A method for preparing a self-assembled graphite sheet thin film and its application.
By employing the self-assembly technology of graphite sheets and ethanol mixture at the gas-liquid interface, the problem of graphite films being unable to be transferred on substrates has been solved, enabling the preparation and transfer of large-area uniform films and expanding their application range.
Patent Information
- Application Number
- CN202410467597.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-18
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-04-18
AI Technical Summary
Existing graphite films cannot be transferred when grown directly on a substrate, and the preparation of multilayer graphite films requires repeated processes, which limits their applications.
The self-assembly technology of graphite sheets and ethanol mixture at the gas-liquid interface is adopted. The surface tension is used to automatically assemble the graphite sheets into a uniform thin film, which can be transferred to other substrates.
The fabrication and transfer of large-area uniform graphite films have been achieved, expanding their applications in electronic devices, sensors, flexible electronics, and heat dissipation.
Smart Images

Figure CN118359192B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials preparation technology, and particularly relates to a method for preparing and applying a self-assembled graphite sheet thin film. Background Technology
[0002] Graphite is a typical conductive material because the weak interactions between the graphite layers in a graphite film allow electrons to conduct freely between them. Graphite film materials have broad application prospects in electronic devices, sensors, and flexible electronics. Furthermore, graphite film materials exhibit excellent thermal conductivity. The graphite layers in a graphite film form good heat conduction channels, making graphite's thermal conductivity better than that of typical polymer materials. Graphite film materials have broad application potential in thermal management and heat dissipation. Graphite films can serve as thermal interface materials, transferring heat to heat sinks and improving the heat dissipation efficiency of devices. Graphite film materials also possess excellent mechanical properties. The low bonding strength between graphite layers gives graphite films good tensile strength. Graphite films can be prepared in various forms, such as thin films, nanowires, and nanosheets, to meet the needs of different applications.
[0003] Currently, there are two main methods for preparing large-area graphene thin films: one is to spin-coat graphene powder onto a target substrate using thin film preparation processes such as spin coating. This method is low-cost, simple, and efficient, producing large-area films, but the resulting films are non-uniform and discontinuous in the two-dimensional direction. The other method is direct growth on a metal substrate using chemical vapor deposition (CVD). The biggest advantage of CVD-prepared graphene films is their good lateral continuity and high quality, but the process is more complex. Furthermore, both methods involve direct growth on the substrate, making film transfer impossible. Preparing multilayer graphene films requires repeated processes, significantly limiting their applications. Summary of the Invention
[0004] The purpose of this invention is to solve the problem that existing graphite films are grown directly on substrates and cannot be transferred, and that the preparation of multilayer graphite films requires repeated processes, which greatly limits the application of graphite films.
[0005] To achieve the above objectives, the present invention provides a method for preparing a graphite self-assembled thin film, comprising the following steps:
[0006] Step 1: Mix 0.1g of graphite sheet with 5ml of ethanol and sonicate to obtain a uniformly dispersed graphite sheet-ethanol mixture.
[0007] Step 2: Clean the glass slides using ethanol, deionized water, and an plasma cleaner;
[0008] Step 3: Cover the clean glass slide with a film of water;
[0009] Step 4: Slowly inject 100 μl of the graphite sheet-ethanol mixture prepared in Step 1 into one corner of the glass slide in Step 3, and let it stand for 20 minutes to obtain a graphite sheet film.
[0010] Furthermore, in step 1, the graphite flakes are black powder with a diameter of 3–5 μm.
[0011] Furthermore, the thickness of the graphite sheet self-assembled film obtained in step 4 is 860 nm.
[0012] A method for transferring a self-assembled graphite film onto a silicon wafer or flexible PI includes the following steps:
[0013] Step 1: Prepare a graphite sheet film using the method for preparing a self-assembled graphite sheet film according to claim 1;
[0014] Step 2: Prepare a beaker filled with deionized water;
[0015] Step 3: Use absorbent filter paper to remove the water under the graphite film prepared in step 1, and then slowly immerse the glass slide covered with the graphite film horizontally into the water surface of the beaker in step 2.
[0016] Step 4: Wait for the graphite film to completely transfer to the water surface, then release the glass slide to let it sink to the bottom of the beaker;
[0017] Step 5: Use a silicon wafer or flexible PI to retrieve the graphite film and uniformly cover the substrate surface with the graphite film.
[0018] Furthermore, in step 3, when the water under the graphite film prepared in step 1 is removed using absorbent filter paper, the graphite film cannot be completely dried.
[0019] Beneficial effects:
[0020] This invention proposes using graphite flake powder as raw material and employing gas-liquid interface self-assembly technology. When a mixture of graphite flakes and anhydrous ethanol is slowly injected onto a glass slide covered with a water film, the ethanol carries the graphite flakes towards the gas-liquid interface. Driven by surface tension, the graphite flakes automatically align. As the dispersion is gradually injected, the automatically aligned graphite flakes gradually move and cover the surface of the water film, forming a complete graphite flake film. The film prepared by this technology exhibits good uniformity, can be fabricated over large areas, and has the advantage of being transferable to other substrates, while also possessing good electrical conductivity. This method can greatly expand the application of graphite thin films in electronic devices, sensors, flexible electronics, and heat dissipation. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of the preparation method of the graphite sheet self-assembled thin film provided by the present invention;
[0022] Figure 2 A photograph of the prepared graphite sheet self-assembled thin film at the interface;
[0023] Figure 3 Field emission scanning electron microscope image of the prepared large-area graphite sheet self-assembled thin film;
[0024] Figure 4 A magnified field emission scanning electron microscope image of the prepared graphite sheet self-assembled thin film;
[0025] Figure 5 The thickness distribution of the prepared graphite sheet self-assembled thin film, as measured by a profilometer;
[0026] Figure 6 This is a physical image of the self-assembled graphite sheet film transferred to a silicon wafer substrate.
[0027] Figure 7 This is a photograph of the prepared graphite sheet self-assembled thin film transferred to a flexible PI substrate.
[0028] Figure 8 Partitioning of self-assembled graphite thin films for resistance measurement;
[0029] Figure 9 The resistance histogram of the measured partitioned graphite self-assembled thin film;
[0030] Figure 10 A photograph of a graphite sheet self-assembled film at the interface prepared using a graphite sheet suspension of 0.5g graphite sheet and 5ml ethanol.
[0031] Figure 11 This is a photograph of a graphite sheet self-assembled film at the interface prepared using a graphite sheet suspension containing 0.01g of graphite sheet and 5ml of ethanol. Detailed Implementation
[0032] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0033] The application principle of the present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0034] Example 1:
[0035] like Figure 1 As shown, a method for preparing a self-assembled graphite sheet thin film includes the following specific steps:
[0036] Step 1: Mix 0.1g of graphite sheet with 5ml of ethanol and sonicate to obtain a uniformly dispersed graphite sheet-ethanol mixture.
[0037] Step 2: Clean the glass slides using ethanol, deionized water, and an plasma cleaner.
[0038] Step 3: Cover the clean glass slide with a film of water.
[0039] Step 4: Slowly inject 100 μl of the graphite sheet-ethanol mixture prepared in Step 1 into one corner of the glass slide in Step 3, and let it stand for 20 minutes to obtain a graphite sheet film. The diameter of the prepared graphite sheet is 3-5 μm.
[0040] Figure 2 The self-assembled graphite film shown exhibits a large area of uniform light gray color, and this uniformity reflects the good uniformity of the film. Figure 3 , Figure 4 As shown, the graphite sheet film after the experiment was observed under a scanning electron microscope, and a micron-sized image of the structure was obtained. Figure 3 The prepared graphite sheet self-assembled film exhibits good uniformity over a large area. The thickness of the graphite sheet film was measured and analyzed using a profilometer. Figure 5 The prepared graphite sheet self-assembled film has a thickness of approximately 860 nm, good uniformity, and a relative standard deviation as low as 3.05%.
[0041] In this invention, the main factor affecting the uniformity of the graphite film is the mass of the graphite sheets in the graphite-ethanol mixture. Through a series of experiments, the optimal mass of graphite was determined to be 0.1 g (5 ml of ethanol). These experiments demonstrate that graphite self-assembled films prepared with a concentration range of 0.1 g exhibit good uniformity; concentrations that are too high or too low will cause defects in the film.
[0042] Example 2:
[0043] The graphite sheet self-assembled thin film prepared by this invention can be transferred to other substrates, such as silicon wafers and flexible polyimide (PI) substrates. The transfer of the graphite thin film mainly includes the following steps:
[0044] Step 1: Prepare graphite sheet film according to the method for preparing graphite film in Example 1.
[0045] Step 2: Prepare a beaker filled with deionized water.
[0046] Step 3: Use absorbent filter paper to remove the water under the graphite film prepared in Step 1 (Note: do not dry it completely). Then, slowly immerse the glass slide covered with the graphite film horizontally into the water surface of the beaker in Step 2.
[0047] Step 4: Wait for the graphite film to completely transfer to the water surface, then release the glass slide to let it sink to the bottom of the beaker.
[0048] Step 5: Use a silicon wafer or flexible PI to retrieve the graphite film and uniformly cover the substrate surface with the graphite film.
[0049] like Figure 6 The diagram shows a silicon wafer used as the substrate for a graphite sheet self-assembled thin film. The graphite sheet self-assembled thin film has a large area on the silicon wafer substrate and exhibits a uniform gray film. For example... Figure 7 As shown, using flexible PI as the substrate for graphite sheet self-assembled films, a uniform gray film still appears on the flexible PI substrate. The experiments demonstrating that silicon wafers and flexible PI can be used as graphite sheet films show that graphite sheet self-assembled films have the advantage of being transferable to other substrates.
[0050] Example 3:
[0051] It has the same implementation content as Embodiment 1 described above. For specific implementation details of the above embodiments, please refer to the above description; the embodiments described here will not be repeated in detail. However, the difference between this embodiment and the above embodiments lies in:
[0052] No treatment is performed on the slide in step 4.
[0053] Preparation of ordinary glass slides as Figure 8 The diagram shows a partition of a self-assembled graphite film used for resistance measurement. The resistance of the self-assembled graphite film in each partition was measured using a multimeter. Figure 9 The image shows the measured resistance histogram of the partitioned graphite self-assembled film. Ordinary glass slides are completely non-conductive, making resistance unmeasurable. However, when a layer of graphite self-assembled film is coated onto its surface, the slide exhibits good conductivity. Furthermore, there is no significant difference in resistance between regions, with a relative standard deviation as low as 4.48%, indicating good uniformity of the graphite self-assembled film.
[0054] Comparative Example 1:
[0055] It has the same implementation content as Embodiment 1 described above. For specific implementation details of the above embodiments, please refer to the above description; the embodiments described here will not be repeated in detail. However, the difference between this embodiment and the above embodiments lies in:
[0056] Step 1: A graphite sheet self-assembled film at the interface is prepared using a graphite sheet suspension containing 0.5g of graphite sheets.
[0057] like Figure 10 As shown, the graphite film is unevenly distributed on the glass slide using the above method, and there is obvious breakage.
[0058] Comparative Example 2:
[0059] It has the same implementation content as Embodiment 2 described above. For specific implementation details of the above embodiments, please refer to the above description; the embodiments described here will not be repeated in detail. However, the difference between this application's embodiment and the above embodiments lies in:
[0060] Step 1: A graphite sheet self-assembled film at the interface is prepared using a graphite sheet suspension containing 0.01g of graphite sheets.
[0061] like Figure 11 As shown, the graphite film prepared by the above method exhibits a small-area blocky distribution, and the graphite sheets show local aggregation or uneven distribution.
[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a self-assembled graphite sheet thin film, characterized in that, Includes the following steps: Step 1: Mix 0.1g of black powder graphite sheet with a diameter of 3~5μm with 5ml of ethanol and sonicate to obtain a uniformly dispersed graphite sheet ethanol mixture. Step 2: Clean the glass slides using ethanol, deionized water, and an plasma cleaner; Step 3: Cover the clean glass slide with a film of water; Step 4: Slowly inject 100 μl of the graphite sheet-ethanol mixture prepared in Step 1 into one corner of the glass slide in Step 3, and let it stand for 20 minutes to obtain a graphite sheet film.
2. The method for preparing a self-assembled graphite sheet thin film according to claim 1, characterized in that, The thickness of the self-assembled graphite film obtained in step 4 is 860 nm.
3. A method for transferring a self-assembled graphite thin film onto a silicon wafer or flexible PI, characterized in that, Includes the following steps: Step 1: Prepare a graphite sheet film using the method for preparing a self-assembled graphite sheet film according to claim 1; Step 2: Prepare a beaker filled with deionized water; Step 3: Use absorbent filter paper to remove the water under the graphite film prepared in step 1, and then slowly immerse the glass slide covered with the graphite film horizontally into the water surface of the beaker in step 2. Step 4: Wait for the graphite film to completely transfer to the water surface, then release the glass slide to let it sink to the bottom of the beaker; Step 5: Use a silicon wafer or flexible PI to retrieve the graphite film and uniformly cover the substrate surface with the graphite film.
4. The method for transferring graphite self-assembled thin films to silicon wafers or flexible PI according to claim 3, characterized in that, In step 3, when the water under the graphite film prepared in step 1 is removed using absorbent filter paper, the graphite film cannot be completely dried.
Citation Information
Patent Citations
Self-assembly graphene nanometer thin film and preparing method and application thereof