bonding strength between the organic component and the inorganic component in the perovskite precursor solution, and form a dispersed and stable colloid.
[0060] In a feasible implementation, the difference between the first temperature T1 and the second temperature T2 is 10°C to 90°C. Further, the difference between the first temperature T1 and the second temperature T2 may be, but is not limited to, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C or 90°C. Preferably, the difference between the first temperature T1 and the second temperature T2 is 20°C to 60°C. More preferably, the difference between the first temperature T1 and the second temperature T2 is 40°C to 60°C.
[0061] In a feasible implementation, the first temperature T1 is 60°C to 90°C, and the second temperature T2 is 0°C to 30°C. Further, the first temperature T1 may be, but is not limited to, 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C, 99°C, 100°C, 101°C, 102°C, 103°C, 104°C The second temperature T2 may be, but is not limited to, 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C or 30°C.
[0062] In a feasible implementation, the first temperature T1 is 65° C. to 75° C., and the second temperature T2 is 15° C. to 25° C. Further, the first temperature T1 may be, but is not limited to, 65° C., 66° C., 67° C., 68° C., 69° C., 70° C., 71° C., 72° C., 73° C., 74° C., or 75° C., and the second temperature T2 may be, but is not limited to, 15° C., 16° C., 17° C., 18° C., 19° C., 20° C., 21° C., 22° C., 23° C., 24° C., or 25° C.
[0063] S30: Step 3, repeat step 1 and step 2, the number of repetitions is ≥ 1, to obtain perovskite ink.
[0064] Figure 3 Schematic diagram of the change of particle size in solution, combined with Figure 3 The principle of the change in the size of the colloid particles in the solution is as follows: in step 1, after the perovskite precursor composition is mixed at the first temperature T1, all the colloid particles in the solution will dissolve, so that the size of the large-sized colloid particles and the small-sized colloid particles will become smaller, and some small-sized colloid particles will be completely dissolved and compounded into the large-sized colloid particles; then in step 2, after mixing at the second temperature T2, all the colloid particles will nucleate and grow, such as Figure 3As shown in (a), at this time, the sizes of the colloid particles are different and the dispersion is large; after repeating the first temperature T1 in step 3, all the colloid particles in the solution will dissolve, making the size of all the colloid particles smaller, but the concentration of the particle size is much more concentrated than when mixing at the first temperature T1 in step 1. After repeating the second temperature T2, all the colloid particles nucleate and grow, as shown in Figure 3 As shown in (b), the dispersion of the colloidal particle size is relatively small at this time; continue to repeat steps 1 and 2, and the colloidal particle size in the obtained perovskite ink is as follows: Figure 3 As shown in (c), the dispersion of the particle size is more uniform. Figure 3 The size and shape of the particles are for illustration only and do not limit the actual size and shape of the particles.
[0065] In step S30, the high and low temperature processes are repeated. The high temperature process can accelerate the dissolution of the participating components, promote the migration of unpaired organic and inorganic components, increase the pairing probability, and pair into organic-inorganic components after migration; at the same time, since the high temperature is not continuous, the probability of destroying the already formed colloidal state can be reduced. By repeating steps one and two, the size and shape of the colloidal particles can be adjusted to be more uniform, thereby improving the stability of the dispersed colloid in the solution, which is conducive to the subsequent formation of a uniform and stable perovskite crystal phase.
[0066] In a feasible implementation, the time for sufficient mixing in step one (t1) is greater than the time for sufficient mixing when step one is repeated in step three (t3-t2). This is because what is dissolved at the first temperature in step one is mainly the precursor solute, and what is dissolved at the first temperature in step three is mainly the colloid, and the time required to dissolve the colloid is less than the dissolution time of the solute. Therefore, the time for sufficient mixing in step one is greater than the time for sufficient mixing when step one is repeated in step three, which is conducive to the sufficient dissolution of the precursor solute in step one. Of course, the present invention does not exclude the situation where the time for sufficient mixing in step one (t1) is less than or equal to the time for sufficient mixing when step one is repeated in step three (t3-t2).
[0067] In a feasible implementation, in step one, the time for sufficient mixing (t1) is 30 min to 120 min; in step two, the time for sufficient mixing (t2-t1) is 10 min to 30 min; in step three, the time for sufficient mixing when repeating step one (t3-t2) is 30 min to 60 min, and the time for sufficient mixing when repeating step two (t4-t3) is 10 min to 30 min. Specifically, in step 1, the operation of fully mixing is: under the first temperature T1, the stirring time (t1) is maintained for 30min~120min; in step 2, the operation of fully mixing is: under the second temperature T2, the stirring time (t2-t1) is maintained for 10min~30min; in step 3, the operation of fully mixing when repeating step 1 is: under the first temperature T1, the stirring time (t3-t2) is maintained for 30min~60min, and the operation of fully mixing when repeating step 2 is: under the second temperature T2, the stirring time (t4-t3) is maintained for 10min~30min. It should be noted that the operation and time of fully mixing in steps 1, 2 and 3 are not limited to this.
[0068] In a feasible implementation, in step 3, the number of times steps 1 and 2 are repeated (i.e. Figure 2 The number of cycles N in the step is 1 to 100. Further, the number of times step 1 and step 2 are repeated may be, but is not limited to, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95 or 100.
[0069] In a feasible implementation, the first temperature T1 in step one is equal to the first temperature T1 in step one repeated in step three, and the second temperature T2 in step two is equal to the second temperature T2 in step two repeated in step three.
[0070] In a feasible implementation, the first temperature T1 in step one is equal to the first temperature T1 in step one repeated in step three, and the second temperature T2 in step two is not equal to the second temperature T2 in step two repeated in step three.
[0071] In a feasible implementation, the first temperature T1 in step one is not equal to the first temperature T1 in step one repeated in step three, and the second temperature T2 in step two is not equal to the second temperature T2 in step two repeated in step three.
[0072] In a feasible implementation, the first temperature T1 in step one is not equal to the first temperature T1 in step one repeated in step three, and the second temperature T2 in step two is equal to the second temperature T2 in step two repeated in step three.
[0073] It should be noted that in the preparation method of the perovskite ink of the present invention, the first temperature T1 and the second temperature in each repetition of step three can meet the conditions in the above-mentioned implementation method, that is, the first temperature T1 in step one and the first temperature T1 in step one repeated in step three can be equal to or unequal; similarly, the second temperature T2 in step two and the second temperature T2 in step two repeated in step three can be equal to or unequal.
[0074] In a feasible implementation, the interval time from obtaining the first mixed solution to fully mixing the first mixed solution at the second temperature T2 is less than 120s. Further, the above-mentioned interval time may be, but is not limited to, 0s, 10s, 20s, 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, 110s or 120s. In this embodiment, rapid cooling can be achieved within the above-mentioned interval time, which is conducive to more uniform precipitated colloidal particles.
[0075] In a feasible implementation, a first temperature control device is used to control the first temperature T1, and a second temperature control device is used to control the second temperature T2. That is, two different temperature control devices can be used to adjust the first temperature and the second temperature.
[0076] In another feasible implementation, the same temperature control device is used to adjust the first temperature T1 and the second temperature T2, and the temperature adjustment speed is 1°C / min~25°C / min. It should be noted that when the temperature is controlled by the temperature control device, the first temperature T1 and the second temperature T2 are the device temperatures. The required adjustment speed of the temperature control device is preferably 1~25°C / min, which can be but not limited to 1°C / min, 5°C / min, 10°C / min, 15°C / min, 20°C / min or 25°C / min.
[0077] The preparation method of perovskite ink using the technical solution of the present invention is conducive to the dissolution of components in the perovskite precursor composition at a first temperature, accelerates the diffusion of components, and can cause the dispersed colloid in the solution to begin to dissolve. Large-particle colloids absorb heat energy and dissolve and become smaller due to interfacial energy reasons; while at a second temperature, it is conducive to the formation of dispersed colloids. By repeating steps one and two, the size and morphology of the colloid particles can be adjusted to be more uniform, thereby improving the stability of the dispersed colloid in the solution, which is conducive to the subsequent formation of a uniform and stable perovskite crystal phase. The above-mentioned preparation method can be used to quickly and efficiently prepare high-quality perovskite ink, which is conducive to mass production control and improving product performance. The perovskite ink of one embodiment is prepared using any of the above-mentioned methods for preparing perovskite inks.
[0078] The size and shape of the colloidal particles in the perovskite ink of the technical solution of the present invention are more uniform and consistent, and the stability of the dispersed colloid is better, which is conducive to the subsequent formation of a uniform and stable perovskite crystal phase.
[0079] See also Figure 4 A method for preparing a perovskite film according to an embodiment of the present invention comprises the following steps:
[0080] S40: providing a substrate.
[0081] The substrate is used to coat the perovskite ink to form a perovskite film. The present invention does not limit the structure of the perovskite solar cell, so the substrate can be any substrate used to coat the perovskite ink.
[0082] S50: coating the perovskite ink on the surface of the substrate, and obtaining a perovskite film after removing the solvent.
[0083] The solvent may be removed by commonly used means in the art, such as heat treatment.
[0084] The method for preparing a perovskite film using the technical solution of the present invention is beneficial for obtaining a stable perovskite film and forming a uniform and stable perovskite crystal phase because the size and morphology of the colloid particles in the above-mentioned perovskite ink are more uniform and consistent, and the stability of the dispersed colloid is better.
[0085] The perovskite film of one embodiment is prepared by using the above-mentioned method for preparing the perovskite ink.
[0086] The size and shape of the colloidal particles in the perovskite film of the technical solution of the present invention are more uniform and consistent, and the stability of the dispersed colloid is better, which is conducive to the subsequent formation of a uniform and stable perovskite crystal phase.
[0087] A perovskite solar cell according to one embodiment includes the perovskite thin film described above.
[0088] The perovskite solar cell of the technical solution of the present invention includes the above-mentioned perovskite film. Since the size and morphology of the colloidal particles in the perovskite film are more uniform and consistent, and the stability of the dispersed colloid is better, the perovskite solar cell of the technical solution of the present invention has a uniform and stable perovskite crystal phase.
[0089] With reference to the above implementation contents, in order to make the technical solution of the present invention more specific, clear and easy to understand, the technical solution of the present invention is now exemplified. However, it should be noted that the contents to be protected by the present invention are not limited to the following embodiments 1 to 4.
[0090] Example 1
[0091] This embodiment provides a perovskite ink and a preparation method thereof, a perovskite film and a preparation method thereof; wherein the perovskite CsPb(I x Br (1-x) )3 precursor as raw material, DMF (N,N-dimethylformamide): NMP (N-methylpyrrolidone) = 6:1 as solvent, prepare 1.4 mol / L perovskite ink; the specific steps are as follows:
[0092] S0: Weigh various raw materials and mix them evenly to obtain a perovskite precursor composition;
[0093] S10: placing the perovskite precursor composition on a hot plate for heating, controlling the temperature to 75° C. and stirring for 60 minutes to obtain a first mixed solution;
[0094] S20: transferring the first mixed solution to room temperature (the room temperature in this embodiment is 25° C.) and stirring for 20 minutes to obtain a second mixed solution;
[0095] S30: repeat steps S10 and S20 four times to obtain the perovskite ink of Example 1;
[0096] S40: providing a substrate;
[0097] S50: spin-coating the perovskite ink obtained in step S30 onto a substrate to form a film, and crystallizing it by VCD (vacuum drying) to obtain the perovskite film of Example 1.
[0098] Example 2
[0099] This embodiment provides a perovskite ink and a preparation method thereof, a perovskite film and a preparation method thereof; wherein the perovskite Cs n FA (1-n) Pb(I x Br (1-x) )3 precursor as raw material, DMF:NMP=6:1 as solvent, prepare 1.4mol / L perovskite ink; the specific steps are as follows:
[0100] S0: Weigh various raw materials and mix them evenly to obtain a perovskite precursor composition;
[0101] S10: heating the perovskite precursor composition on a hot plate, controlling the temperature to 70° C. and stirring for 45 minutes to obtain a first mixed solution;
[0102] S20: transferring the first mixed solution to room temperature (the room temperature in this embodiment is 20° C.) and stirring for 20 minutes to obtain a second mixed solution;
[0103] S30: repeating steps S10 and S20 four times to obtain the perovskite ink of Example 2;
[0104] S40: providing a substrate;
[0105] S50: spin-coating the perovskite ink obtained in step S30 onto a substrate to form a film, and crystallizing it by VCD (vacuum drying) to obtain the perovskite film of Example 2.
[0106] Example 3
[0107] This embodiment provides a perovskite ink and a preparation method thereof, a perovskite film and a preparation method thereof; wherein the perovskite FA (1-m) MA m Pb(I x Br (1-x) )3 precursor as raw material, DMF:NMP=6:1 as solvent, prepare 1.4mol / L perovskite ink; the specific steps are as follows:
[0108] S0: Weigh various raw materials and mix them evenly to obtain a perovskite precursor composition;
[0109] S10: heating the perovskite precursor composition on a hot plate, controlling the temperature to 60° C. and stirring for 30 minutes to obtain a first mixed solution;
[0110] S20: transferring the first mixed solution to room temperature (the room temperature in this embodiment is 25° C.) and stirring for 20 minutes to obtain a second mixed solution;
[0111] S30: repeating steps S10 and S20 four times to obtain the perovskite ink of Example 3;
[0112] S40: providing a substrate;
[0113] S50: spin-coating the perovskite ink obtained in step S30 onto a substrate to form a film, and crystallizing it by VCD (vacuum drying) to obtain the perovskite film of Example 2.
[0114] Example 4
[0115] This embodiment provides a perovskite ink and a preparation method thereof, a perovskite film and a preparation method thereof; wherein the perovskite CsPb(IxBr (1-x) )3 precursor as raw material, DMF:NMP=6:1 as solvent, prepare 1.4mol / L perovskite ink; the specific steps are as follows:
[0116] S0: Weigh various raw materials and mix them evenly to obtain a perovskite precursor composition;
[0117] S10: heating the perovskite precursor composition on a hot plate, controlling the temperature to 60° C. and stirring for 60 minutes to obtain a first mixed solution;
[0118] S20: transferring the first mixed solution to 35° C. and stirring for 20 min to obtain a second mixed solution;
[0119] S30: repeating steps S10 and S20 four times to obtain the perovskite ink of Example 4;
[0120] S40: providing a substrate;
[0121] S50: spin-coating the perovskite ink obtained in step S30 onto a substrate to form a film, and crystallizing it by VCD (vacuum drying) to obtain the perovskite film of Example 4.
[0122] Comparative Example 1
[0123] This comparative example is a comparative example of Example 1, and provides a perovskite ink and a preparation method thereof, a perovskite film and a preparation method thereof; wherein the perovskite CsPb(IxBr (1-x) )3 precursor as raw material, DMF:NMP=6:1 as solvent, prepare 1.4mol / L perovskite ink; the specific steps are as follows:
[0124] S0: Weigh various raw materials and mix them evenly to obtain a perovskite precursor composition;
[0125] S10: heating the perovskite precursor composition on a hot plate, controlling the temperature to 75° C. and stirring for 10 h, until the solute is visually completely dissolved, to obtain a mixed solution;
[0126] S20: the mixed solution is further stirred and aged at room temperature (the room temperature of this comparative example is 25° C.) for 24 hours to obtain the perovskite ink of comparative example 1;
[0127] S30: providing a substrate;
[0128] S40: spin-coating the perovskite ink obtained in step S20 onto a substrate to form a film, and crystallizing it by VCD (vacuum drying) to obtain the perovskite film of comparative example 1.
[0129] Comparative Example 2
[0130] This comparative example is a comparative example of Example 2, and provides a perovskite ink and a preparation method thereof, a perovskite film and a preparation method thereof: wherein the perovskite Cs n FA (1-n) Pb(I x Br (1-x) )3 precursor as raw material, DMF:NMP=6:1 as solvent, prepare 1.4mol / L perovskite ink; the specific steps are as follows:
[0131] S0: Weigh various raw materials and mix them evenly to obtain a perovskite precursor composition;
[0132] S10: heating the perovskite precursor composition on a hot plate, controlling the temperature to 70° C. and stirring for 10 h, until the solute is visually completely dissolved, to obtain a mixed solution;
[0133] S20: the mixed solution is further stirred and aged at room temperature (the room temperature in this comparative example is 20° C.) for 24 hours to obtain the perovskite ink of comparative example 2;
[0134] S30: providing a substrate;
[0135] S40: spin-coating the perovskite ink obtained in step S20 onto a substrate to form a film, and crystallizing it by VCD (vacuum drying) to obtain the perovskite film of comparative example 2.
[0136] Comparative Example 3
[0137] This comparative example is a comparative example of Example 3, and provides a perovskite ink and a preparation method thereof, a perovskite film and a preparation method thereof: wherein the perovskite FA (1-m) MA m Pb(I x Br (1-x) )3 precursor as raw material, DMF:NMP=6:1 as solvent, prepare 1.4mol / L perovskite ink; the specific steps are as follows:
[0138] S0: Weigh various raw materials and mix them evenly to obtain a perovskite precursor composition;
[0139] S10: heating the perovskite precursor composition on a hot plate, controlling the temperature to 60° C. and stirring for 10 h, until the solute is visually completely dissolved, to obtain a mixed solution;
[0140] S20: the mixed solution is further stirred and aged at room temperature (the room temperature in this comparative example is 25° C.) for 24 hours to obtain the perovskite ink of comparative example 3;
[0141] S30: providing a substrate;
[0142] S40: spin-coating the perovskite ink obtained in step S20 onto a substrate to form a film, and crystallizing it by VCD (vacuum drying) to obtain the perovskite film of comparative example 3.
[0143] Performance Test:
[0144] (1) The perovskite films prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were characterized by scanning electron microscopy to obtain Figure 5~Figure 11 .
[0145] Specifically, Figure 5 This is a scanning electron microscope (SEM) image of the perovskite film prepared in Example 1. Figure 6 The scanning electron microscope (SEM) image of the perovskite film prepared in Comparative Example 1. Figure 5 and Figure 6 It can be seen that compared with the perovskite film prepared in Comparative Example 1, the grain size of the perovskite film prepared in Example 1 is larger and more uniform.
[0146] Figure 7 The SEM image of the perovskite film prepared in Example 4. The temperature difference between the first temperature T1 and the second temperature T2 in the preparation method of Example 4 is smaller than that in the preparation method of Example 1. Figure 5 and Figure 7 It can be seen that the grain size of the perovskite film prepared in Example 1 is larger and more uniform than that of the perovskite film prepared in Example 4. This indicates that a larger temperature difference is more conducive to the grain growth of the perovskite film, resulting in a larger grain size and a more uniform grain size.
[0147] Figure 8 This is a scanning electron microscope (SEM) image of the perovskite film prepared in Example 2. Fig. 9 This is a scanning electron microscope (SEM) image of the perovskite film prepared in Comparative Example 2. Figure 8 and Fig. 9 It can be seen that compared with the perovskite film prepared in Comparative Example 2, the grain size of the perovskite film prepared in Example 2 is larger and more uniform.
[0148] Fig.10 This is a scanning electron microscope (SEM) image of the perovskite film prepared in Example 3. Fig.11 The scanning electron microscope (SEM) image of the perovskite film prepared in Comparative Example 3. Fig.10 and Fig.11 It can be seen that compared with the perovskite film prepared in comparative example 3, the grain size of the perovskite film prepared in example 3 is larger and more uniform.
[0149] (2) Based on the ITO / NiOx / PVK (perovskite film) / PCBM / BCP / Ag device structure, the perovskite inks of Examples 1 to 4 and Comparative Examples 1 to 3 were respectively fabricated into perovskite solar cells. The current density voltage (IV) curves of the perovskite solar cells fabricated from the perovskite inks of Examples 1 to 4 and Comparative Examples 1 to 3 were tested using PCE. The test conditions were: the simulated light intensity was 100 mW·cm -2 (AM 1.5G), temperature 25℃±3℃. The test results are shown in Table 1.
[0150] Table 1
[0151]
[0152] As can be seen from Table 1, compared with the perovskite solar cell made of the perovskite ink of Comparative Example 1, the perovskite solar cells made of the perovskite inks of Examples 1 and 4 of the present invention have a higher photoelectric conversion efficiency; compared with the perovskite solar cell made of the perovskite ink of Comparative Example 2, the perovskite solar cell made of the perovskite ink of Example 2 of the present invention has a higher photoelectric conversion efficiency; compared with the perovskite solar cell made of the perovskite ink of Comparative Example 3, the perovskite solar cell made of the perovskite ink of Example 3 of the present invention has a higher photoelectric conversion efficiency. Combined with the scanning electron microscope images of the perovskite films prepared in Examples 1 to 4 and Comparative Examples 1 to 3, it can be shown that the preparation method of the perovskite ink of the technical solution of the present invention can adjust the size and morphology of the colloidal particles to be more uniform, thereby improving the stability of the dispersed colloid in the solution, which is conducive to the subsequent formation of a uniform and stable perovskite crystal phase, and further improving the photoelectric conversion efficiency of the perovskite solar cell.
[0153] In addition, Example 1 is compared with Example 4, wherein the temperature difference between the first temperature T1 and the second temperature T2 in the preparation method of Example 4 is smaller than the temperature difference in the preparation method of Example 1. As can be seen from Table 1, the photoelectric conversion efficiency of the perovskite solar cell made of the perovskite ink of Example 1 is higher than that of Example 4. Combining the scanning electron microscope images of the perovskite films prepared in Example 1 and Example 4, it can be shown that the preparation method of the perovskite ink of Example 1 can adjust the size and morphology of the colloidal particles to be more uniform, thereby improving the stability of the dispersed colloid in the solution, which is conducive to the subsequent formation of a uniform and stable perovskite crystal phase, and further improving the photoelectric conversion efficiency of the perovskite solar cell.
[0154] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0155] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing perovskite ink, characterized in that: The steps include: Step 1: fully mixing the perovskite precursor composition at a first temperature to obtain a first mixed solution; Step 2: fully mixing the first mixed solution at a second temperature to obtain a second mixed solution, wherein the second temperature is lower than the first temperature; as well as Step 3, repeating step 1 and step 2, the number of repetitions is ≥ 1, to obtain perovskite ink; The first temperature is 60°C to 90°C, and the second temperature is 0°C to 30°C or 35°C.
2. The method for preparing perovskite ink according to claim 1, characterized in that: The perovskite precursor composition comprises a perovskite precursor, an organic solvent and an auxiliary agent; The perovskite precursor is a precursor of perovskite, and the perovskite is an ABX3 structure, wherein A represents an organic cation selected from MA + , FA + With Cs + At least one of; B represents a metal cation Pb 2+ ; X represents a halogen anion selected from I - Br - With Cl - At least one of; The organic solvent is selected from at least one of dimethylformamide, N-methylpyrrolidone and dimethyl sulfoxide; The auxiliary agent is selected from at least one of γ-butyrolactone, methylamine chloride and 1-butyl-3-methylimidazolium tetrafluoroborate.
3. The method for preparing perovskite ink according to claim 1, characterized in that: The time for fully mixing in step one is greater than the time for fully mixing when step one is repeated in step three, and the time for fully mixing in step two is equal to, greater than or less than the time for fully mixing when step two is repeated in step three.
4. The method for preparing perovskite ink according to claim 1 or 3, characterized in that: In step 1, the time for sufficient mixing is 30min~120min; in step 2, the time for sufficient mixing is 10min~30min; in step 3, the time for sufficient mixing when repeating step 1 is 30min~60min, and the time for sufficient mixing when repeating step 2 is 10min~30min.
5. The method for preparing perovskite ink according to claim 1, characterized in that: In step 3, the number of times steps 1 and 2 are repeated is 1 to 100.
6. The method for preparing perovskite ink according to claim 1, characterized in that: The first temperature in step one is equal to the first temperature in step one repeated in step three, and the second temperature in step two is equal to the second temperature in step two repeated in step three; or The first temperature in step one is equal to the first temperature in step one repeated in step three, and the second temperature in step two is not equal to the second temperature in step two repeated in step three; or The first temperature in step one is not equal to the first temperature in step one repeated in step three, and the second temperature in step two is not equal to the second temperature in step two repeated in step three; or The first temperature in step one is not equal to the first temperature in step one repeated in step three, and the second temperature in step two is equal to the second temperature in step two repeated in step three.
7. The method for preparing perovskite ink according to claim 1, characterized in that: The interval time from obtaining the first mixed solution to fully mixing the first mixed solution at the second temperature is less than 120 seconds.
8. The method for preparing perovskite ink according to claim 1, characterized in that: A first temperature control device is used to control the first temperature, and a second temperature control device is used to control the second temperature; or The first temperature and the second temperature are adjusted by a temperature control device, and the temperature adjustment speed is 1°C / min~25°C / min.
9. A perovskite ink, characterized in that: The perovskite ink is prepared by the method for preparing the perovskite ink according to any one of claims 1 to 8.
10. A method for preparing a perovskite film, characterized in that: The steps include: providing a substrate; and The perovskite ink according to claim 9 is applied to the surface of the substrate, and the perovskite film is obtained after removing the solvent.
11. A perovskite film, characterized in that: The perovskite ink is prepared by the method for preparing the perovskite ink according to claim 10.
12. A perovskite solar cell, characterized in that: Comprising the perovskite film according to claim 11.