A flux for high nitrogen flux-cored wire surfacing and a preparation method thereof

By using a combination of magnesium oxide, calcium fluoride, alumina, wollastonite, magnesium carbonate, rutile, barium titanate and other ingredients in the flux, the problems of pores and indentations during high-nitrogen flux-cored wire welding are solved, achieving It improves the hardness and shape of the weld seam to ensure welding quality and beautiful surface.

CN118357633BActive Publication Date: 2024-10-29TIANJIN GOLDEN BRIDGE WELDING MATERIALS GRP CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410780554.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-29
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

Existing high-nitrogen flux-cored welding wires are prone to pores and indentations during the welding process, resulting in poor surface quality of the weld, especially when welding to large specifications, and the hardness is not enough to meet high requirements.

Method used

A flux formula including magnesium oxide, calcium fluoride, alumina, wollastonite, magnesium carbonate, rutile, and barium titanate is used. Through the combination of these ingredients, the slag viscosity, fluidity, and reactivity of the flux are adjusted to inhibit Nitrogen is generated and dissolved in the weld through the reaction of barium titanate and titanium nitride to avoid the generation of nitrogen.

Benefits of technology

It realizes that pores and indentations are not easily generated during the welding process, the surface of the weld is beautiful, and the HRC hardness of the weld reaches more than 40, which meets the hardness and forming requirements of high-nitrogen welding wire.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118357633B_ABST
    Figure CN118357633B_ABST
Patent Text Reader

Abstract

The invention provides a flux for high nitrogen flux-cored wire surfacing and a preparation method thereof, the flux comprising powder and a binder, wherein the powder comprises by weight: 30-35% magnesium oxide, 20-25% calcium fluoride, 5-10% magnesium carbonate, 20-25% aluminum oxide, 5-10% wollastonite, 2-3% rutile, and 2-3% barium titanate. The flux for high nitrogen flux-cored wire surfacing prepared by the invention can be used for large-scale standard welding, the HRC hardness of the surfacing layer can reach more than 40, and the weld is bright without pores or indentations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding materials, in particular to a flux used for high nitrogen flux-cored wire surfacing and a preparation method thereof. Background Art

[0002] Surfacing technology is a type of welding technology, but it is different from general welding. It is not a general structural connection, but a method of welding to coat a layer of metal with special properties on the surface of the part so that it can serve in a special working environment.

[0003] Overlay welding is widely used in the surface treatment of automobiles, tractors, and metallurgical rollers. The rational use of overlay welding technology has great economic significance. The wear resistance of a welded roller is more than twice that of a new roller, which reduces the maintenance cost of the roller and the purchase cost of the roller.

[0004] The commonly used flux-cored cladding wires in the industry are mainly strengthened with C, Cr, Mo, and Mn elements. For example, Patent 101564804A designs a cladding flux that mainly relies on C compounds (silicon carbide) to assist in hardness enhancement. However, considering the requirements for toughness and crack resistance, 1Cr13 welding wire products have an upper limit on the carbon content of the cladding layer and rely on the use of precious metals for strengthening. In order to reduce the cost, the industry later developed and promoted high-nitrogen welding wires, using more N elements for hardness enhancement. However, nitrogen-containing substances are easily decomposed into nitrogen at high temperatures, causing nitrogen pores or indentations, resulting in poor surface quality, which is particularly evident under large-scale welding. Summary of the invention

[0005] In view of this, the present invention aims to propose a flux for high nitrogen flux-cored wire surfacing and a preparation method thereof, the flux can meet the requirements of excellent slag removal performance and beautiful weld surface shape, especially it is not easy to produce pores and indentations when a larger standard welding is adopted during the welding process, and the HRC hardness of the surfacing layer reaches above 40.

[0006] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0007] A flux for high nitrogen flux-cored wire surfacing comprises powder and a binder. The powder comprises, by weight percentage, 30-35% magnesium oxide, 20-25% calcium fluoride, 5-10% magnesium carbonate, 20-25% aluminum oxide, 5-10% wollastonite, 2-3% rutile and 2-3% barium titanate.

[0008] Among them, magnesium oxide is a kind of alkaline oxide with a high melting point. Its main function in sintering flux is slag formation. It is an indispensable raw material in the manufacture of sintering flux. The viscosity of flux slag can be adjusted in sintering flux, which can effectively improve welding processability. However, when the magnesium oxide content is high, the weld line will be thickened. The designed addition amount is: 30-35%.

[0009] Calcium fluoride is a common raw material in alkaline flux. CaF2 can also effectively reduce the H content in the weld metal and arc atmosphere. At the same time, an appropriate amount of calcium fluoride can also effectively improve the fluidity of the slag during welding, but the F element will also produce a reverse ionization effect, and excessive amounts will cause arc instability. The designed addition amount is: 20-25%.

[0010] The addition of alumina ensures the slag removal during welding. Alumina has a high melting point and low density. It can float above the molten pool during welding, leading the formation of the slag shell, so that the flux has good slag removal. The welding slag during the welding process can evenly cover the surface of the weld metal, making the slag shell well-formed, facilitating slag removal during on-site welding, and obtaining good weld formation. The designed addition amount is: 20-25%.

[0011] The main components of wollastonite are silicon dioxide and calcium oxide. The main role of silicon dioxide in the flux is to form slag and reduce the basicity of the flux slag system. The appropriate silicon dioxide content in the flux can well ensure that the fluidity of the molten iron during welding is moderate, the surface of the welding slag is flat, and the slag removal is good. However, excessive silicates are likely to increase the burnout of the weld, which may have an adverse effect on the hardness of the cladding. The designed addition amount is: 5-10%.

[0012] Magnesium carbonate is an important additive to achieve the effect of anti-porosity and indentation: magnesium carbonate will produce magnesium oxide and carbon dioxide gas during welding. The carbon dioxide atmosphere can inhibit the nitrogen in the flux-cored wire from overflowing at high temperature to a certain extent. The decomposition temperature of magnesium carbonate itself is low, and the carbon dioxide overflow speed is also fast. A small amount of addition will not produce carbon dioxide pores. The designed addition amount is: 5-10%.

[0013] The use of rutile and barium titanate in combination with magnesium carbonate is the focus of the present invention: barium titanate can react with nitrogen-containing substances in flux-cored welding wire to produce titanium nitride, which will be dissolved in the weld to avoid the generation of nitrogen. The main component of rutile itself is titanium oxide, and its main function here is to adjust the titanium content in the flux slag and promote the titanium nitride reaction. At the same time, the carbon dioxide decomposed from magnesium carbonate also has the effect of inhibiting the generation of nitrogen, which also promotes the formation of titanium nitride. The amount of barium titanate added should correspond to the nitrogen content in the flux-cored welding wire. After rutile reaches the threshold, excessive addition has no obvious effect on promoting the reaction. The designed addition amount is: rutile: 2-3%, barium titanate: 2-3%.

[0014] Furthermore, the binder is sodium water glass, and its addition amount is 22-25% of the total mass of the powder.

[0015] Furthermore, since barium titanate needs to participate in the gold melting reaction, the particle size of barium titanate is 200-300 mesh, and the particle size of the remaining powders is 40-100 mesh.

[0016] Furthermore, the moisture content of the powder is less than 0.1%.

[0017] The present invention also provides a method for preparing the flux for high nitrogen flux-cored wire surfacing as described above, the method comprising the following steps:

[0018] 1) Mix the drug powder according to the formula ratio, add water glass, stir and granulate;

[0019] 2) Bake at 400-500 degrees Celsius for 1-2 hours.

[0020] Furthermore, the method further comprises step 1) drying and baking the medicine powder after mixing at a temperature of 100-120°C.

[0021] Compared with the prior art, the flux for high nitrogen flux-cored wire surfacing and the preparation method thereof described in the present invention have the following advantages:

[0022] The flux for high nitrogen flux-cored wire surfacing of the present invention can ensure good flux forming and avoid nitrogen pores when welding 1Cr13 high nitrogen flux-cored wire even with a larger welding specification. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0024] Figure 1 The welding photos of the flux prepared in each embodiment and comparative example; (a) is embodiment 1, (b) is embodiment 2, (c) is comparative example 1, (d) is comparative example 2, (e) is comparative example 3, (f) is comparative example 4, and (g) is comparative example 5. DETAILED DESCRIPTION

[0025] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] A flux for high nitrogen flux-cored wire surfacing, the composition of which is shown in the following table.

[0028] Table 1. Example and comparative example ratio table (%)

[0029]

[0030] According to the above ratio table, the powders are mixed according to the formula ratio. Except for barium titanate, the particle size of the remaining powders is 40-100 mesh, and the water content of the powders is less than 0.1%. If necessary, it can be baked at 120 degrees Celsius. Then add sodium water glass, the amount of sodium water glass added is 24% of the total weight of the powder, and then stir and granulate. Then bake at 500 degrees Celsius for 2 hours. After the flux cools down, welding can be carried out.

[0031] Use 4.0mm flux-cored wire, and the welding specifications are shown in the table below. Perform 6 layers of cladding on Q345 base material. After cladding, grind the top layer, then use an HRC hardness tester to measure, and observe the welding process.

[0032] Table 2. Wire welding specifications

[0033]

[0034] Table 3. Comparison of wire welding results

[0035]

[0036] It can be seen from the photos and data that the surface quality of Examples 1 and 2 is good, and the hardness values ​​are both above 40. The surface indentations of Comparative Examples 1-2 are obvious, and the surface indentation of Comparative Example 3 is serious. Although the hardness values ​​of Comparative Examples 4 and 5 are also good, there is a sticky residue phenomenon on the surface of Comparative Example 4, and there is a shallow indentation on the surface of Comparative Example 5.

[0037] Analyzing the reasons, it can be seen from Comparative Examples 1-2 that due to the lack of addition of rutile and barium titanate, the nitrogen generated during welding cannot be combined with the alloy elements in the weld, and the weld has a low solubility for nitrogen, and can only be discharged from the weld in the form of nitrogen, and finally an indentation is formed on the weld surface. It can be seen from Comparative Example 3 that when magnesium carbonate is not added, due to the lack of other atmospheres, the gas phase pressure on the weld surface is low, which makes the nitrogen in the weld form nitrogen more quickly and violently to be discharged from the weld, and finally a serious indentation is formed. It can be seen from Comparative Example 4 that when barium titanate is more, because the titanium compound has a high melting temperature, short slag, and is easy to crystallize, the aluminum-containing material in the slag shell is combined with the weld surface. Comparative Example 5 shows that the particle size of barium titanate in the formula is very critical. The titanium in barium titanate can help the nitrogen element to remain in the weld in the form of a solid solution, thereby reducing the generation of nitrogen escaping in the form of gas. The powder with a coarser particle size cannot be completely transitioned during the fusion welding process, and part of it will be lost in the slag shell, and the effect will be weakened, resulting in an increase in overflow nitrogen. The present invention first uses a certain amount of magnesium carbonate to adjust the atmospheric pressure on the weld surface, slowing down the nitrogen discharge speed and giving it sufficient time to react with the weld alloy, while adding rutile and barium titanate. The titanium element in these two products can react with nitrogen to form titanium nitride substances, which are solid-dissolved in the weld, and ultimately reduce the loss and emission of nitrogen. In addition, according to the specified formula design, better weld bead shaping and weld hardness can be formed.

[0038] The flux of the present invention can be used for a special high nitrogen type flux-cored cladding wire. The HRC hardness of the weld after welding meets 40 or above, the weld is beautifully formed, and even with a large heat input, it is still not easy to produce pores and indentation defects.

[0039] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A flux for high nitrogen flux-cored wire surfacing, characterized in that: The invention comprises medicine powder and a binder. The medicine powder comprises, by weight percentage, 30-35% magnesium oxide, 20-25% calcium fluoride, 5-10% magnesium carbonate, 20-25% aluminum oxide, 5-10% wollastonite, 2-3% rutile and 2-3% barium titanate. The particle size of the barium titanate is 200-300 meshes.

2. The flux for high nitrogen flux-cored wire surfacing according to claim 1, characterized in that: The binder is sodium water glass, and its addition amount is 22-25% of the total weight of the powder.

3. The flux for high nitrogen flux-cored wire surfacing according to claim 1, characterized in that: The particle size of the remaining drug powders except barium titanate is 40-100 mesh.

4. The flux for high nitrogen flux-cored wire surfacing according to claim 1, characterized in that: The moisture content of the powder is less than 0.1%.

5. A method for preparing a flux for high nitrogen flux-cored wire surfacing according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: 1) Mix the drug powder according to the formula ratio, add the binder, stir and granulate; 2) Bake at 400-500 degrees Celsius for 1-2 hours.

6. The method for preparing the flux for high nitrogen flux-cored wire surfacing according to claim 5, characterized in that: The method also includes step 1) drying and baking the powder after mixing at a temperature of 100-120°C.

Citation Information

Patent Citations

  • Hard surfacing sintered flux and manufacturing method thereof

    CN101564804A

  • 9Ni steel sintered flux and preparation method thereof

    CN101954553A

  • Titanium carbide high-crack-resistance surfacing flux-cored wire, and preparation method and application thereof

    CN113977131A