Hollow porous composite sodium iron pyrophosphate positive electrode material and preparation method thereof, positive electrode and sodium ion battery
By adopting the preparation method of hollow porous composite sodium iron pyrophosphate cathode material in sodium-ion batteries, and using hydrothermal method and microemulsion method to construct a core-shell structure, the problems of low-voltage gas evolution and high-voltage Fe3+ dissolution in sodium-ion batteries are solved. problem, improving the cycle life and electrochemical performance of the battery.
Patent Information
- Application Number
- CN202410827998.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-06-25
AI Technical Summary
Sodium-ion batteries have problems with low-voltage gas evolution and high-voltage Fe3+ dissolution, which lead to capacity attenuation of the positive electrode material and deposition of transition metal ions on the negative electrode surface, affecting the cycle life of the battery.
A hollow porous composite sodium iron pyrophosphate cathode material is prepared by hydrothermal method to generate a sodium iron pyrophosphate coating layer on the surface of carbon-based particles, which is then sintered in an oxygen environment to form a porous structure of sodium manganese iron nickel layered oxidation. materials, using microemulsion method to construct spherical templates to improve electrochemical performance.
The high-voltage Fe3+ dissolution phenomenon is reduced, the voltage range is broadened, the low-voltage gas production is reduced, the specific surface area and electrochemical performance of the cathode material are improved, and the cycle life of the battery is extended.
Smart Images

Figure CN118373401B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of battery material preparation, and in particular to a hollow porous composite sodium iron pyrophosphate positive electrode material and a preparation method thereof, a positive electrode and a sodium ion battery. Background Art
[0002] Sodium ion batteries are batteries that use layered oxides (such as nickel iron manganese oxide and copper iron manganese oxide) materials, Prussian blue analogs (such as iron-based Prussian white, etc.), polyanions (such as sodium iron sulfate, sodium iron phosphate, etc.) as positive electrodes, and carbon materials (such as hard carbon, soft carbon) as negative electrodes. They mainly use esters and ethers as solvents. + Metal salts (such as sodium fluoride salts, sodium borate salts and perchlorates) electrolytes and various additives (such as film-forming, flame retardant and overcharge protection) form an electrolyte. Although sodium ion batteries have the advantages of good low-temperature performance, low cost, high safety and long cycle life, they still have serious low-voltage gassing problems, among which high-temperature low-voltage gassing is more obvious. In addition, high-voltage Fe 3+ The dissolution phenomenon is serious, which will lead to the attenuation of the positive electrode material capacity and the deposition of transition metal ions on the negative electrode surface, resulting in irreversible capacity attenuation. Based on the above two urgent problems (low voltage gas evolution and high voltage transition metal ion dissolution), the present invention is specially proposed. Summary of the invention
[0003] The object of the present invention is to provide a hollow porous composite sodium iron pyrophosphate positive electrode material and a preparation method thereof, a positive electrode and a sodium ion battery, aiming to improve at least one problem mentioned in the background technology.
[0004] The present invention is achieved in that:
[0005] In a first aspect, the present invention provides a method for preparing a hollow porous composite sodium iron pyrophosphate positive electrode material, comprising:
[0006] Prepare an emulsion including a surface loaded with Na + and Fe 2+ carbon-based particles, phosphate ions, water, cationic surfactants and oily organic solvents;
[0007] Raise the emulsion temperature to 120-160°C, and generate sodium iron pyrophosphate composite carbon-based particles after sufficient reaction;
[0008] The sodium iron pyrophosphate composite carbon-based particles are mixed with a metal salt colloidal solution to obtain a mixed colloidal solution, wherein the metal salt colloidal solution includes water, sodium ions, manganese ions, nickel ions, iron ions and a cross-linking agent;
[0009] Raising the temperature of the mixed glue solution to 160-200°C, and obtaining a composite cathode material precursor after sufficient reaction;
[0010] The positive electrode material precursor is placed at 550-650°C in an oxygen atmosphere and calcined for 1-12 hours.
[0011] In an optional embodiment, the preparation method provided by the present invention includes at least one of the following technical features (1) to (10):
[0012] (1) Carbon-based particles are Na + and Fe 2+ Ion exchange resin particles having adsorption capacity;
[0013] (2) the carbon-based particles are ion exchange resin particles, and the ion exchange resin is selected from at least one of isobutylene exchange resin, acrylic acid exchange resin and sulfonated polystyrene exchange resin;
[0014] (3) The particle size of the ion exchange resin particles is 2~3μm;
[0015] (4) Calcination time is 3.5~4.5h;
[0016] (5) After the sodium iron pyrophosphate composite carbon-based particles are fully reacted, the method further comprises: extracting the sodium iron pyrophosphate composite carbon-based particles from the liquid environment and washing them with pure water for multiple times;
[0017] mixing the washed sodium iron pyrophosphate composite carbon-based particles with a metal salt colloidal solution;
[0018] (6) The ratio of the amount of the mixed glue to the mass of the sodium iron pyrophosphate composite carbon-based particles is 100-200 mL: 8-60 g;
[0019] (7) the cationic surfactant is at least one selected from the group consisting of dodecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and benzalkonium chloride;
[0020] (8) The oily organic solvent is at least one selected from cyclohexane, cyclobutane, n-pentanol and isopropanol;
[0021] (9) The cross-linking agent is selected from at least one of PVP, PVA and PE;
[0022] (10) The molar ratio of sodium ion, manganese ion, nickel ion and iron ion in the metal salt colloidal solution is 1~6:0.7~4:0.7~4:0.7~4.
[0023] In an optional embodiment, the emulsion is prepared by:
[0024] The carbon-based particles are mixed with Na + , Fe 2+Mixed with mixed metal salt aqueous solution of phosphate ion to make Na + and Fe 2 + Adsorbed on the surface of carbon-based particles, a turbid solution is obtained, and the pH value of the mixed metal salt aqueous solution ranges from 5 to 7;
[0025] Mixing a cationic surfactant and an oily organic solvent to obtain an organic mixed liquid;
[0026] The turbid liquid and the organic mixed liquid are mixed and stirred to obtain an emulsion;
[0027] The ratio of carbon-based particles to oily organic solvent is 1~2g:100~200mL;
[0028] The mass ratio of carbon-based particles to cationic surfactant is 1~2:2~4.
[0029] In an optional embodiment, the mixed metal salt aqueous solution Na + The concentration is 0.5~2mol / L.
[0030] In an optional embodiment, the preparation method of the mixed metal salt aqueous solution is:
[0031] Ferrous sulfate and sodium phosphate are dissolved in water to obtain an iron-sodium composite solution, and sodium carbonate is added to the iron-sodium composite solution to adjust the pH value of the solution to 5-7 to obtain a mixed metal salt aqueous solution.
[0032] In an optional embodiment, the method further includes preparing a metal salt colloidal solution before obtaining the mixed colloidal solution. The method for preparing the metal salt colloidal solution includes:
[0033] Dissolving sodium salt, manganese salt, nickel salt and iron salt in water to obtain a metal salt solution;
[0034] Mixing the cross-linking agent and the metal salt solution and stirring them uniformly to obtain a metal salt colloidal solution;
[0035] The concentration of metal ions in the metal salt solution is 1~3 mol / L;
[0036] The ratio of the amount of the cross-linking agent to the amount of the metal salt solution is 0.2~0.4g:100~200mL.
[0037] In an optional embodiment, the sodium salt is sodium nitrate, the manganese salt is manganese acetate, the nickel salt is nickel acetate, and the iron salt is iron acetate.
[0038] In a second aspect, the present invention provides a hollow porous composite sodium iron pyrophosphate positive electrode material, which is prepared by the preparation method of any one of the aforementioned embodiments.
[0039] In a third aspect, the present invention provides a positive electrode, comprising the positive electrode material according to the aforementioned embodiment.
[0040] In a fourth aspect, the present invention provides a sodium ion battery comprising a positive electrode as described in the aforementioned embodiment.
[0041] The present invention has the following beneficial effects:
[0042] The preparation method provided by the present invention first reacts on the surface of carbon-based particles by a hydrothermal method to generate a layer of sodium iron pyrophosphate coating, then the mixed glue is loaded on the sodium iron pyrophosphate coating, the sodium ions, manganese ions, nickel ions and iron ions in the glue are reacted by a hydrothermal reaction to generate a composite hydroxide and loaded outside the sodium iron pyrophosphate coating, and finally the composite hydroxide is converted into a sodium manganese iron nickel layered oxide by sintering in an oxygen environment, and the carbon-based particles are oxidized to overflow as a gas, thereby obtaining a structure with sodium iron pyrophosphate having a hollow structure as the core and a layered oxide as the shell; and since the cross-linking agent of the outer layer of the precursor will oxidize and overflow in the form of gas during calcination, the outer layer of the sodium manganese iron nickel layered oxide layer is a porous structure. In addition, the present invention constructs a template with a water-in-oil microsphere therein by a microemulsion method, and can obtain a positive electrode material with a morphology more similar to a sphere than directly using carbon-based particles as a template, thereby further improving the electrochemical performance of the obtained positive electrode material.
[0043] The hollow porous composite sodium iron pyrophosphate positive electrode material prepared by the preparation method provided by the present invention is a hollow porous sodium iron pyrophosphate phase composite layered oxide material with a core-shell structure. The layered oxide in the positive electrode material is a shell that not only slows down the high voltage Fe 3+ Dissolution phenomenon, and the core dissolved Fe 3+ It can also be partially embedded in the interlayer of layered oxides. In addition, the two-phase composite also broadens the voltage range and greatly reduces the low-voltage gas production of the composite material; and the hollow multi-hole structure makes the positive electrode material have an ultra-high specific surface area. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0045] Figure 1 This is a SEM image of the composite sodium iron pyrophosphate positive electrode material prepared in Example 1 of the present invention, wherein Figure a and Figure b are SEM images at different magnifications. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0047] The following is a detailed description of the hollow porous composite sodium iron pyrophosphate positive electrode material and its preparation method, positive electrode and sodium ion battery provided in the embodiments of the present invention.
[0048] The present invention provides a method for preparing a hollow porous composite sodium iron pyrophosphate positive electrode material, comprising:
[0049] Prepare an emulsion including a surface loaded with Na + and Fe 2+ carbon-based particles, phosphate ions, water, cationic surfactants and oily organic solvents;
[0050] Raise the emulsion temperature to 120-160°C, and generate sodium iron pyrophosphate composite carbon-based particles after sufficient reaction;
[0051] The sodium iron pyrophosphate composite carbon-based particles are mixed with a metal salt colloidal solution to obtain a mixed colloidal solution, wherein the metal salt colloidal solution includes water, sodium ions, manganese ions, nickel ions, iron ions and a cross-linking agent;
[0052] Raising the temperature of the mixed glue solution to 160-200°C, and obtaining a composite cathode material precursor after sufficient reaction;
[0053] The positive electrode material precursor is placed at 550-650°C in an oxygen atmosphere and calcined for 1-12 hours.
[0054] The preparation method provided by the embodiment of the present invention is to first react on the surface of the carbon-based particles by a hydrothermal method to generate a layer of sodium iron pyrophosphate coating, and then load the mixed glue on the sodium iron pyrophosphate coating, and react the sodium ions, manganese ions, nickel ions and iron ions in the glue to generate composite hydroxides and load them outside the sodium iron pyrophosphate coating by a hydrothermal reaction, and finally sinter in an oxygen environment to convert the composite hydroxide into sodium manganese iron nickel layered oxide, and oxidize the carbon-based particles to overflow as gas, thereby obtaining a structure with sodium iron pyrophosphate having a hollow structure as the core and layered oxide as the shell; and because the cross-linking agent of the outer layer of the precursor will oxidize and overflow in the form of gas during calcination, the outer layer of sodium manganese iron nickel layered oxide layer is a porous structure. In addition, the present invention uses a microemulsion method to construct a template with oil-in-water microspheres, and can obtain a positive electrode material with a morphology more similar to a sphere than directly using carbon-based particles as templates, thereby further improving the electrochemical performance of the obtained positive electrode material.
[0055] The hollow porous composite sodium iron pyrophosphate positive electrode material prepared by the preparation method provided by the present invention is a sodium iron pyrophosphate phase composite layered oxide material with a hollow porous core-shell structure. The layered oxide in the positive electrode material is a shell that not only slows down the high voltage Fe 3+ Dissolution phenomenon, and the core dissolved Fe 3+ It can also be partially embedded in the interlayer of layered oxides. In addition, the two-phase composite also broadens the voltage range and greatly reduces the low-voltage gas production of the composite material; and the hollow multi-hole structure makes the positive electrode material have an ultra-high specific surface area.
[0056] The preparation method is specifically as follows:
[0057] S1. Obtaining carbon-based particles
[0058] The carbon-based microparticles may be purchased directly with a certain particle size, or the carbon-based materials may be purchased and then crushed into carbon-based microparticles with a suitable particle size.
[0059] Optionally, the particle size of the ion exchange resin particles is 2-3 μm.
[0060] Optionally, the crushing method is: use a crusher and an ultrasonic crusher to crush the carbon-based material to a particle size of 5 microns, and then use a planetary ball mill to further spheroidize it, and after screening, obtain 2-3 micron carbon-based particles.
[0061] It should be noted that the particle size of the carbon-based microspheres should not be too large. If the particle size of the carbon-based microspheres is too large, the hollow volume of the prepared positive electrode material will be larger after calcination, which will have an adverse effect on the particle size and specific surface area of the material.
[0062] Optionally, the carbon-based material is Na + and Fe 2+ Ion exchange resin particles with adsorption capacity.
[0063] Optionally, in order to ensure that the carbon-based microparticles have good adsorption properties for ferrous ions and sodium ions, the ion exchange resin is selected from at least one of isobutylene exchange resins, acrylic acid exchange resins and sulfonated polystyrene exchange resins.
[0064] S2, obtain mixed metal salt aqueous solution
[0065] Ferrous sulfate and sodium phosphate are dissolved in water to obtain an iron-sodium composite solution, and sodium carbonate is added to the iron-sodium composite solution to adjust the pH value of the solution to 5-7 to obtain a mixed metal salt aqueous solution.
[0066] Optionally, Na +The concentration is 0.5~2mol / L (e.g. 0.5mol / L, 1.0mol / L, 1.5mol / L or 2.0mol / L). Sodium ions, ferrous ions and phosphate ions are mixed in a stoichiometric ratio to generate ferric pyrophosphate.
[0067] S3, carbon-based microparticles adsorb metal ions
[0068] The ion exchange resin particles obtained in step S1 are added to the mixed metal salt aqueous solution obtained in step S2 and stirred sufficiently to allow the ion exchange resin to fully desorb H + , adsorption of Na + and Fe 2+ A turbid liquid was obtained.
[0069] S4. Preparation of emulsion
[0070] The cationic surfactant and the oily organic solvent are mixed to obtain an organic mixed liquid, and the turbid liquid and the organic mixed liquid are mixed and stirred to obtain an emulsion.
[0071] Optionally, the ratio of the carbon-based microparticles to the oily organic solvent is 1-2 g:100-200 mL (e.g., 1 g:200 mL, 2 g:200 mL, 1.5 g:100 mL, 2 g:100 mL, or 2 g:100 mL);
[0072] Optionally, the mass ratio of the carbon-based microparticles to the cationic surfactant is 1-2:2-4 (eg, 1:4, 1:2, 2:2, 1:3 or 2:3).
[0073] Optionally, the cationic surfactant is selected from at least one of dodecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and benzalkonium chloride.
[0074] Optionally, the oily organic solvent is selected from at least one of cyclohexane, cyclobutane, n-pentanol and isopropanol.
[0075] S5. First hydrothermal reaction
[0076] The temperature of the emulsion is raised to 120-160°C (e.g., 120°C, 140°C, or 160°C) and the reaction is carried out for 10-14h (e.g., 10h, 12h, or 14h) to allow the sodium ions, ferrous ions, and phosphate ions to react on the surface of the ion exchange resin to form a sodium ferric pyrophosphate coating layer to obtain sodium ferric pyrophosphate composite carbon-based particles.
[0077] S6. Preparation of metal salt colloidal solution
[0078] Dissolving sodium salt, manganese salt, nickel salt and iron salt in water to obtain a metal salt solution;
[0079] The cross-linking agent and the metal salt solution are mixed and stirred evenly to obtain a metal salt colloidal solution.
[0080] The concentration of metal ions in the metal salt solution is 0.3-1.4 mol / L (e.g., 0.3 mol / L, 0.5 mol / L, 0.8 mol / L, 1 mol / L or 0.1 mol / L), preferably 0.335-1.335 mol / L (e.g., 0.335 mol / L, 0.5 mol / L, 0.8 mol / L, 1 mol / L or 1.335 mol / L);
[0081] The ratio of the amount of the cross-linking agent to the amount of the metal salt solution is 0.2-0.4 g:100-200 mL (e.g., 0.2 g:100 mL, 0.2 g:200 mL, 0.4 g:100 mL, 0.3 g:100 mL or 0.3 g:200 mL);
[0082] Optionally, in order to make the prepared positive electrode material particles have better morphology, the sodium salt is sodium nitrate, the manganese salt is manganese acetate, the nickel salt is nickel acetate, and the iron salt is iron acetate.
[0083] Optionally, the molar ratio of sodium ions, manganese ions, nickel ions and iron ions in the metal salt solution is 1-6:0.7-4:0.7-4:0.7-4 (for example, 1:4:4:1, 6:1:2:1, 3:3:1:3, 2:0.7:4:3.3, 2:3.3:0.7:4, 4:2:3.3:0.7, etc.).
[0084] Optionally, the cross-linking agent is selected from at least one of PVP (polyvinyl pyrrolidone), PVA (polyvinyl alcohol) and PE (polyethylene).
[0085] S7, preparation of mixed glue solution
[0086] The sodium iron pyrophosphate composite carbon-based microparticles prepared in step S5 are extracted from the liquid environment and washed with pure water for multiple times.
[0087] The washed sodium iron pyrophosphate composite carbon-based particles are evenly mixed with the metal salt colloid solution to obtain a mixed colloid solution.
[0088] Optionally, the ratio of the amount of the mixed colloid to the mass of the sodium iron pyrophosphate composite carbon-based particles is 100~200mL: 8~60g (for example, 100mL: 60g, 200mL: 8g, 100mL: 8g, 200mL: 60g, 100mL: 10g, 100mL: 20g or 100mL: 30g).
[0089] S8. Second hydrothermal reaction
[0090] The temperature of the mixed gel solution is raised to 160-200° C. (eg, 160° C., 180° C. or 200° C.), and after reacting for 10-14 hours (eg, 10 hours, 12 hours or 14 hours), a layer of metal hydroxide is formed on the surface of the sodium iron pyrophosphate layer to obtain a composite positive electrode material precursor.
[0091] S9. Calcination
[0092] The composite positive electrode material precursor obtained by S8 is placed at 550-650°C (e.g., 550°C, 600°C or 650°C) in an oxygen atmosphere, calcined for 1-12h (e.g., 1h, 3h, 5h, 8h or 12h), and annealed for 0.5-1.5h (e.g., 0.5h, 1h or 1.5h).
[0093] During the calcination process, most of the ion exchange resin in the middle of the particle is oxidized into gas and overflows, thereby forming a hollow structure in the middle of the positive electrode material particle; and the metal hydroxide in the outermost layer is also decomposed into layered oxides, and the cross-linking agent in this layer is also oxidized into gas, thereby forming a porous structure in the outermost layer, and thus obtaining a hollow spherical multi-layer structure of a composite sodium iron pyrophosphate positive electrode material.
[0094] Preferably, the calcination time is 3.5-4.5 h (eg, 3.5 h, 4 h or 4.5 h). Calcination at this temperature can ensure that a suitable amount of ion exchange resin is not oxidized, and these unoxidized ion exchange resins can give the positive electrode material the ability to adsorb trivalent iron ions.
[0095] The hollow porous composite sodium iron pyrophosphate positive electrode material provided in the embodiment of the present invention is prepared by the preparation method provided in the embodiment of the present invention. The positive electrode material has better electrochemical performance.
[0096] The positive electrode provided by the embodiment of the present invention includes the hollow porous composite sodium iron pyrophosphate positive electrode material provided by the embodiment of the present invention.
[0097] The sodium ion battery provided by the embodiment of the present invention includes the positive electrode provided by the embodiment of the present invention.
[0098] The features and properties of the present invention are further described in detail below in conjunction with specific embodiments and comparative examples.
[0099] Example 1
[0100] 15 g of ferrous sulfate and 40 g of sodium phosphate were dissolved in water to obtain an iron-sodium composite solution, and sodium carbonate was added to the iron-sodium composite solution to adjust the pH of the solution to 5 to obtain a mixed metal salt aqueous solution, wherein the sodium ion concentration was 0.8 mol / L;
[0101] Add 2 g of acrylic acid cation exchange resin particles with a particle size of 2-3 μm to 50 mL of mixed metal salt aqueous solution and stir thoroughly. The ion exchange resin completes the ion exchange treatment and desorbs H + , adsorption of Na + and Fe 2+ A turbid liquid was obtained;
[0102] 4 g of dodecyltrimethylammonium chloride and 200 ml of cyclohexane were mixed to obtain an organic mixed solution, and the turbid liquid and the organic mixed solution were mixed and stirred to obtain an emulsion;
[0103] The emulsion was heated to 140° C. and reacted for 12 hours to obtain sodium iron pyrophosphate composite carbon-based particles, and the sodium iron pyrophosphate composite carbon-based particles were removed from the solution and washed three times for later use;
[0104] Dissolve 6 g of sodium nitrate, 4 g of manganese acetate, 4 g of nickel acetate, and 4 g of ferric acetate in 200 mL of water to obtain a metal salt solution;
[0105] 0.4 g PVP was mixed with the metal salt solution and stirred to obtain a metal salt colloidal solution;
[0106] The washed sodium iron pyrophosphate composite carbon-based particles and the metal salt colloidal solution were mixed uniformly in a ratio of 30 g: 200 mL to obtain a mixed colloidal solution;
[0107] The temperature of the mixed gel solution was raised to 160°C, and after reacting for 12 hours, a composite cathode material precursor was obtained;
[0108] The composite cathode material precursor was placed at 600°C in an oxygen atmosphere, calcined for 4 h, and annealed for 1 h to obtain a hollow porous composite sodium iron pyrophosphate cathode material, whose microstructure is as follows Figure 1 As shown in the figure, it can be seen that the particles have high sphericity and uniform particle size distribution.
[0109] Example 2
[0110] Dissolve 15 g of ferrous sulfate and 40 g of sodium phosphate in water to obtain an iron-sodium composite solution, add sodium carbonate to the iron-sodium composite solution to adjust the pH of the solution to 6, and obtain a mixed metal salt aqueous solution, wherein the sodium ion concentration is 0.13 mol / L;
[0111] Add 2 g of isobutylene cation exchange resin particles with a particle size of 2-3 μm into 50 mL of mixed metal salt aqueous solution and stir thoroughly. The ion exchange resin completes the ion exchange treatment and desorbs H + , adsorption of Na + and Fe 2+ A turbid liquid was obtained;
[0112] 8 g of dodecyltrimethylammonium chloride and 400 mL of cyclohexane were mixed to obtain an organic mixed solution, and the turbid liquid and the organic mixed solution were mixed and stirred to obtain an emulsion;
[0113] The emulsion was heated to 120° C. and reacted for 14 hours to obtain sodium iron pyrophosphate composite carbon-based particles, and the sodium iron pyrophosphate composite carbon-based particles were removed from the solution and washed three times for later use;
[0114] Dissolve 12 g of sodium nitrate, 8 g of manganese acetate, 8 g of nickel acetate, and 8 g of ferric acetate in 200 mL of water to obtain a metal salt solution;
[0115] 0.8 g PVA was mixed with the metal salt solution and stirred to obtain a metal salt colloidal solution;
[0116] The washed sodium iron pyrophosphate composite carbon-based particles and the metal salt colloidal solution were mixed uniformly in a ratio of 30 g: 200 mL to obtain a mixed colloidal solution;
[0117] The temperature of the mixed gel solution was raised to 180°C, and after reacting for 10 hours, a composite cathode material precursor was obtained;
[0118] The composite cathode material precursor was placed at 550° C. in an oxygen atmosphere, calcined for 5 h, and annealed for 1 h to obtain a hollow porous composite sodium iron pyrophosphate cathode material.
[0119] Example 3
[0120] Dissolve 15 g of ferrous sulfate and 40 g of sodium phosphate in water to obtain an iron-sodium composite solution, add sodium carbonate to the iron-sodium composite solution to adjust the pH of the solution to 7, and obtain a mixed metal salt aqueous solution, wherein the sodium ion concentration is 0.13 mol / L;
[0121] Add 2 g of sulfonated polystyrene exchange resin particles with a particle size of 2-3 μm into 50 mL of mixed metal salt aqueous solution and stir thoroughly. The ion exchange resin completes the ion exchange treatment and desorbs H + , adsorption of Na + and Fe 2+ A turbid liquid was obtained;
[0122] 2 g of dodecyltrimethylammonium chloride and 200 ml of cyclohexane were mixed to obtain an organic mixed solution, and the turbid solution and the organic mixed solution were mixed and stirred to obtain an emulsion;
[0123] The emulsion was heated to 160° C. and reacted for 10 hours to obtain sodium iron pyrophosphate composite carbon-based particles, and the sodium iron pyrophosphate composite carbon-based particles were removed from the solution and washed three times for later use;
[0124] Dissolve 2 g of sodium nitrate, 1.5 g of manganese acetate, 1.5 g of nickel acetate, and 1.5 g of ferric acetate in 150 mL of water to obtain a metal salt solution;
[0125] 0.2 g PE was mixed with the metal salt solution and stirred to obtain a metal salt colloidal solution;
[0126] The washed sodium iron pyrophosphate composite carbon-based particles and the metal salt colloidal solution were mixed uniformly in a ratio of 30 g: 200 mL to obtain a mixed colloidal solution;
[0127] The temperature of the mixed gel solution was raised to 200°C, and after reacting for 8 hours, a composite cathode material precursor was obtained;
[0128] The composite cathode material precursor was placed in an oxygen atmosphere at 650° C., calcined for 3 h, and annealed for 1 h to obtain a hollow porous composite sodium iron pyrophosphate cathode material.
[0129] Example 4
[0130] Dissolve 30 g of ferrous sulfate and 80 g of sodium phosphate in water to obtain an iron-sodium composite solution, add sodium carbonate to the iron-sodium composite solution to adjust the pH of the solution to 5, and obtain a mixed metal salt aqueous solution, wherein the sodium ion concentration is 1.6 mol / L;
[0131] Add 2 g of acrylic acid cation exchange resin particles with a particle size of 2-3 μm to 100 mL of mixed metal salt aqueous solution and stir thoroughly. The ion exchange resin completes the ion exchange treatment and desorbs H + , adsorption of Na + and Fe 2+ A turbid liquid was obtained;
[0132] 4 g of dodecyltrimethylammonium chloride and 200 ml of cyclohexane were mixed to obtain an organic mixed solution, and the turbid liquid and the organic mixed solution were mixed and stirred to obtain an emulsion;
[0133] The emulsion was heated to 140° C. and reacted for 12 hours to obtain sodium iron pyrophosphate composite carbon-based particles, and the sodium iron pyrophosphate composite carbon-based particles were removed from the solution and washed three times for later use;
[0134] Dissolve 6 g of sodium nitrate, 4 g of manganese acetate, 4 g of nickel acetate, and 4 g of ferric acetate in 100 mL of water to obtain a metal salt solution;
[0135] 0.4 g PVP was mixed with the metal salt solution and stirred to obtain a metal salt colloidal solution;
[0136] The washed sodium iron pyrophosphate composite carbon-based particles and the metal salt colloidal solution were mixed uniformly in a ratio of 60 g: 100 mL to obtain a mixed colloidal solution;
[0137] The temperature of the mixed gel solution was raised to 160°C, and after reacting for 12 hours, a composite cathode material precursor was obtained;
[0138] The composite cathode material precursor was placed at 600°C in an oxygen atmosphere, calcined for 4 h, and annealed for 1 h to obtain a hollow porous composite sodium iron pyrophosphate cathode material, whose microstructure is as follows Figure 1 As shown in the figure, it can be seen that the particles have high sphericity and uniform particle size distribution.
[0139] Example 5
[0140] 15 g of ferrous sulfate and 40 g of sodium phosphate were dissolved in water to obtain an iron-sodium composite solution, and sodium carbonate was added to the iron-sodium composite solution to adjust the pH of the solution to 5 to obtain a mixed metal salt aqueous solution, wherein the sodium ion concentration was 0.8 mol / L;
[0141] Add 2 g of acrylic acid cation exchange resin particles with a particle size of 2-3 μm to 50 mL of mixed metal salt aqueous solution and stir thoroughly. The ion exchange resin completes the ion exchange treatment and desorbs H + , adsorption of Na + and Fe 2+ A turbid liquid was obtained;
[0142] 4 g of dodecyltrimethylammonium chloride and 200 ml of cyclohexane were mixed to obtain an organic mixed solution, and the turbid liquid and the organic mixed solution were mixed and stirred to obtain an emulsion;
[0143] The emulsion was heated to 140° C. and reacted for 12 hours to obtain sodium iron pyrophosphate composite carbon-based particles, and the sodium iron pyrophosphate composite carbon-based particles were removed from the solution and washed three times for later use;
[0144] Dissolve 6 g of sodium nitrate, 4 g of manganese acetate, 4 g of nickel acetate, and 4 g of ferric acetate in 200 mL of water to obtain a metal salt solution;
[0145] 0.4 g PVP was mixed with the metal salt solution and stirred to obtain a metal salt colloidal solution;
[0146] The washed sodium iron pyrophosphate composite carbon-based particles and the metal salt colloidal solution were mixed uniformly in a ratio of 8 g: 200 mL to obtain a mixed colloidal solution;
[0147] The temperature of the mixed gel solution was raised to 160°C, and after reacting for 12 hours, a composite cathode material precursor was obtained;
[0148] The composite cathode material precursor was placed at 600°C in an oxygen atmosphere, calcined for 4 h, and annealed for 1 h to obtain a hollow porous composite sodium iron pyrophosphate cathode material, whose microstructure is as follows Figure 1 As shown in the figure, it can be seen that the particles have high sphericity and uniform particle size distribution.
[0149] Comparative Example 1
[0150] This comparative example is basically the same as Example 1, except that calcination is performed after obtaining the sodium iron pyrophosphate composite carbon-based particles, and the specific operation method of the calcination step is the same as that of Example 1.
[0151] Comparative Example 2
[0152] This comparative example is basically the same as Example 1, except that after obtaining the turbid liquid, it is not mixed with a surfactant and an oily organic solvent, but is directly heated to perform a hydrothermal reaction. The operating conditions of the hydrothermal reaction and the operation method after the hydrothermal reaction are the same as those of Example 1.
[0153] Comparative Example 3
[0154] This comparative example is basically the same as Example 1, except that the metal salt solution is not mixed with PVP, and the hydrothermal reaction is directly carried out, and the operating conditions of the hydrothermal reaction and the operation method after the hydrothermal reaction are the same as those in Example 1.
[0155] Comparative Example 4
[0156] This comparative example is basically the same as Example 1, except that the ion exchange resin particles are replaced by metal copper particles. The obtained positive electrode material particles do not have a hollow structure.
[0157] Experimental example
[0158] The positive electrode materials prepared in each embodiment and comparative example were coated with a synthetic active material oil-based formula to prepare positive electrode sheets, the negative electrode was coated with a hard carbon water-based formula to prepare negative electrode sheets, a polypropylene separator was used as the separator, and 1M sodium salt + ester solvent (EC / DMC) was used as the electrolyte to prepare a laminated 5Ah soft-pack battery.
[0159] Each embodiment and comparative example was tested for 0.1C / 0.1C charge / discharge capacity, first coulomb efficiency, capacity retention rate at 5C rate, capacity retention rate after 100 cycles of 0.1C / 0.1C charge / discharge, gas production after 100 cycles of 0.1C / 0.1C charge / discharge, and capacity retention rate after 100 cycles of 0.5C / 1C high temperature cycles. The test results are recorded in Table 1.
[0160] Table 1 Electrochemical properties of the batteries prepared in the examples and comparative examples
[0161]
[0162] It can be seen from Table 1 that the positive electrode materials prepared in various embodiments of the present invention have better electrochemical performance after being assembled into batteries.
[0163] Comparing Example 1 with Comparative Example 1, the specific capacity and cycle performance of Comparative Example 1 are poor, and the product prepared in Comparative Example 1 does not have a layered oxide layer compared to Example 1, which indicates that forming a layered oxide coating layer outside the sodium iron pyrophosphate can improve the specific capacity and cycle performance of the positive electrode material.
[0164] Comparing Example 1 with Comparative Example 2, the cycle performance of Comparative Example 2 is poor. Compared with Example 1, Comparative Example 2 directly uses ion exchange resin as the core instead of using oil-in-water droplets as a template through the microemulsion method. This shows that the positive electrode material prepared by the microemulsion method can improve the cycle performance of the positive electrode material.
[0165] Comparing Example 1 with Comparative Example 3, the specific capacity and cycle performance of Comparative Example 3 are poor. Compared with Example 1, Comparative Example 3 does not use a cross-linking agent. If a cross-linking agent is not used, the positive electrode material prepared in Comparative Example 3 does not have a porous structure, which indicates that the porous structure of the prepared positive electrode material can improve the surface electrochemical activity and wettability of the positive electrode material.
[0166] Comparing Example 1 with Comparative Example 4, the specific capacity of Comparative Example 4 is poor. Compared with Example 1, Comparative Example 4 does not use carbon-based particles as a template, and the finished product does not have a hollow structure, which indicates that the hollow structure of the prepared positive electrode material can improve the surface electrochemical activity and wettability of the positive electrode material.
[0167] In summary, the method for preparing the hollow porous composite sodium iron pyrophosphate positive electrode material provided in the embodiment of the present invention has the following characteristics:
[0168] 1. Sodium iron pyrophosphate high voltage Fe 3+ The dissolution is serious, but coating with layered oxides can alleviate the dissolution phenomenon (first, the iron content of the layered oxide itself is low; second, the Fe dissolved in the core 3+ It can be partially embedded in the interlayer of layered oxides, and it can broaden the voltage range, reduce the problem of low-voltage gas production, and improve the overall capacity (with less cost increase);
[0169] 2. The microemulsion method can be used to construct a uniform microsphere structure core (sodium iron pyrophosphate), and the hydrothermal method can further deposit the shell (layered oxide) using the core as a template to construct a core-shell structure microsphere, which can produce a positive electrode material with good morphology;
[0170] 3. The hollow porous structure increases the specific surface area of the material and stimulates the material capacity. When the ion exchange resin particles are used as the core, the ion exchange resin remaining after calcination can also play a small amount of Fe 3+ Exchange effect;
[0171] 4. The preparation process only has one calcination step, which is conducive to the composite and crystallization of the two phases.
[0172] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a hollow porous composite sodium iron pyrophosphate positive electrode material, characterized in that: include: Prepare an emulsion, wherein the emulsion includes a surface loaded with Na + and Fe 2+ carbon-based particles, phosphate ions, water, cationic surfactants and oily organic solvents; Raising the temperature of the emulsion to 120-160° C. to generate sodium iron pyrophosphate composite carbon-based particles after sufficient reaction; The sodium iron pyrophosphate composite carbon-based particles are mixed with a metal salt colloidal solution to obtain a mixed colloidal solution, wherein the metal salt colloidal solution includes water, sodium ions, manganese ions, nickel ions, iron ions and a cross-linking agent; Raising the temperature of the mixed glue solution to 160-200° C., and obtaining a composite positive electrode material precursor after sufficient reaction; The positive electrode material precursor is placed in an oxygen atmosphere at 550-650° C. and calcined for 1-12 hours.
2. The preparation method according to claim 1, characterized in that: It includes at least one of the following technical features (1) to (10): (1) The carbon-based particles are Na + and Fe 2+ Ion exchange resin particles having adsorption capacity; (2) The carbon-based particles are ion exchange resin particles, and the ion exchange resin is selected from at least one of isobutylene exchange resin, acrylic acid exchange resin and sulfonated polystyrene exchange resin; (3) The particle size of the ion exchange resin particles is 2-3 μm; (4) Calcination time is 3.5~4.5h; (5) After the sodium iron pyrophosphate composite carbon-based particles are fully reacted to form the sodium iron pyrophosphate composite carbon-based particles, the method further comprises: extracting the sodium iron pyrophosphate composite carbon-based particles from the liquid environment and washing them with pure water for multiple times; mixing the washed sodium iron pyrophosphate composite carbon-based particles with a metal salt colloidal solution; (6) The ratio of the amount of the mixed glue to the mass of the sodium iron pyrophosphate composite carbon-based particles is 100-200 mL: 8-60 g; (7) The cationic surfactant is at least one selected from the group consisting of dodecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and benzalkonium chloride; (8) The oily organic solvent is selected from at least one of cyclohexane, cyclobutane, n-pentanol and isopropanol; (9) The cross-linking agent is selected from at least one of PVP, PVA and PE; (10) The molar ratio of sodium ions, manganese ions, nickel ions and iron ions in the metal salt colloidal solution is 1-6:0.7-4:0.7-4:0.7-4.
3. The preparation method according to claim 1, characterized in that: The method of configuring the emulsion includes: The carbon-based particles are mixed with Na + , Fe 2+ Mixed with mixed metal salt aqueous solution of phosphate ion to make Na + and Fe 2 + Adsorbing on the surface of the carbon-based particles to obtain a turbid solution, wherein the pH value of the mixed metal salt aqueous solution is 5-7; Mixing the cationic surfactant and the oily organic solvent to obtain an organic mixed liquid; The turbid liquid and the organic mixed liquid are mixed and stirred to obtain the emulsion; The ratio of the carbon-based microparticles to the oily organic solvent is 1-2 g: 100-200 mL; The mass ratio of the carbon-based particles to the cationic surfactant is 1-2:2-4.
4. The preparation method according to claim 3, characterized in that: The mixed metal salt aqueous solution contains Na + The concentration is 0.5~2mol / L.
5. The preparation method according to claim 3, characterized in that: The preparation method of the mixed metal salt aqueous solution is: Ferrous sulfate and sodium phosphate are dissolved in water to obtain an iron-sodium composite solution, and sodium carbonate is added to the iron-sodium composite solution to adjust the pH value of the solution to 5-7 to obtain the mixed metal salt aqueous solution.
6. The preparation method according to claim 1, characterized in that: Before obtaining the mixed colloid solution, the method further includes preparing the metal salt colloid solution. The method for preparing the metal salt colloid solution includes: Dissolving sodium salt, manganese salt, nickel salt and iron salt in water to obtain a metal salt solution; Mixing the cross-linking agent and the metal salt solution and stirring them uniformly to obtain the metal salt colloidal solution; The concentration of metal ions in the metal salt solution is 0.3-1.4 mol / L; The ratio of the amount of the cross-linking agent to the amount of the metal salt solution is 0.2-0.4 g: 100-200 mL.
7. The preparation method according to claim 6, characterized in that: The sodium salt is sodium nitrate, the manganese salt is manganese acetate, the nickel salt is nickel acetate, and the iron salt is iron acetate.
8. A hollow porous composite sodium iron pyrophosphate positive electrode material, characterized in that: The method is prepared according to any one of claims 1 to 7.
9. A positive electrode, characterized in that Comprising the positive electrode material as claimed in claim 8.
10. A sodium ion battery, characterized in that: Comprising the positive electrode as claimed in claim 9.