A water-resistant multi-color continuous phase silicone acrylic emulsion and preparation method thereof

By preparing a silicone-acrylic emulsion with a cross-linked structure, the problems of poor water resistance and poor flame retardant properties of the silicone-acrylic emulsion coating film when exposed to water are solved, and efficient waterproofing, flame retardancy and mechanical performance improvement are achieved, ensuring that the coating safety and environmental protection.

CN118344517BActive Publication Date: 2024-10-22JIANG SU HENSJOR NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410370639.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-10-22
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

The existing silicone-acrylic emulsion coating film has poor water resistance when exposed to water, and the flame retardant performance without adding flame retardants is poor, which affects the decorative effect of the coating and life, health and safety.

Method used

A method for preparing a water-resistant colorful continuous phase silicone-acrylic emulsion is used, by combining isooctyl acrylate, methyl methacrylate, γ-methacryloyloxypropyltrimethoxysilane, and sodium dodecylbenzene sulfonate. , additives and ammonium persulfate and other raw materials are emulsified and polymerized, and tert-butyl hydroperoxide and hanging white block are added to prepare a silicone-acrylic emulsion with a cross-linked structure to improve its waterproof and flame retardant properties.

Benefits of technology

It significantly improves the flame retardant performance, waterproof performance, mechanical performance and UV resistance of the emulsion, and has good compatibility with the matrix, long-term stable performance, low VOC content, and is green and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004765431020000031
    Figure BDA0004765431020000031
  • Figure BDA0004765431020000032
    Figure BDA0004765431020000032
  • Figure BDA0004765431020000041
    Figure BDA0004765431020000041
Patent Text Reader

Abstract

The invention discloses a water-resistant multi-color continuous phase silicone acrylic emulsion and a preparation method thereof, and belongs to the technical field of silicone acrylic emulsion. Each raw material is calculated as follows according to weight parts: 55-65 parts of isooctyl acrylate, 65-75 parts of methyl methacrylate, 6-10 parts of acrylic acid, 4-6 parts of γ-methacryloxypropyl trimethoxysilane, 0.5-1.5 parts of sodium dodecylbenzene sulfonate, 100-120 parts of deionized water, 5-15 parts of auxiliary agents, 0.2-0.4 parts of ammonium persulfate, 0.1-0.3 parts of tert-butyl hydroperoxide, and 0.1-0.3 parts of bleaching powder. The emulsion prepared by the present invention has stable and efficient flame retardant performance, waterproof performance, mechanical performance and a certain degree of anti-ultraviolet performance, and is green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicone acrylic emulsions, and in particular relates to a water-resistant multi-colored continuous phase silicone acrylic emulsion and a preparation method thereof. Background Art

[0002] In recent years, the types of architectural coatings have increased day by day, and people have more and more choices for architectural coatings. Among them, water-in-water multi-color coatings are all-water-based, multi-color, environmentally friendly high-tech coating products. They are mainly used to imitate various natural marbles. They have extremely high simulation and excellent adhesion and elasticity. Their hanging weight is only one twentieth of that of real stone paints. They are widely used for their low VOC (volatile organic compounds) and other characteristics. Water-in-water multi-color coatings and their derivative products (including sand-in-water multi-color coatings) are widely used for their realistic imitation stone effects and low VOC (volatile organic compounds) and other characteristics.

[0003] Water-based multi-color paint is divided into two parts: base paint and continuous phase. The continuous phase is composed of protective glue and emulsion. At present, the emulsions used for the continuous phase mainly include pure acrylic emulsion, styrene acrylic emulsion, silicone acrylic emulsion and fluoroacrylic emulsion. Among them, silicone acrylic emulsion is the most widely used emulsion due to its excellent cost performance. Silicone acrylic emulsion not only has good weather resistance, but also has good water resistance. However, even if silicone acrylic emulsion with good water resistance is used to prepare water-based multi-color paint, there is still a common problem of poor water whitening resistance of the coating film. This is because the silicone-acrylic emulsion is a multiphase system. When encountering rain, the water absorption rate of each component is different, resulting in different refractive indices of light, causing the coating surface to turn white when exposed to water, affecting the decorative effect and protective function of the colorful paint. If a waterproofing agent is added, it has poor compatibility with the silicone-acrylic emulsion, which will affect the mechanical properties of the colorful paint. Moreover, the silicone-acrylic emulsion without adding flame retardants has poor flame retardant properties, which will seriously affect people's life, health and safety when encountering a fire. In summary, it is urgent to design a silicone-acrylic emulsion that can improve the above problems to meet the higher demands in the field of water-based colorful paint technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a water-resistant multi-colored continuous phase silicone acrylic emulsion and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a water-resistant multi-color continuous phase silicone-acrylic emulsion comprises the following steps:

[0007] A1. Add isooctyl acrylate, methyl methacrylate, acrylic acid, γ-methacryloxypropyltrimethoxysilane (KH-570), sodium dodecylbenzenesulfonate (emulsifier) ​​and deionized water into a reactor, emulsify to obtain an emulsion; add an auxiliary agent and ammonium persulfate (initiator), keep the reaction at 80-85°C for 2h to initiate a polymerization reaction;

[0008] A2. When the reaction kettle is cooled to 70-75°C, tert-butyl hydroperoxide (oxidant) is added to the product obtained in step A1, and bleaching powder (reducing agent) is added after 5 minutes. After keeping warm for 30 minutes, a water-resistant multi-colored continuous phase silicone acrylic emulsion is obtained.

[0009] The raw materials are calculated in parts by weight as follows: 55-65 parts of isooctyl acrylate, 65-75 parts of methyl methacrylate, 6-10 parts of acrylic acid, 4-6 parts of γ-methacryloxypropyltrimethoxysilane, 0.5-1.5 parts of sodium dodecylbenzene sulfonate, 100-120 parts of deionized water, 5-15 parts of auxiliary agents, 0.2-0.4 parts of ammonium persulfate, 0.1-0.3 parts of tert-butyl hydroperoxide, and 0.1-0.3 parts of bleaching powder.

[0010] By selecting isooctyl acrylate and methyl methacrylate as the matrix, the silicone-acrylic emulsion obtained has higher water resistance and hardness; tert-butyl hydroperoxide is weakly alkaline and bleaching powder is weakly acidic, which can stabilize the acid-base balance of the chemical reaction system and facilitate the chemical reaction; the introduction of γ-methacryloxypropyltrimethoxysilane cross-links with the matrix, making the emulsion film dense and improving the water resistance of the emulsion.

[0011] Furthermore, the auxiliary agent is prepared by the following steps:

[0012] S1. In a three-necked flask equipped with a stirring device, iminodiacetic acid, hydroxyethyl acrylate and N,N-dimethylformamide (DMF) were mixed uniformly, stirred until the solid was dissolved, and then dibutyltin oxide (catalyst) and dicyclohexylcarbodiimide (DCC, dehydrating agent) were added, and the temperature was raised to 85° C. for reaction for 4 h. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, the solvent was removed by rotary evaporation, and vacuum dried to obtain intermediate 1; the ratio of iminodiacetic acid, hydroxyethyl acrylate, DMF, dibutyltin oxide and DCC was 14.5 g:11.6 g:75 mL:0.2 g:20.6 g;

[0013] Under the catalysis of dibutyltin oxide and DCC, the carboxyl group on the iminodiacetic acid and the hydroxyl group on the hydroxyethyl acrylate undergo esterification reaction. By controlling the molar ratio of the two to be close to 1:1 and the iminodiacetic acid to be slightly excessive, only one carboxyl group on the iminodiacetic acid participates in the reaction to obtain intermediate 1. The specific reaction process is as follows:

[0014]

[0015] S2, at room temperature, in a three-necked flask equipped with a stirring device, the intermediate 1, dichlorodiphenylsilane, triethylamine and DMF were mixed and stirred uniformly under nitrogen protection, the reaction temperature was controlled to 75°C, and the reaction was kept warm for 5 hours. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by vacuum distillation, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 4:7), and the eluent was removed by rotary evaporation to obtain intermediate 2; the ratio of the amount of intermediate 1, dichlorodiphenylsilane, triethylamine and DMF was 48.5g:25.1g:15mL:100mL;

[0016] Intermediate 1 and dichlorodiphenylsilane undergo nucleophilic substitution, and the molar ratio of the two is controlled to be close to 2:1 and intermediate 1 is slightly excessive, and triethylamine removes the hydrogen chloride generated by the reaction to obtain intermediate 2; the specific reaction process is as follows:

[0017]

[0018] S3. In a three-necked flask equipped with a stirring device, 2,2,6,6-tetramethylpiperidinol, n-octane and molybdenum trioxide were mixed and stirred evenly, heated to 85°C, and tert-butyl hydroperoxide aqueous solution (mass fraction 18%) was added dropwise. After the addition was completed, the mixture was refluxed for 10 hours, filtered, activated carbon was added to the filtrate, stirred for 1 hour, allowed to stand, filtered, the filtrate was taken, and n-octane was removed by vacuum distillation to obtain intermediate 3; the ratio of 2,2,6,6-tetramethylpiperidinol, n-octane, molybdenum trioxide and tert-butyl hydroperoxide aqueous solution was 15.7g:15.8g:0.4g:10.3g;

[0019] Under the catalysis of molybdenum trioxide and the oxidation of tert-butyl hydroperoxide, 2,2,6,6-tetramethylpiperidinol and n-octane undergo a free radical coupling reaction; n-octane participates in the reaction process as a reactant and also acts as a reaction solvent, which can reduce the formation of by-products to obtain intermediate 3; the specific reaction process is as follows:

[0020]

[0021] S4. In a three-necked flask equipped with a stirring device, intermediate 2, intermediate 3 and DMF were mixed, stirred until the solid was completely dissolved, and then dibutyltin oxide and DCC were added, and the temperature was raised to 85°C for reaction for 4 hours. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. The mixture was purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 7:3). The eluent was removed by rotary evaporation to obtain an auxiliary agent. The ratio of the amount of intermediate 2, intermediate 3, DMF, dibutyltin oxide and DCC was 64.2 g: 58.8 g: 200 mL: 1.1 g: 41.2 g.

[0022] Under the catalysis of dibutyltin oxide and DCC, the carboxyl group on intermediate 2 and the hydroxyl group on intermediate 3 undergo esterification reaction. By controlling the molar ratio of the two to be close to 1:2 and the intermediate 3 to be slightly excessive, the two hydroxyl groups on intermediate 3 participate in the reaction to obtain an auxiliary agent; the structure of the auxiliary agent is shown below:

[0023]

[0024] The prepared auxiliary agent molecules contain Si-N flame retardant components, hindered amines, long carbon chains, and benzene ring structures. Among them, the Si-N flame retardant component has the synergistic flame retardant effect of silicon-based and nitrogen-based flame retardants. Compared with general silicon-based flame retardants in which silicon and oxygen are directly connected, Si-N is a covalent bond, with stable physical and chemical properties, and generates a dense Si-C or Si-Si layer during combustion, with a better flame retardant effect; in addition, the hindered amine in the auxiliary agent acts as a light stabilizer, which decomposes hydrogen dioxide to produce stable nitrogen oxide free radicals during light protection. This compound can very effectively capture the free radicals generated in photo-oxidative degradation, which can It effectively inhibits the photo-oxidative degradation of the matrix and can be regenerated under stable conditions, significantly improving the matrix's UV resistance; the long carbon chain belongs to the methylene chain segment, has a strong hydrophobicity, can improve the matrix's waterproof performance and a certain degree of mechanical properties, and can be interspersed in the matrix's molecular chain to improve stability; finally, the additive contains a benzene ring, and under the action of the initiator, the acrylate structure at one end of the additive can participate in the reaction during the polymerization process and connect to the acrylic acid molecular chain, improving the compatibility of the additive with the matrix and improving the waterproofness and mechanical properties of the matrix; and the performance is stable and not easy to fall off.

[0025] Beneficial effects of the present invention:

[0026] 1. The emulsion prepared by the present invention uses water as solvent, has low VOC content, and is green and environmentally friendly;

[0027] 2. Using the silicon cross-linking method to introduce silicone into acrylic acid can greatly improve the waterproof performance of the emulsion;

[0028] 3. The prepared additive can significantly improve the flame retardant, waterproof, mechanical and UV resistance of the emulsion, and has good compatibility with the matrix and long-term stable performance;

[0029] Therefore, the emulsion prepared by the invention has stable and efficient flame retardant performance, waterproof performance, mechanical performance and a certain degree of anti-ultraviolet performance, and is green and environmentally friendly. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] Preparation aids:

[0033] S1. In a three-necked flask equipped with a stirring device, 14.5 g of iminodiacetic acid, 11.6 g of hydroxyethyl acrylate and 75 mL of DMF were mixed evenly, stirred until the solid was dissolved, and then 0.2 g of dibutyltin oxide and 20.6 g of DCC were added, and the temperature was raised to 85° C. for reaction for 4 h. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, the solvent was removed by rotary evaporation, and vacuum dried to obtain intermediate 1.

[0034] S2. At room temperature, 48.5 g of intermediate 1, 25.1 g of dichlorodiphenylsilane, 15 mL of triethylamine and 100 mL of DMF were mixed and stirred evenly in a three-necked flask equipped with a stirring device under nitrogen protection. The reaction temperature was controlled to 75° C. and the reaction was kept warm for 5 h. After the reaction was completed, the product was filtered and partially distilled off under reduced pressure. The product was then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 4:7), and the eluent was removed by rotary evaporation to obtain intermediate 2.

[0035] S3, in a three-necked flask equipped with a stirring device, 15.7g of 2,2,6,6-tetramethylpiperidinol, 15.8g of n-octane, and 0.4g of molybdenum trioxide were mixed and stirred evenly, heated to 85°C, and 10.3g of tert-butyl hydroperoxide aqueous solution (mass fraction 18%) was added dropwise. After the addition was completed, reflux reaction was carried out for 10h, filtered, activated carbon was added to the filtrate, stirred for 1h, allowed to stand, filtered, the filtrate was taken, and n-octane was removed by vacuum distillation to obtain intermediate 3;

[0036] S4. In a three-necked flask equipped with a stirring device, 64.2 g of intermediate 2, 58.8 g of intermediate 3 and 200 mL of DMF were mixed and stirred until the solid was completely dissolved. Then, 1.1 g of dibutyltin oxide and 41.2 g of DCC were added and the temperature was raised to 85°C for reaction for 4 h. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered and part of the solvent was removed by rotary evaporation. The mixture was purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 7:3). The eluent was removed by rotary evaporation to obtain an auxiliary agent.

[0037] Example 2

[0038] Preparation aids:

[0039] S1. In a three-necked flask equipped with a stirring device, 29 g of iminodiacetic acid, 23.2 g of hydroxyethyl acrylate and 150 mL of DMF were mixed evenly, stirred until the solid was dissolved, and then 0.4 g of dibutyltin oxide and 41.2 g of DCC were added, and the temperature was raised to 85° C. for reaction for 4 h. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, the solvent was removed by rotary evaporation, and vacuum dried to obtain intermediate 1;

[0040] S2. At room temperature, under nitrogen protection, 97 g of intermediate 1, 50.2 g of dichlorodiphenylsilane, 30 mL of triethylamine and 200 mL of DMF were mixed and stirred evenly in a three-necked flask equipped with a stirring device. The reaction temperature was controlled to 75° C. and the reaction was kept warm for 5 h. After the reaction was completed, the mixture was filtered and partially distilled off under reduced pressure. The mixture was then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 4:7), and the eluent was removed by rotary evaporation to obtain intermediate 2.

[0041] S3, in a three-necked flask equipped with a stirring device, 31.4g of 2,2,6,6-tetramethylpiperidinol, 31.6g of n-octane, and 0.8g of molybdenum trioxide were mixed and stirred evenly, heated to 85°C, and 20.6g of tert-butyl hydroperoxide aqueous solution (mass fraction 18%) was added dropwise. After the addition was completed, the reaction was refluxed for 10h, filtered, activated carbon was added to the filtrate, stirred for 1h, allowed to stand, filtered, the filtrate was taken, and n-octane was removed by vacuum distillation to obtain intermediate 3;

[0042] S4. In a three-necked flask equipped with a stirring device, 128.4 g of intermediate 2, 117.6 g of intermediate 3 and 400 mL of DMF were mixed and stirred until the solid was completely dissolved. Then 2.2 g of dibutyltin oxide and 82.4 g of DCC were added and the temperature was raised to 85°C for reaction for 4 h. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered and part of the solvent was removed by rotary evaporation. The mixture was purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 7:3). The eluent was removed by rotary evaporation to obtain an auxiliary agent.

[0043] Example 3

[0044] A method for preparing a water-resistant multi-color continuous phase silicone-acrylic emulsion comprises the following steps:

[0045] A1, 55g of isooctyl acrylate, 65g of methyl methacrylate, 6g of acrylic acid, 4g of γ-methacryloxypropyltrimethoxysilane, 0.5g of sodium dodecylbenzenesulfonate and 100g of deionized water were added to a reactor and emulsified to obtain an emulsion; 5 parts of the auxiliary agent obtained in Example 1 and 0.2g of ammonium persulfate were added, and the mixture was kept at 80°C for 2h to initiate a polymerization reaction;

[0046] A2. When the temperature of the reaction kettle drops to 70°C, add 0.1 g of tert-butyl hydroperoxide to the product obtained in step A1, and then add 0.1 g of bleaching powder after 5 minutes. After keeping the temperature for 30 minutes, a water-resistant multi-colored continuous phase silicone acrylic emulsion is obtained;

[0047] Water-based multi-color paint was prepared according to the formula in Table 1:

[0048] Table 1

[0049]

[0050] The base paint and the protective glue are mixed, and then mixed with a continuous phase to prepare a water-based multi-color paint.

[0051] Example 4

[0052] A method for preparing a water-resistant multi-color continuous phase silicone-acrylic emulsion comprises the following steps:

[0053] A1, 60g of isooctyl acrylate, 70g of methyl methacrylate, 8g of acrylic acid, 5g of γ-methacryloxypropyltrimethoxysilane, 1g of sodium dodecylbenzenesulfonate and 110g of deionized water were added to a reactor, emulsified to obtain an emulsion; 10g of the auxiliary agent obtained in Example 2 and 0.3g of ammonium persulfate were added, and the mixture was kept at 80°C for 2h to initiate a polymerization reaction;

[0054] A2. When the temperature of the reaction kettle drops to 70°C, add 0.2g of tert-butyl hydroperoxide to the product obtained in step A1, and add 0.2g of bleaching powder after 5 minutes. After keeping warm for 30 minutes, a water-resistant multi-colored continuous phase silicone acrylic emulsion is obtained;

[0055] Water-based multi-color paint was prepared according to the formula in Table 2:

[0056] Table 2

[0057]

[0058] The base paint and the protective glue are mixed, and then mixed with a continuous phase to prepare a water-based multi-color paint.

[0059] Example 5

[0060] A method for preparing a water-resistant multi-color continuous phase silicone-acrylic emulsion comprises the following steps:

[0061] A1, 65g of isooctyl acrylate, 75g of methyl methacrylate, 10g of acrylic acid, 6g of γ-methacryloxypropyltrimethoxysilane, 1.5g of sodium dodecylbenzenesulfonate and 120g of deionized water were added to a reactor, emulsified to obtain an emulsion; 15g of the auxiliary agent obtained in Example 2 and 0.4g of ammonium persulfate were added, and the mixture was kept at 80°C for 2h to initiate a polymerization reaction;

[0062] A2. When the temperature of the reaction kettle drops to 70°C, add 0.3g of tert-butyl hydroperoxide to the product obtained in step A1, and then add 0.3g of bleaching powder after 5 minutes. After keeping warm for 30 minutes, a water-resistant multi-colored continuous phase silicone acrylic emulsion is obtained;

[0063] Water-based multi-color paint was prepared according to the formula in Table 3:

[0064] Table 3

[0065]

[0066] The base paint and the protective glue are mixed, and then mixed with a continuous phase to prepare a water-based multi-color paint.

[0067] Comparative Example 1

[0068] No auxiliary agent was added, and the remaining steps were the same as in Example 5.

[0069] Comparative Example 2

[0070] Use commercially available silicone-acrylic emulsion produced by Beijing Jiasheng Building Materials Co., Ltd.

[0071] The following performance tests were performed on the silicone acrylic emulsion prepared in step A2 of Example 3-5:

[0072] Viscosity and pH value: The viscosity (mPa·s) of the latex was measured by a rheometer; the pH value of the latex was measured by a pH meter;

[0073] Solid content: Weigh 0.2g of sample in a flat-bottom dish, place in a vacuum oven at 125℃ and air pressure below 20kPa for 1h, and calculate the solid content (%);

[0074] The measured results are shown in Table 4:

[0075] Table 4

[0076]

[0077] The water-based multi-color coatings prepared in Examples 3-5 and Comparative Examples 1-2 were subjected to the following performance tests:

[0078] The performance was measured using the HG / T 4343-2012 "Water-based Multi-color Architectural Coatings" standard; and the water resistance of the coating was tested after 30 days;

[0079] Place the test piece tightly on the fine sand with a thickness of 20mm, with the coating facing upwards. Then drop a steel spherical weight I with a diameter of (50±4)mm and a mass of (500±20)g or a steel spherical weight II with a diameter of (60±4)mm and a mass of (1000±20)g freely from a height of 100cm±1cm. Select three positions on the test piece that are not less than 50mm apart and not less than 50mm from the edge of the test piece for testing. Observe the surface coating of the test piece with the naked eye to see if there are cracks or peeling, and evaluate the impact resistance grade (if the steel spherical weight I passes, it is Grade I, and if the steel spherical weight II passes, it is Grade II);

[0080] The VOC content is determined using the national standard GB 18582-2020 "Limits of Hazardous Substances in Architectural Wall Coatings";

[0081] The national standard GB 12441-2005 "Surface fire retardant coating" was used to measure the flame retardant time and mass loss of the sample before and after 30 days of application;

[0082] The measured results are shown in Table 5:

[0083] Table 5

[0084]

[0085] As can be seen from Table 5, the silicone acrylic emulsion prepared by the present invention has higher flame retardancy, waterproofness, mechanical properties and UV resistance than the control example, and has low VOC content, is green and environmentally friendly, and has stable performance, and has important application value in the field of water-based multi-color coating technology.

[0086] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0087] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a water-resistant multi-color continuous phase silicone acrylic emulsion, characterized in that: The following steps are involved: A1. Add isooctyl acrylate, methyl methacrylate, acrylic acid, γ-methacryloxypropyltrimethoxysilane, sodium dodecylbenzenesulfonate and deionized water into a reaction kettle, emulsify and prepare an emulsion; add an auxiliary agent and ammonium persulfate, keep the temperature at 80-85°C for 2 hours to initiate a polymerization reaction; A2. When the temperature of the reaction kettle drops to 70-75°C, add tert-butyl hydroperoxide to the product obtained in step A1, and add bleaching powder after 5 minutes. After keeping warm for 30 minutes, a water-resistant multi-colored continuous phase silicone acrylic emulsion is obtained; The raw materials are calculated in parts by weight as follows: 55-65 parts of isooctyl acrylate, 65-75 parts of methyl methacrylate, 6-10 parts of acrylic acid, 4-6 parts of γ-methacryloxypropyltrimethoxysilane, 0.5-1.5 parts of sodium dodecylbenzenesulfonate, 100-120 parts of deionized water, 5-15 parts of auxiliary agent, 0.2-0.4 parts of ammonium persulfate, 0.1-0.3 parts of tert-butyl hydroperoxide, and 0.1-0.3 parts of bleaching agent; Wherein, the auxiliary agent is prepared by the following steps: S1. Mix iminodiacetic acid, hydroxyethyl acrylate and DMF evenly, stir until the solid is dissolved, then add dibutyltin oxide and dicyclohexylcarbodiimide, heat to 85°C and react for 4 hours, stir continuously during the reaction, filter, rotary evaporate and vacuum dry to obtain intermediate 1; the ratio of iminodiacetic acid, hydroxyethyl acrylate, DMF, dibutyltin oxide and DCC is 14.5g:11.6g:75mL:0.2g:20.6g; S2. At room temperature, under nitrogen protection, the intermediate 1, dichlorodiphenylsilane, triethylamine and DMF were mixed and stirred uniformly, the reaction temperature was controlled to 75°C, and the reaction was kept warm for 5 hours. After the reaction was completed, the intermediate 2 was obtained by filtration, vacuum distillation, column chromatography purification, and rotary evaporation. The ratio of the amount of intermediate 1, dichlorodiphenylsilane, triethylamine and DMF was 48.5g:25.1g:15mL:100mL. S3, 2,2,6,6-tetramethylpiperidinol, n-octane, and molybdenum trioxide were mixed and stirred uniformly, heated to 85°C, and tert-butyl hydroperoxide aqueous solution was added dropwise. After the addition was completed, the mixture was refluxed for 10 hours, filtered, activated carbon was added to the filtrate, stirred for 1 hour, allowed to stand, filtered, the filtrate was taken, and distilled under reduced pressure to obtain intermediate 3; the ratio of 2,2,6,6-tetramethylpiperidinol, n-octane, molybdenum trioxide, and tert-butyl hydroperoxide aqueous solution was 15.7g:15.8g:0.4g:10.3g; S4. Mix intermediate 2, intermediate 3 and DMF, stir until the solid is completely dissolved, then add dibutyltin oxide and DCC, raise the temperature to 85°C and react for 4 hours, stir continuously during the reaction, and after the reaction is completed, filter, rotary evaporate, and purify by column chromatography. Remove the eluent by rotary evaporation to obtain an auxiliary agent; the usage ratio of intermediate 2, intermediate 3, DMF, dibutyltin oxide and DCC is 64.2g:58.8g:200mL:1.1g:41.2g.

2. A water-resistant multi-color continuous phase silicone acrylic emulsion, characterized in that: Prepared according to the method of claim 1.