A processing method for improving residual compressive stress on rolling surface of bearing roller
Through quenching, tempering and cold treatment, combined with multiple grinding and polishing treatments, the problem of small residual compressive stress and poor distribution uniformity on the surface of the bearing roller is solved, and efficient residual compressive stress control on the roller surface is achieved, significantly improving improve the fatigue life of the bearing.
Patent Information
- Application Number
- CN202410791963.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-19
AI Technical Summary
In the existing bearing roller processing methods, the residual compressive stress on the roller surface is small and the distribution uniformity is poor, which affects the fatigue life of the bearing.
Through quenching, tempering and cold treatment, combined with rough grinding, semi-fine grinding, fine grinding and super-finishing, the residual compressive stress on the working surface of the roller is controlled, and specific abrasives and grinding wheel speeds are used to perform multiple grinding and polishing treatments. , ensuring uniformity and efficiency of residual compressive stress.
Significantly improves the fatigue life of bearing rollers, ensuring that the residual compressive stress is not less than 680MPa and the range is not greater than 63MPa, improving the fatigue resistance of the roller surface.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a processing method for improving the residual compressive stress of a rolling surface of a bearing roller, and belongs to the technical field of bearing roller processing. Background Art
[0002] As an important component of the bearing, the life of the roller directly determines the reliability of the bearing. Studies have shown that the residual stress distribution on the working surface of the bearing has an important influence on the initiation and expansion of cracks on the working surface of the bearing parts, which in turn affects the fatigue life of the bearing. When there is residual compressive stress on the working surface of the bearing parts, it can effectively inhibit the initiation and expansion of cracks; conversely, residual tensile stress has a certain promoting effect on the generation of cracks. Therefore, controlling the residual compressive stress on the working surface of the roller can improve the fatigue life of the bearing.
[0003] The existing bearing roller processing technology is as follows: turning → soft grinding rolling surface, end surface → turning both ends chamfering → heat treatment → rough grinding rolling surface, end surface → fine grinding rolling surface → fine grinding end surface → fine grinding rolling surface → final grinding rolling surface, super fine grinding rolling surface, wherein the heat treatment can adjust the residual stress of the bearing roller, and mechanical methods can also be used to improve the residual compressive stress of the bearing roller. For example, Chinese patent document CN112276785B uses an ultrasonic grinding device to apply ultrasonic rolling to the surface of the bearing roller, so that the roller obtains a nanostructure layer and a high-value surface residual compressive stress, which can improve the anti-fatigue, anti-wear and anti-corrosion performance of the bearing. Chinese patent document CN111843810B puts the bearing steel ball to be strengthened in the drum, and then puts in grinding powder and nitrogen-rich strengthening grinding modification liquid. Through the complex movement of the bearing steel ball under the action of centrifugal force and gravity in the drum, the surface of the bearing steel ball is processed to have a double-layer composite structure with "surface texture layer, nitrogen-metal complex surface strengthening layer" and residual compressive stress. Although the method provided in the above patent document can increase the residual compressive stress on the surface of the bearing roller, the operation is complicated and the distribution uniformity of the residual compressive stress on the surface is poor, which affects the fatigue life of the bearing. Summary of the invention
[0004] The purpose of the present invention is to provide a processing method for improving the residual compressive stress of the rolling surface of a bearing roller, which can solve the problem that the residual compressive stress on the surface of the processed bearing roller is too small and the distribution uniformity is poor when processing and preparing bearing rollers.
[0005] In order to achieve the above objectives, the technical solution adopted by the processing method of improving the residual compressive stress of the rolling surface of the bearing roller of the present invention is:
[0006] A processing method for improving the residual compressive stress of a bearing roller rolling surface comprises the following steps:
[0007] S1, sequentially quenching, tempering and cold treating the bearing roller blank to obtain a heat-treated part;
[0008] S2, rough grinding the rolling surface and double end surface of the heat-treated part to obtain a rough-ground part;
[0009] S3, tempering the rough ground part, and then semi-finishing the rolling surface and double end surfaces of the tempered rough ground part to obtain a semi-finished part;
[0010] S4, the semi-finished workpiece is subjected to tempering treatment and polishing treatment in sequence, and then the rolling surface and double end surfaces are finely ground to obtain a finely ground workpiece; finally, the rolling surface of the finely ground workpiece is subjected to super-finishing.
[0011] The processing method for improving the residual compressive stress of the rolling surface of the bearing roller of the present invention realizes the gradual improvement of the residual compressive stress of the roller working surface through the progressive processing of each process (specifically, the parameters such as the grinding parameters and heat treatment temperature in each process can be controlled and the additional tempering process can be adjusted), and the residual compressive stress range can be well controlled, which can effectively improve the fatigue life of the bearing. The residual compressive stress on the surface of the bearing roller processed by the present invention is not less than 680MPa, and the residual compressive stress range is not greater than 63MPa.
[0012] In the present invention, the bearing roller blank can be obtained by lathing, for example, the metal blank is lathe-machined to obtain the bearing roller blank. In order to improve the compressive stress generated during lathing, preferably, the cutting speed during lathing is 0.06-0.1 mm / s. For example, the cutting speed during lathing is 0.08 mm / s.
[0013] In the present invention, the material of the bearing roller blank is bearing steel. For example, the material of the bearing roller blank is 8Cr4Mo4V bearing steel.
[0014] Preferably, the quenching temperature in step S1 is 1065-1085°C, and the time is 40-50 min. Preferably, the tempering temperature in step S1 is 535-545°C, and the time is 2-2.5 h. Preferably, the cold treatment temperature in step S1 is -90--75°C, and the time is 2 h-2.5 h. Heat treatment of the bearing roller blank can make the hardness of the heat-treated part reach 60HRC-64HRC, thereby providing a good foundation for subsequent grinding.
[0015] Preferably, the tempering treatment in step S3 is performed at a temperature of 515-525° C. for 4-6 hours. The tempering treatment in step S3 can eliminate the internal stress of the rough ground part and improve the uniformity of the residual stress.
[0016] Preferably, the tempering treatment in step S4 is performed at a temperature of 245-255° C. for 8-10 hours. The tempering treatment in step S4 can eliminate the internal stress of the semi-finished part.
[0017] Preferably, the rough grinding in step S2 is to rough grind the rolling surface and the double end surface of the heat-treated part in sequence; the abrasive of the grinding wheel used for rough grinding of the rolling surface is white corundum abrasive, the particle size is not less than 100 mesh, and the rotation speed of the grinding wheel is 500-600r / min; the abrasive of the grinding wheel used for rough grinding of the double end surface is white corundum abrasive, the particle size is not less than 80 mesh, and the rotation speed of the grinding wheel is 600-700r / min. For example, a through-type grinder is used for rough grinding of the rolling surface, and the grinding wheel used is a WA100PR type grinding wheel, and the rotation speed of the grinding wheel is 560r / min. For example, a double end surface grinder is used for rough grinding of the double end surface, and the grinding wheel used is a WA80MB type grinding wheel, and the rotation speed of the grinding wheel is 640r / min. When rough grinding the rolling surface and double end surface, using specific abrasives and grinding wheel speeds can not only achieve higher processing efficiency, but also ensure that the roughness of the processed rolling surface and double end surface meets the requirements, and can improve the uniformity of the distribution of residual compressive stress to a certain extent.
[0018] In order to improve processing efficiency and reduce processing costs, preferably, the processing method for improving the residual compressive stress of the rolling surface of the bearing roller further includes the following steps: after step S2, the rough ground part is inspected, and if the rough ground part has no defects, the rough ground part is then subjected to subsequent processing. During the inspection, pickling inspection or magnetic particle inspection, or other flaw detection methods can be used to select defective products.
[0019] Preferably, the semi-finishing in step S3 is to semi-finish grinding the rolling surface and semi-finish grinding the double-end surfaces of the rough-ground piece after tempering treatment in sequence; the abrasive of the grinding wheel used for semi-finishing the rolling surface is white corundum abrasive, the particle size is not less than 100 mesh, and the rotation speed of the grinding wheel is 500-600r / min; the abrasive of the grinding wheel used for semi-finishing the double-end surfaces is white corundum abrasive, the particle size is not less than 80 mesh, and the rotation speed of the grinding wheel is 600-700r / min. For example, a through-type grinder is used for semi-finishing the rolling surface, and the grinding wheel used is a WA100PR type grinding wheel, and the rotation speed of the grinding wheel is 560r / min. For example, a double-end surface grinder is used for semi-finishing the double-end surfaces, and the grinding wheel used is a WA80MB type grinding wheel, and the rotation speed of the grinding wheel is 640r / min. When semi-finishing the rolling surface and double end surface, using specific abrasives and grinding wheel speeds can not only achieve higher processing efficiency, but also ensure that the roughness of the processed rolling surface and double end surface is further reduced, and can improve the uniformity of the distribution of residual compressive stress to a certain extent.
[0020] The polishing treatment in step S4 can remove burrs and impurities on the surface of the parts, and exert an effect on the rolling surface through the corundum and the roller, resulting in extruded plastic deformation and increasing the residual compressive stress on the rolling surface. Preferably, the polishing treatment is to rotate and mix the semi-finished parts after tempering with the cross-linking material. In order to improve the effect of the polishing treatment, the cross-linking material includes corundum. In order to make the semi-finished parts and the cross-linking material more evenly contact and mix, the cross-linking material also includes water, the mass ratio of the semi-finished parts, corundum and water is 5: (1~3): 3, the rotation speed of the rotation mixing is 40~45r / min, and the time of the polishing treatment is not less than 2h.
[0021] Preferably, the fine grinding in step S4 includes the following steps: fine grinding the rolling surface for the first time, then fine grinding the double end surfaces for the first time, then fine grinding the double end surfaces for the second time, and finally fine grinding the rolling surface for the second time; the abrasive of the grinding wheel used for the first fine grinding of the rolling surface is green silicon carbide abrasive, the particle size is not less than 120 mesh, and the rotation speed of the grinding wheel is 1000~1200r / min; the abrasive of the grinding wheel used for the first fine grinding of the double end surfaces is white corundum abrasive, the particle size is not less than 100 mesh, and the rotation speed of the grinding wheel is 600~700r / min; the abrasive of the grinding wheel used for the second fine grinding of the double end surfaces is white corundum abrasive, the particle size is not less than 180 mesh; the abrasive of the grinding wheel used for the second fine grinding of the rolling surface is green silicon carbide abrasive, the particle size is not less than 120 mesh, and the rotation speed of the grinding wheel is 1000~1200r / min. For example, when the rolling surface is finely ground for the first time, a through-type grinder is used, the grinding wheel used is a GC120LV type grinding wheel, and the grinding wheel speed is 1100r / min. For example, when the double-end surface is finely ground for the first time, a double-end surface grinder is used, the grinding wheel used is a WA100MB type grinding wheel, and the grinding wheel speed is 640r / min. For example, when the rolling surface is finely ground for the second time, a through-type grinder is used, the grinding wheel used is a GC120LV type grinding wheel, and the grinding wheel speed is 1100r / min.
[0022] Preferably, a double-end surface grinder is used for the second fine grinding of the double end surfaces, the upper disc speed is 40-50 r / min, the lower disc speed is 45-55 r / min, and the lower disc speed is greater than the upper disc speed. For example, a double-end surface grinder is used for the second fine grinding of the double end surfaces, the grinding wheel used is a WA180MB grinding wheel, the upper disc speed is 45 r / min, and the lower disc speed is 50 r / min.
[0023] In order to improve the processing efficiency and at the same time to reduce the roughness of the roller surface and improve the uniformity of the distribution of residual compressive stress on the roller surface, preferably, the total grinding amount for rough grinding of the rolling surface is A1, the total grinding amount for semi-finishing grinding of the rolling surface is B1, the total grinding amount for the first fine grinding of the rolling surface is C1, and the total grinding amount for the second fine grinding of the rolling surface is D1, then A1:B1:C1:D1=(0.1~0.2):(0.02~0.06):(0.06~0.12):(0.02~0.06).
[0024] In order to reduce the roughness of the roller surface, preferably, the number of grinding times when the rolling surface is roughly ground is 2 or more. Preferably, the number of grinding times when the rolling surface is semi-finished ground is 2 or more. Preferably, the number of grinding times when the rolling surface is first finely ground is 3 or more. Preferably, the number of grinding times when the rolling surface is second finely ground is 4 or more.
[0025] Preferably, the number of grindings when rough grinding the double end surfaces is 2 or more. Preferably, the number of grindings when semi-finishing grinding the double end surfaces is 2 or more. Preferably, the number of grindings when first fine grinding the double end surfaces is 3 or more.
[0026] Preferably, the total grinding amount when the rolling surface is rough ground is 0.1-0.2 mm, and the single grinding amount is 0.05-0.1 mm. Preferably, the total grinding amount when the rolling surface is semi-finished ground is 0.02-0.06 mm, and the single grinding amount is 0.01-0.03 mm. Preferably, the total grinding amount when the rolling surface is finely ground for the first time is 0.06-0.12 mm, and the single grinding amount is 0.02-0.04 mm. Preferably, the total grinding amount when the rolling surface is finely ground for the second time is 0.02-0.06 mm, and the single grinding amount is 0.005-0.015 mm.
[0027] Preferably, the total grinding amount when rough grinding the double end surfaces is A2, the total grinding amount when semi-finishing grinding the double end surfaces is B2, the total grinding amount when the first fine grinding of the double end surfaces is C2, and the total grinding amount when the second fine grinding of the double end surfaces is D2, then A2:B2:C2:D2=(0.06~0.1):(0.04~0.08):(0.06~0.12):(0.01~0.02).
[0028] Preferably, the total grinding amount when the double end faces are rough ground is 0.06-0.1 mm, and the single grinding amount is 0.03-0.05 mm. Preferably, the total grinding amount when the double end faces are semi-finished ground is 0.04-0.08 mm, and the single grinding amount is 0.02-0.04 mm. Preferably, the total grinding amount when the double end faces are finely ground for the first time is 0.06-0.12 mm, and the single grinding amount is 0.02-0.04 mm. Preferably, the total grinding amount when the double end faces are finely ground for the second time is 0.01-0.02 mm. For example, the total grinding amount when the double end faces are finely ground for the second time is 0.015 mm.
[0029] Preferably, the superfinishing is to perform superfinishing on the rolling surface of the fine grinding piece n times, and each time the superfinishing is performed, the oilstone pressure is independently 0.15-0.6MPa, the oilstone oscillation frequency is independently 250-600 times / min, and the workpiece speed is independently 100-300r / min; n≥2, the opening distance is independently 0.55-0.65 times the diameter of the fine grinding piece; the machining allowance of superfinishing is 0.005-0.010mm. In order to improve efficiency, n=3, and in order to improve the superfinishing effect, a through-type superfinishing machine is used, for example, a five-station through-type superfinishing machine is used. Superfinishing can finely adjust the size of the rolling surface and further reduce the roughness of the rolling surface. The number of superfinishing treatments and the end point of superfinishing can be determined according to whether the size and shape of the product meet the requirements. Too large or too small an opening distance will affect the machining quality of the roller. DETAILED DESCRIPTION
[0030] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0031] Example 1
[0032] The processing method for improving the residual compressive stress of the rolling surface of the bearing roller of this embodiment specifically comprises the following steps:
[0033] (1) According to the process requirements of cylindrical roller products, a CNC lathe is used to turn a heat-resistant steel bar (the material of the heat-resistant steel bar is 8Cr4Mo4V bearing steel). After turning and forming, a bearing roller blank is obtained; the cutting speed during turning is 0.08 mm / s;
[0034] (2) The bearing roller blank is heat treated to obtain a heat-treated part; the heat treatment is to quench, temper and cold-treat the bearing roller blank in sequence; wherein the quenching temperature is 1065°C, the time is 40 min, the cooling rate of quenching is 120°C / min, and the coolant used is quenching oil; the tempering temperature is 535°C, the time is 2 h, the cooling rate after tempering is 20°C / min, and the coolant used is air; the cold treatment temperature is -90°C, the time is 2 h, and the cold treatment is carried out in a freezer;
[0035] (3) The rolling surface and double end surfaces of the heat-treated part are coarsely ground in sequence to obtain a coarsely ground part; a through-type grinder is used for coarse grinding of the rolling surface, the grinding wheel used is a WA100PR type grinding wheel, the rotation speed of the grinding wheel is 560 r / min, the total grinding amount for coarse grinding of the rolling surface is 0.15 mm, and the single grinding amount is 0.075 mm; a double end surface grinder is used for coarse grinding of the double end surfaces, the grinding wheel used is a WA80MB type grinding wheel, the rotation speed of the grinding wheel is 640 r / min, the total grinding amount for coarse grinding of the double end surfaces is 0.08 mm, and the single grinding amount is 0.04 mm;
[0036] (4) Use magnetic particle inspection to inspect the rough-ground parts and select the rough-ground parts without cracks and other defects for subsequent processing;
[0037] (5) The rough-ground workpiece is tempered, and then the rough-ground workpiece after the tempering treatment is semi-finished on the rolling surface and semi-finished on the double-end surfaces in turn to obtain a semi-finished workpiece; wherein the tempering temperature is 515°C, the time is 4h, the cooling rate after tempering is 20°C / min, and the coolant used is air; when the rolling surface is semi-finished, a through-type grinder is used, the grinding wheel used is a WA100PR grinding wheel, the rotation speed of the grinding wheel is 560r / min, the total grinding amount when the rolling surface is semi-finished is 0.04mm, and the single grinding amount is 0.02mm; when the double-end surfaces are semi-finished, a double-end surface grinder is used, the grinding wheel used is a WA80MB grinding wheel, the rotation speed of the grinding wheel is 640r / min, the total grinding amount when the double-end surfaces are semi-finished is 0.06mm, and the single grinding amount is 0.03mm;
[0038] (6) The semi-finished workpiece is subjected to tempering treatment and polishing treatment in sequence, and then the rolling surface is subjected to the first fine grinding, and then the double end surfaces are subjected to the first fine grinding, and then the double end surfaces are subjected to the second fine grinding, and then the rolling surface is subjected to the second fine grinding to obtain a finely ground workpiece; finally, the rolling surface of the finely ground workpiece is subjected to super-finishing to obtain a bearing roller;
[0039] The tempering temperature is 245℃, the time is 8h, the cooling rate after tempering is 20℃ / min, and the coolant is air; the blasting treatment is to rotate and mix the semi-finished parts after tempering with the blasting material in a blasting barrel. During the blasting treatment, the blasting barrel is tilted at 45°, the rotation speed of the rotation mixing is 45r / min, the blasting treatment time is 2h, the blasting material is composed of water and corundum, and the mass ratio of the semi-finished parts, corundum and water is 5:1:3;
[0040] When the rolling surface is finely ground for the first time, a through-type grinder is used, the grinding wheel used is a GC120LV grinding wheel, the rotation speed of the grinding wheel is 1100r / min, the total grinding amount of the rolling surface is 0.09mm, and the single grinding amount is 0.03mm; when the double end faces are finely ground for the first time, a double end face grinder is used, the grinding wheel used is a WA100MB grinding wheel, the rotation speed of the grinding wheel is 640r / min, the total grinding amount of the double end faces is 0.09mm, and the single grinding amount is 0.03mm; The double-end surface vertical grinder was used for the second fine grinding of the double-end surface, the grinding wheel used was WA180MB type grinding wheel, the upper plate speed was 45r / min, the lower plate speed was 50r / min, and the total grinding amount for the second fine grinding of the double-end surface was 0.015mm; the through-type grinder was used for the second fine grinding of the rolling surface, the grinding wheel used was GC120LV type grinding wheel, the grinding wheel speed was 1100r / min, the total grinding amount for the second fine grinding of the rolling surface was 0.04mm, and the single grinding amount was 0.01mm;
[0041] Super finishing is to use a five-station through-type super finishing machine to perform super finishing treatment three times on the rolling surface of the fine grinding part. During each super finishing treatment, the oil stone pressure is 0.15MPa, the oil stone oscillation frequency is 250 times / min, the workpiece speed is 100r / min, the opening distance is 0.55 times the diameter of the fine grinding part, and the super finishing machining allowance is 0.010mm.
[0042] Example 2
[0043] The processing method for improving the residual compressive stress of the rolling surface of the bearing roller of this embodiment specifically comprises the following steps:
[0044] (1) According to the process requirements of cylindrical roller products, a CNC lathe is used to turn a heat-resistant steel bar (the material of the heat-resistant steel bar is 8Cr4Mo4V bearing steel). After turning and forming, a bearing roller blank is obtained; the cutting speed during turning is 0.06 mm / s;
[0045] (2) The bearing roller blank is heat treated to obtain a heat-treated part; the heat treatment is to quench, temper and cold-treat the bearing roller blank in sequence; wherein the quenching temperature is 1085°C, the time is 50 min, the cooling rate of quenching is 120°C / min, and the coolant used is quenching oil; the tempering temperature is 545°C, the time is 2.5 h, the cooling rate after tempering is 20°C / min, and the coolant used is air; the cold treatment temperature is -75°C, the time is 2.5 h, and the cold treatment is carried out in a freezer;
[0046] (3) The rolling surface and double end surfaces of the heat-treated part are rough-ground in sequence to obtain a rough-ground part; a through-type grinder is used for rough grinding of the rolling surface, the grinding wheel used is a WA100PR type grinding wheel, the rotation speed of the grinding wheel is 500 r / min, the total grinding amount for rough grinding of the rolling surface is 0.2 mm, and the single grinding amount is 0.1 mm; a double end surface grinder is used for rough grinding of the double end surfaces, the grinding wheel used is a WA80MB type grinding wheel, the rotation speed of the grinding wheel is 600 r / min, the total grinding amount for rough grinding of the double end surfaces is 0.1 mm, and the single grinding amount is 0.05 mm;
[0047] (4) Use magnetic particle inspection to inspect the rough-ground parts and select the rough-ground parts without cracks and other defects for subsequent processing;
[0048] (5) The rough-ground workpiece is tempered, and then the rough-ground workpiece after the tempering treatment is semi-finished on the rolling surface and semi-finished on the double-end surfaces in turn to obtain a semi-finished workpiece; wherein the tempering temperature is 525°C, the time is 6 hours, the cooling rate after tempering is 20°C / min, and the coolant used is air; when the rolling surface is semi-finished, a through-type grinder is used, the grinding wheel used is a WA100PR grinding wheel, the rotation speed of the grinding wheel is 500r / min, the total grinding amount when the rolling surface is semi-finished is 0.06mm, and the single grinding amount does not exceed 0.03mm; when the double-end surfaces are semi-finished, a double-end surface grinder is used, the grinding wheel used is a WA80MB grinding wheel, the rotation speed of the grinding wheel is 600r / min, the total grinding amount when the double-end surfaces are semi-finished is 0.08mm, and the single grinding amount is 0.04mm;
[0049] (6) The semi-finished workpiece is subjected to tempering treatment and polishing treatment in sequence, and then the rolling surface is subjected to the first fine grinding, and then the double end surfaces are subjected to the first fine grinding, and then the double end surfaces are subjected to the second fine grinding, and then the rolling surface is subjected to the second fine grinding to obtain a finely ground workpiece; finally, the rolling surface of the finely ground workpiece is subjected to super-finishing to obtain a bearing roller;
[0050] The tempering temperature is 255℃, the time is 10h, the cooling rate after tempering is 20℃ / min, and the coolant is air; the blasting treatment is to rotate and mix the semi-finished parts after tempering with the blasting material in a blasting barrel. During the blasting treatment, the blasting barrel is tilted at 45°, the rotation speed of the mixing is 45r / min, the blasting treatment time is 2h, the blasting material is composed of water and corundum, and the mass ratio of the semi-finished parts, corundum and water is 5:2:3;
[0051] The first fine grinding of the rolling surface was performed using a through-type grinder, the grinding wheel used was a GC120LV grinding wheel, the rotation speed of the grinding wheel was 1000r / min, the total grinding amount for the first fine grinding of the rolling surface was 0.12mm, and the single grinding amount was 0.04mm; the first fine grinding of the double-end faces was performed using a double-end face grinder, the grinding wheel used was a WA100MB grinding wheel, the rotation speed of the grinding wheel was 600r / min, the total grinding amount for the first fine grinding of the double-end faces was 0.12mm, and the single grinding amount was 0.04mm; The double-end surface was finely ground for the second time using a double-end surface vertical grinder, the grinding wheel used was a WA180MB grinding wheel, the upper plate speed was 40r / min, the lower plate speed was 45r / min, and the total grinding amount for the second fine grinding of the double-end surface was 0.015mm; the second fine grinding of the rolling surface was done using a through-type grinder, the grinding wheel used was a GC120LV grinding wheel, the grinding wheel speed was 1000r / min, the total grinding amount for the second fine grinding of the rolling surface was 0.06mm, and the single grinding amount was 0.015mm;
[0052] Super finishing is to use a five-station through-type super finishing machine to perform super finishing treatment three times on the rolling surface of the fine grinding part. During each super finishing treatment, the oilstone pressure is 0.6MPa, the oilstone oscillation frequency is 600 times / min, the workpiece speed is 300r / min, the opening distance is 0.65 times the diameter of the fine grinding part, and the super finishing machining allowance is 0.008mm.
[0053] Example 3
[0054] The processing method for improving the residual compressive stress of the rolling surface of the bearing roller of this embodiment specifically comprises the following steps:
[0055] (1) According to the process requirements of cylindrical roller products, a CNC lathe is used to turn a heat-resistant steel bar (the material of the heat-resistant steel bar is 8Cr4Mo4V bearing steel). After turning and forming, a bearing roller blank is obtained; the cutting speed during turning is 0.1 mm / s;
[0056] (2) The bearing roller blank is heat treated to obtain a heat-treated part; the heat treatment is to quench, temper and cold-treat the bearing roller blank in sequence; wherein the quenching temperature is 1075°C, the time is 45 minutes, the cooling rate of the quenching is 120°C / min, and the coolant used is quenching oil; the tempering temperature is 540°C, the time is 2.2 hours, the cooling rate after tempering is 20°C / min, and the coolant used is air; the cold treatment temperature is -80°C, the time is 2.2 hours, and the cold treatment is carried out in a freezer;
[0057] (3) The rolling surface and double end surfaces of the heat-treated part are rough-ground in sequence to obtain a rough-ground part; a through-type grinder is used for rough grinding of the rolling surface, the grinding wheel used is a WA100PR grinding wheel, the rotation speed of the grinding wheel is 600 r / min, the total grinding amount for rough grinding of the rolling surface is 0.1 mm, and the single grinding amount is 0.05 mm; a double end surface grinder is used for rough grinding of the double end surfaces, the grinding wheel used is a WA80MB grinding wheel, the rotation speed of the grinding wheel is 700 r / min, the total grinding amount for rough grinding of the double end surfaces is 0.06 mm, and the single grinding amount is 0.03 mm;
[0058] (4) Use magnetic particle inspection to inspect the rough-ground parts and select the rough-ground parts without cracks and other defects for subsequent processing;
[0059] (5) The rough-ground workpiece is tempered, and then the rough-ground workpiece after the tempering treatment is semi-finished on the rolling surface and semi-finished on the double-end surfaces in turn to obtain a semi-finished workpiece; wherein the tempering temperature is 520°C, the time is 5h, the cooling rate after tempering is 20°C / min, and the coolant used is air; a through-type grinder is used for semi-finishing the rolling surface, the grinding wheel used is a WA100PR grinding wheel, the rotation speed of the grinding wheel is 600r / min, the total grinding amount for semi-finishing the rolling surface is 0.02mm, and the single grinding amount is 0.01mm; a double-end surface grinder is used for semi-finishing the double-end surfaces, the grinding wheel used is a WA80MB grinding wheel, the rotation speed of the grinding wheel is 700r / min, the total grinding amount for semi-finishing the double-end surfaces is 0.04mm, and the single grinding amount is 0.02mm;
[0060] (6) The semi-finished workpiece is subjected to tempering treatment and polishing treatment in sequence, and then the rolling surface is subjected to the first fine grinding, and then the double end surfaces are subjected to the first fine grinding, and then the double end surfaces are subjected to the second fine grinding, and then the rolling surface is subjected to the second fine grinding to obtain a finely ground workpiece; finally, the rolling surface of the finely ground workpiece is subjected to super-finishing to obtain a bearing roller;
[0061] The tempering temperature is 250℃, the time is 9h, the cooling rate after tempering is 20℃ / min, and the coolant is air; the blasting treatment is to rotate and mix the semi-finished parts after tempering with the blasting material in a blasting barrel. During the blasting treatment, the blasting barrel is tilted at 45°, the rotation speed of the rotation mixing is 45r / min, the blasting treatment time is 2h, the blasting material is composed of water and corundum, and the mass ratio of the semi-finished parts, corundum and water is 5:3:3;
[0062] The first fine grinding of the rolling surface was performed using a through-type grinder, the grinding wheel used was a GC120LV grinding wheel, the rotation speed of the grinding wheel was 1200r / min, the total grinding amount for the first fine grinding of the rolling surface was 0.06mm, and the single grinding amount was 0.02mm; the first fine grinding of the double-end faces was performed using a double-end face grinder, the grinding wheel used was a WA100MB grinding wheel, the rotation speed of the grinding wheel was 700r / min, the total grinding amount for the first fine grinding of the double-end faces was 0.06mm, and the single grinding amount was 0.02mm; The double-end surface was finely ground for the second time using a double-end surface vertical grinder, the grinding wheel used was a WA180MB grinding wheel, the upper plate speed was 50r / min, the lower plate speed was 55r / min, and the total grinding amount for the second fine grinding of the double-end surface was 0.015mm; the second fine grinding of the rolling surface was done using a through-type grinder, the grinding wheel used was a GC120LV grinding wheel, the grinding wheel speed was 1200r / min, the total grinding amount for the second fine grinding of the rolling surface was 0.02mm, and the single grinding amount was 0.005mm;
[0063] Super finishing is to use a five-station through-type super finishing machine to perform super finishing treatment three times on the rolling surface of the fine grinding part. During each super finishing treatment, the oil stone pressure is 0.3MPa, the oil stone oscillation frequency is 400 times / min, the workpiece speed is 200r / min, the opening distance is 0.6 times the diameter of the fine grinding part, and the super finishing machining allowance is 0.005mm.
[0064] Comparative Example 1
[0065] The difference between the processing method for improving the residual compressive stress of the rolling surface of the bearing roller of this comparative example and the processing method for improving the residual compressive stress of the rolling surface of the bearing roller of Example 1 is only that in step (2) of the processing method for improving the residual compressive stress of the rolling surface of the bearing roller of this comparative example, cold treatment is first performed after quenching and then tempering is performed, that is, the order of cold treatment and tempering in step (2) is reversed.
[0066] Comparative Example 2
[0067] The difference between the processing method for improving the residual compressive stress of the rolling surface of the bearing roller of this comparative example and the processing method for improving the residual compressive stress of the rolling surface of the bearing roller of Example 1 is only that the quenching temperature in step (2) of the processing method for improving the residual compressive stress of the rolling surface of the bearing roller of this comparative example is 1035°C.
[0068] Comparative Example 3
[0069] The difference between the processing method for improving the residual compressive stress of the rolling surface of the bearing roller of this comparative example and the processing method for improving the residual compressive stress of the rolling surface of the bearing roller of Example 1 is that, in the processing method for improving the residual compressive stress of the rolling surface of the bearing roller of this comparative example, the tempering treatment in step (5) is omitted, and the tempering treatment in step (6) is adjusted to a secondary tempering treatment, wherein the first tempering treatment is the same as the tempering treatment in step (5) of Example 1, and the second tempering treatment is the same as the tempering treatment in step (6) of Example 1.
[0070] Experimental example
[0071] In order to evaluate the residual compressive stress of bearing rollers prepared by different processing methods, the residual compressive stress of the working surface (rolling surface) of the bearing rollers prepared by Examples 1-3 and Comparative Examples 1-3 was tested in the same way (the number of bearing rollers processed by different processing methods was 20), and then the residual compressive stress range was calculated. The results are shown in Table 1. The "-" sign in the residual compressive stress value in Table 1 only represents the residual compressive stress. Among them, the test method of residual compressive stress is carried out in accordance with GB / T 7704 "Non-destructive Testing X-ray Stress Determination Method", and the residual compressive stress range is equal to the difference between the maximum and minimum values of the residual compressive stress tested on the same sample. The residual compressive stress in Table 1 represents the minimum value of the residual compressive stress of 20 bearing rollers processed by different processing methods.
[0072] Table 1 Residual compressive stress and residual compressive stress range of bearing rollers prepared by different processing methods
[0073]
Claims
1. A processing method for improving the residual compressive stress of the rolling surface of a bearing roller, characterized in that: The following steps are involved: S1, quenching, tempering and cold treating the bearing roller blank in sequence to obtain a heat-treated part; the quenching temperature in step S1 is 1065-1085°C, the time is 40-50min, the tempering temperature is 535-545°C, the time is 2-2.5h, and the cold treatment temperature is -90--75°C, the time is 2h-2.5h; the bearing roller blank is made of 8Cr4Mo4V bearing steel; S2, rough grinding the rolling surface and double end surface of the heat-treated part to obtain a rough-ground part; S3, tempering the rough ground part, and then semi-finishing the rolling surface and double end surface of the rough ground part after tempering to obtain a semi-finished part; the tempering temperature in step S3 is 515-525°C, and the time is 4-6h; S4, the semi-finished workpiece is subjected to tempering treatment and polishing treatment in sequence, and then the rolling surface and double-end surface are finely ground to obtain a finely ground workpiece; finally, the rolling surface of the finely ground workpiece is super-finished; the tempering treatment temperature in step S4 is 245~255℃, and the time is 8~10h.
2. The processing method for improving the residual compressive stress of the rolling surface of a bearing roller according to claim 1, characterized in that: The rough grinding in step S2 is to rough grind the rolling surface and the double end surfaces of the heat-treated part in sequence; the abrasive of the grinding wheel used for the rough grinding of the rolling surface is white corundum abrasive, the particle size is not less than 100 mesh, and the rotation speed of the grinding wheel is 500~600r / min; the abrasive of the grinding wheel used for the rough grinding of the double end surfaces is white corundum abrasive, the particle size is not less than 80 mesh, and the rotation speed of the grinding wheel is 600~700r / min.
3. The processing method for improving the residual compressive stress of the rolling surface of a bearing roller according to claim 1, characterized in that: The semi-finishing in step S3 is to semi-finish grinding the rolling surface and semi-finish grinding the double end surfaces of the rough-ground workpiece after tempering in sequence; the abrasive of the grinding wheel used for semi-finishing the rolling surface is white corundum abrasive, the particle size is not less than 100 mesh, and the rotation speed of the grinding wheel is 500~600r / min; the abrasive of the grinding wheel used for semi-finishing the double end surfaces is white corundum abrasive, the particle size is not less than 80 mesh, and the rotation speed of the grinding wheel is 600~700r / min.
4. The processing method for improving the residual compressive stress of the rolling surface of a bearing roller according to claim 1, characterized in that: The fine grinding in step S4 includes the following steps: fine grinding the rolling surface for the first time, then fine grinding the double end surfaces for the first time, then fine grinding the double end surfaces for the second time, and finally fine grinding the rolling surface for the second time; the abrasive of the grinding wheel used for the first fine grinding of the rolling surface is green silicon carbide abrasive, the particle size is not less than 120 mesh, and the rotation speed of the grinding wheel is 1000~1200r / min; the abrasive of the grinding wheel used for the first fine grinding of the double end surfaces is white corundum abrasive, the particle size is not less than 100 mesh, and the rotation speed of the grinding wheel is 600~700r / min; the abrasive of the grinding wheel used for the second fine grinding of the double end surfaces is white corundum abrasive, the particle size is not less than 180 mesh; the abrasive of the grinding wheel used for the second fine grinding of the rolling surface is green silicon carbide abrasive, the particle size is not less than 120 mesh, and the rotation speed of the grinding wheel is 1000~1200r / min.
5. The processing method for improving the residual compressive stress of the rolling surface of a bearing roller according to claim 1, characterized in that: The super finishing is to perform super finishing on the rolling surface of the fine grinding piece n times, and during each super finishing, the oilstone pressure is independently 0.15-0.6MPa, the oilstone oscillation frequency is independently 250-600 times / min, and the workpiece rotation speed is independently 100-300r / min; n≥2.