Ionic liquid and preparation method, perovskite solar cell and preparation method, photovoltaic module

By using small-molecular ionic liquids enriched with functional group in perovskite solar cells, passivating the defects of the perovskite layer and forming a three-dimensional framework network, the problem of poor stability of the perovskite layer is solved, and the photoelectric conversion efficiency and long-term development are improved. stability.

CN118373841BActive Publication Date: 2024-12-06TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410809752.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-12-06
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

The poor stability and short life of perovskite solar cells are mainly due to the perovskite grain boundary defects in the perovskite layer that lead to the penetration of water and oxygen in the air, which accelerates the decomposition, affecting the photoelectric conversion efficiency and long-term stability.

Method used

A small molecule ionic liquid including alkyl chains, -COOH, -B(OH)2, -PO(OH)2, -CF3, -NH2, -SO3H and other functional groups is used, and is transferred to the perovskite layer to passivate. Defects and polymerize at grain boundaries to form a three-dimensional framework network, improving the stability of the perovskite layer and photoelectric conversion efficiency.

Benefits of technology

By passivating the defects of the perovskite layer and reducing the risk of water and oxygen penetration, the photoelectric conversion efficiency and long-term stability of perovskite solar cells are significantly improved, and the life of the equipment is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118373841B_ABST
    Figure CN118373841B_ABST
Patent Text Reader

Abstract

The present application relates to the field of batteries, and proposes an ionic liquid and a preparation method, a perovskite solar cell and a preparation method, and a photovoltaic module. The ionic liquid includes #imgabs0#, wherein R1 includes an alkyl chain; R2 includes at least one of ‑COOH, ‑B(OH)2, ‑PO(OH)2, ‑CF3, ‑NH2, and ‑SO3H; and Ar includes an aromatic heterocycle containing a substituent. Thus, adding the ionic liquid to the perovskite layer can improve the long-term stability of the perovskite layer and improve the photoelectric conversion efficiency of the perovskite solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and specifically, to ionic liquids and preparation methods, perovskite solar cells and preparation methods, and photovoltaic modules. Background Art

[0002] At present, perovskite solar cells have attracted widespread attention because their photoelectric conversion efficiency exceeds that of traditional silicon solar cells. However, the poor stability and short life of perovskite solar cells limit their development. The stability of perovskite solar cells depends to a certain extent on the stability of the perovskite layer. The perovskite layer usually contains a large number of grain boundary defects, which makes it easy for water and oxygen in the air to penetrate into the perovskite through the defects, causing the perovskite to decompose. Therefore, the current perovskite solar cells need further improvement. Summary of the invention

[0003] The present application aims to solve one of the technical problems in the related art at least to some extent.

[0004] In a first aspect, the present application proposes an ionic liquid comprising , wherein R1 includes an alkyl chain; R2 includes at least one of -COOH, -B(OH)2, -PO(OH)2, -CF3, -NH2, and -SO3H; and Ar includes an aromatic heterocycle containing a substituent. Thus, adding the above-mentioned small molecule ionic liquid to the perovskite layer can passivate the defects of the perovskite layer, improve the quality of the perovskite layer, and thus improve the photoelectric conversion efficiency of the perovskite solar cell. The small molecule ionic liquid can also be polymerized in situ in the perovskite layer to form a polymer of the ionic liquid. The three-dimensional skeleton network formed by the polymer can improve the long-term stability of the perovskite layer, thereby improving the life of the perovskite solar cell.

[0005] According to some embodiments of the present application, at least one of the following conditions is met: (1) R1 includes one of the alkyl chains of 1 to 18 carbon atoms; (2) R2 includes at least one of -B(OH)2 or -PO(OH)2; (3) Ar includes Formula 1, Formula 2: Formula 3, Formula 4: Formula 5, Formula 6, Formula 7, At least one of formula 8, fluorobenzene, and a benzene ring.

[0006] According to some embodiments of the present application, at least one of the following conditions is satisfied: (1) R1 includes one of the alkyl chains of 1 to 4 carbon atoms; Ar includes Formula 1, Formula 5-1, At least one of Formula 5-2.

[0007] The second aspect of the present application provides a method for preparing the ionic liquid provided in the first aspect of the present application, comprising: mixing vinyl imidazole, R2-Ar-R1-Br, and a solvent, heating to reflux, and drying to obtain the ionic liquid. Thus, the ionic liquid prepared by the method has all the characteristics and advantages of the aforementioned ionic liquid, which will not be repeated here. In general, it has at least the advantages of improving the quality of the perovskite layer and improving the long-term stability of the perovskite layer.

[0008] According to some embodiments of the present application, the molar ratio of the vinyl imidazole to the R2-Ar-R1-Br is 1:(1.1-2).

[0009] According to some embodiments of the present application, the molar ratio of the vinyl imidazole to the R2-Ar-R1-Br is 1:(1.1-1.5).

[0010] According to some embodiments of the present application, the temperature of the heating reflux is 50° C.-70° C., and the time of the heating reflux is 12 h-24 h.

[0011] The third aspect of the present application provides a perovskite solar cell, comprising: a substrate; a perovskite layer, the perovskite layer is arranged on one side of the substrate, the perovskite layer comprises a perovskite material and an additive, the additive comprises the ionic liquid provided in the first aspect of the present application and a polymer formed by the ionic liquid; an electrode layer, the electrode layer is arranged on a side of the perovskite layer away from the substrate. Thus, the photoelectric conversion efficiency and long-term stability of the perovskite cell can be improved.

[0012] According to some embodiments of the present application, the molar ratio of the additive to the perovskite material is (1-10):150.

[0013] According to some embodiments of the present application, the molar ratio of the additive to the perovskite material is (3-5):150.

[0014] In this way, the photoelectric conversion efficiency of the perovskite cell is improved while the long-term stability of the perovskite cell is improved.

[0015] According to some embodiments of the present application, the perovskite solar cell further includes: a hole transport layer, the hole transport layer is located between the substrate and the perovskite layer; an electron transport layer, the electron transport layer is located on a side of the perovskite layer away from the hole transport layer; a hole blocking layer, the hole blocking layer is located on a side of the electron transport layer away from the perovskite layer, and the electrode layer is located on a side of the hole blocking layer away from the electron transport layer.

[0016] According to some embodiments of the present application, the perovskite cell satisfies at least one of the following conditions: the perovskite material includes ABX3, wherein A includes Cs + 、MA + (CH3NH3 + ), FA + (CH(NH2)2 + ), Rb + At least one of B including Pb 2 + Sn 2+ , Mn 2+ at least one of, X comprises at least one of halogen ions; the material forming the hole transport layer comprises at least one of [2-(9H-carbazole-9-yl)ethyl]phosphoric acid, [4-(9H-carbazole-9-yl)butyl]phosphoric acid, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid, [2-(3,6-dimethyl-9H-carbazole-9-yl)ethyl]phosphoric acid, [2-(3,6-di-tert-butyl-9H-carbazole-9-yl)ethyl]phosphoric acid, [4-(3,6-dibromo-9H-carbazole-9-yl)butyl]phosphoric acid, poly[bis(4-phenyl) (2,4,6-trimethylphenyl)amine], poly(3-hexylthiophene-2,5-diyl), polyethylenedioxythiophene-poly(styrene sulfonate); the material forming the electron transport layer comprises [6,6]-phenyl-C 61 -Methyl butyrate, C 60 , tin oxide; the material forming the hole blocking layer includes at least one of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline or zirconium acetylacetonate; the material forming the electrode layer includes at least one of silver, copper, oxide, and carbon electrode.

[0017] The fourth aspect of the present application provides a method for preparing the perovskite solar cell provided in the third aspect of the present application, comprising: mixing an ionic liquid, an A source, a B source, an X source, and a solvent to form a precursor solution, forming the precursor solution on one side of the substrate, heating and annealing to form the perovskite layer; and forming an electrode layer on the side of the perovskite layer away from the substrate. Thus, the perovskite solar cell prepared by the method has a high photoelectric conversion efficiency and can also improve the long-term stability of the perovskite solar cell.

[0018] According to some embodiments of the present application, the method of forming the perovskite layer includes: mixing the ionic liquid, A source, B source, X source, and solvent to form a precursor solution, forming the precursor solution on one side of the substrate, and heating and annealing to form the perovskite layer.

[0019] According to some embodiments of the present application, the mass percentage of the ionic liquid in the precursor solution is 0.5 mg / mL-3 mg / mL.

[0020] According to some embodiments of the present application, the temperature of the heating annealing is 100° C.-150° C., and the time of the heating annealing is 30 min-40 min.

[0021] According to some embodiments of the present application, the method further includes: forming a hole transport layer between the substrate and the perovskite layer; forming an electron transport layer on a side of the perovskite layer away from the hole transport layer; forming a hole blocking layer on a side of the electron transport layer away from the perovskite layer; and forming the electrode layer on a side of the hole blocking layer away from the electron transport layer.

[0022] The fifth aspect of the present application provides a photovoltaic module, including the perovskite solar cell provided in the third aspect of the present application or the perovskite solar cell prepared by the method provided in the fourth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0024] Figure 1 A schematic structural diagram of a perovskite solar cell according to an embodiment of the present application is shown.

[0025] Reference numerals:

[0026] 1: Perovskite solar cell; 11: substrate; 12: hole transport layer; 13: perovskite layer; 14: electron transport layer; 15: hole blocking layer; 16: electrode layer. DETAILED DESCRIPTION

[0027] The embodiments of the present application are described in detail below. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific technology or conditions are indicated in the embodiments, the technology or conditions described in the document in this area or the product specification are used. The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained commercially.

[0028] The stability of perovskite solar cells depends to a certain extent on the stability of the perovskite layer. The perovskite layer usually contains a large number of grain boundary defects, which cause water and oxygen in the air to penetrate into the perovskite through these defects, thereby causing the perovskite to decompose. At the same time, due to the unstable energy of interface defects, it is easily destroyed by external factors (such as light, electric field, heat, etc.), which will also accelerate the decomposition of perovskite. In order to improve the stability of the perovskite layer, the stability problem can be alleviated to a certain extent by adjusting the perovskite composition and improving the packaging technology. However, under high temperature and high humidity conditions, perovskite solar cells still have low stability and low photoelectric conversion efficiency.

[0029] The first aspect of the present application provides an ionic liquid, comprising , wherein R1 includes an alkyl chain; R2 includes at least one of -COOH, -B(OH)2, -PO(OH)2, -CF3, -NH2, and -SO3H; and Ar includes an aromatic heterocycle containing a substituent. Thus, adding this small molecule ionic liquid to the perovskite layer can improve the quality of the perovskite layer, improve the stability of the perovskite layer under high temperature and high humidity conditions, and improve the photoelectric conversion efficiency of the perovskite solar cell.

[0030] The following is an explanation of the principle by which the present application can achieve the above beneficial effects:

[0031] The small molecule ionic liquid proposed in the present application includes a vinyl imidazole unit, R1 and R2, wherein the introduction of heteroatoms can improve the coordination ability of the ionic liquid with the ions in the perovskite layer, and R2 can also form hydrogen bonds with the ions, thereby increasing the interaction between the ionic liquid and the ions in the perovskite layer, reducing the migration rate of the ions, passivating related defects, and thereby improving the quality of the perovskite layer. In addition, the small molecule ionic liquid can also aggregate at the grain boundaries, thereby reducing the risk of water and oxygen in the air penetrating into the perovskite through the grain boundary defects, reducing the probability of perovskite decomposition, and improving the stability of the perovskite. The small molecule ionic liquid enriched at the grain boundaries is more likely to polymerize to form a polymer, so that it can be effectively cross-linked when doped at a low concentration, thereby passivating the grain boundary defects. The polymer formed by the polymerization of the small molecule ionic liquid can also form a three-dimensional skeleton network to further reduce the defect density, reduce the rate of lateral carrier transmission and ion movement, and passivate the defects. By in-situ polymerization of small molecule ionic liquids in the perovskite layer to form polymers, compared to directly adding polymers to the perovskite layer, the uniformity of distribution of small molecule ionic liquids and polymers in the perovskite layer can be improved, thereby improving the overall quality of the perovskite layer and being more conducive to the preparation of large-area devices; compared to only adding small molecule ionic liquids to the perovskite layer, polymers are more stable during the long-term operation of perovskite solar cells and have a lower risk of volatilization, thereby improving the long-term stability of perovskite solar cells.

[0032] In the present application, the structure of the ionic liquid can be identified by hydrogen nuclear magnetic resonance spectroscopy and high-resolution mass spectrometry.

[0033] According to some embodiments of the present application, R1 includes an alkyl chain.

[0034] As an example, R1 may include one of alkyl chains of 1 to 18 carbon atoms.

[0035] As an example, R1 may include one of the alkyl chains of 1 to 4 carbon atoms, such as methyl, ethyl, propyl or butyl.

[0036] According to some embodiments of the present application, R2 includes at least one of -COOH, -B(OH)2, -PO(OH)2, -CF3, -NH2, and -SO3H. Thus, the above-mentioned types of R2 can form hydrogen bonds with ions in the perovskite layer, thereby increasing the binding force between the small molecule ionic liquid and the ions, reducing the migration rate of the ions, and thus passivating the defects of the perovskite layer, improving the quality of the perovskite layer, and improving the photoelectric conversion efficiency. According to some specific embodiments of the present application, R2 includes at least one of -B(OH)2 or -PO(OH)2.

[0037] According to some embodiments of the present application, Ar includes Formula 1, Formula 2: Formula 3, Formula 4: Formula 5, Formula 6, Formula 7, At least one of formula 8, fluorobenzene, and benzene ring. The above-mentioned types of Ar can form hydrogen bonds with ions in the perovskite layer, thereby increasing the binding force between the small molecule ionic liquid and the ions, reducing the migration rate of the ions, and thus passivating the defects of the perovskite layer, improving the quality of the perovskite layer, and improving the photoelectric conversion efficiency.

[0038] As an example, the fluorobenzene includes: Formula 5-1, Formula 5-2 Formula 5-3, At least one of formula 5-4.

[0039] According to some specific embodiments of the present application, Ar includes Formula 1, Formula 5-1, At least one of Formula 5-2.

[0040] The second aspect of the present application provides a method for preparing the ionic liquid provided in the first aspect of the present application, comprising: mixing vinyl imidazole, R2-Ar-R1-Br, and a solvent, heating to reflux, and drying to obtain the ionic liquid. Thus, the ionic liquid prepared by the method has all the characteristics and advantages of the aforementioned ionic liquid, which will not be repeated here. In general, it has at least the advantages of improving the photoelectric conversion efficiency of perovskite solar cells and improving their long-term stability.

[0041] According to some embodiments of the present application, the molar ratio of the vinyl imidazole to the R2-Ar-R1-Br can be 1: (1.1-2), for example, 1: 1.1, 1: 1.2, 1: 1.4, 1: 1.6, 1: 1.8 or 1: 2, etc., or can be a range of any of the above numerical values. Thus, the vinyl imidazole can be fully converted, which is beneficial to the separation and purification of subsequent products. According to some specific embodiments of the present application, the molar ratio of the vinyl imidazole to the R2-Ar-R1-Br can be 1: (1.1-1.5).

[0042] According to some embodiments of the present application, the temperature of the heating reflux is 50° C.-70° C., and the time of the heating reflux is 12 h-24 h.

[0043] As an example, the temperature of the heating reflux may be 50° C., 55° C., 60° C., 65° C. or 70° C., or may be a range consisting of any of the above values.

[0044] As an example, the heating reflux time can be 12h-24h, for example, 12h, 14h, 16h, 18h, 20h, 22h, 24h, etc., or can be a range consisting of any of the above values.

[0045] Therefore, by keeping the temperature and time of heating reflux within the above range, vinyl imidazole and R2-Ar-R1-Br can be fully dissolved in the reaction solution, thereby improving the reaction conversion rate, making full use of the raw materials, and reducing costs.

[0046] The third aspect of the present application provides a perovskite solar cell 1, referring to Figure 1The perovskite solar cell 1 comprises: a substrate 11; a perovskite layer 13, the perovskite layer 13 is arranged on one side of the substrate 11, the perovskite layer 13 comprises a perovskite material and an additive, the additive comprises the aforementioned ionic liquid and a polymer formed by the ionic liquid; an electrode layer 16, the electrode layer 16 is arranged on the side of the perovskite layer 13 away from the substrate 11. Thus, the additive of the perovskite layer comprises a small molecule ionic liquid and a polymer formed by the same, the introduction of heteroatoms can improve the coordination ability of the ionic liquid with the ions in the perovskite layer, R2 can also form hydrogen bonds with the ions, thereby improving the interaction between the ionic liquid and the ions in the perovskite layer, reducing the migration rate of the ions, passivating related defects, and thereby improving the quality of the perovskite layer. In addition, the small molecule ionic liquid can also gather at the grain boundary, thereby reducing the risk of water and oxygen in the air penetrating into the perovskite through the grain boundary defects, reducing the probability of perovskite decomposition, and improving the stability of the perovskite. Small molecule ionic liquids enriched at grain boundaries are more likely to polymerize to form polymers, which can effectively cross-link when doped at low concentrations, thereby passivating grain boundary defects. The polymers formed by the polymerization of small molecule ionic liquids can also form a three-dimensional skeleton network to further reduce the defect density, reduce the rate of lateral carrier transport and ion movement, and passivate defects. Compared with directly adding polymers to the perovskite layer, the in-situ polymerization of small molecule ionic liquids in the perovskite layer to form polymers can improve the uniformity of the distribution of small molecule ionic liquids and polymers in the perovskite layer, thereby improving the overall quality of the perovskite layer and being more conducive to the preparation of large-area devices; compared with only adding small molecule ionic liquids to the perovskite layer, the polymers are more stable during the long-term operation of perovskite solar cells and have a lower risk of volatilization, thereby improving the long-term stability of perovskite solar cells.

[0047] According to some embodiments of the present application, the molar ratio of the additive to the perovskite material may be (1-10):150, for example, 1:150, 3:150, 5:150, 7:150, 9:150 or 10:150, or may be a range of any of the above numerical values. Thus, while improving the quality and stability of the perovskite layer, the mass proportion of the perovskite material in the perovskite layer is increased, thereby improving the photoelectric conversion efficiency of the perovskite solar cell. According to some specific embodiments of the present application, the molar ratio of the additive to the perovskite material may be (3-5):150.

[0048] As an example, the perovskite material may include ABX3, wherein A includes Cs + 、MA + (CH3NH3 + ), FA + (CH(NH2)2 + ), Rb +At least one of B including Pb 2+ Sn 2+ , Mn 2+ At least one of, X comprises at least one of halogen ions.

[0049] According to some embodiments of the present application, reference Figure 1 The perovskite solar cell 1 may further include: a hole transport layer 12, the hole transport layer 12 is located between the substrate 11 and the perovskite layer 13; an electron transport layer 14, the electron transport layer 14 is located on the side of the perovskite layer 13 away from the hole transport layer 12; a hole blocking layer 15, the hole blocking layer 15 is located on the side of the electron transport layer 14 away from the perovskite layer 13, and the electrode layer 16 is located on the side of the hole blocking layer 15 away from the electron transport layer 14. Thus, the photoelectric conversion efficiency of the perovskite solar cell 1 is improved.

[0050] As an example, the material forming the hole transport layer may include at least one of [2-(9H-carbazole-9-yl)ethyl]phosphoric acid, [4-(9H-carbazole-9-yl)butyl]phosphoric acid, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid, [2-(3,6-dimethyl-9H-carbazole-9-yl)ethyl]phosphoric acid, [2-(3,6-di-tert-butyl-9H-carbazole-9-yl)ethyl]phosphoric acid, [4-(3,6-dibromo-9H-carbazole-9-yl)butyl]phosphoric acid, poly[bis(4-phenyl) (2,4,6-trimethylphenyl)amine], poly(3-hexylthiophene-2,5-diyl), and polyethylenedioxythiophene-poly(styrene sulfonate).

[0051] As an example, the material forming the electron transport layer may include [6,6]-phenyl-C 61 -Methyl butyrate, C 60 , tin oxide or at least one of the following.

[0052] As an example, the material forming the hole blocking layer may include at least one of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline or zirconium acetylacetonate.

[0053] As an example, the material forming the electrode layer may include at least one of silver, copper, oxide, and carbon electrode.

[0054] The fourth aspect of the present application provides a method for preparing a perovskite solar cell, comprising: mixing the ionic liquid, A source, B source, X source, and solvent to form a precursor solution, forming the precursor solution on one side of the substrate, heating and annealing to form a perovskite layer; and forming an electrode layer on a side of the perovskite layer away from the substrate.

[0055] According to some embodiments of the present application, the substrate may be conductive glass. The conductive glass is ultrasonically cleaned with deionized water, acetone, and isopropanol in sequence, and placed in a drying oven for drying. The dried conductive glass substrate is placed in an ultraviolet ozone machine for treatment to remove organic impurities on its surface and optimize its surface wettability.

[0056] According to some embodiments of the present application, an ionic liquid, a source A, a source B, a source X, and a solvent are mixed to form a precursor solution, and the precursor solution is formed on one side of the substrate in an inert gas glove box. For example, the perovskite precursor solution can be formed on one side of the substrate by spin coating, and after heating and annealing, a perovskite layer having a small molecule ionic liquid, a polymer of the ionic liquid, and a perovskite material can be formed.

[0057] According to some embodiments of the present application, the temperature of the heating annealing is 100° C.-150° C., and the time of the heating annealing is 30 min-40 min.

[0058] As an example, the temperature of the heating annealing may be 100° C., 110° C., 120° C., 130° C., 140° C. or 150° C., or may be a range consisting of any of the above values.

[0059] As an example, the heating annealing time may be 30 min, 32 min, 34 min, 36 min, 38 min or 40 min, etc., or may be a range consisting of any of the above values.

[0060] Therefore, by making the temperature and time of the heating annealing within the above range, the nucleation and growth of the perovskite can be regulated, and the cross-linking reaction between the ionic liquids can be promoted to form high-quality perovskite crystals.

[0061] According to some embodiments of the present application, the mass proportion of the ionic liquid in the precursor solution can be 0.5 mg / mL-3 mg / mL. For example, it can be 0.5 mg / mL, 1 mg / mL, 1.5 mg / mL, 2 mg / mL, 2.5 mg / mL or 3 mg / mL, etc., or it can be a range composed of any of the above numerical values. Thus, by making the content of the ionic liquid in the precursor solution within the above range, the ionic liquid can form a cross-linked network at the perovskite grain boundary, thereby improving the quality of the perovskite film.

[0062] According to some embodiments of the present application, before forming the perovskite layer, the method may further include: forming a hole transport layer on one side of the substrate. The method for forming the hole transport layer is not particularly limited. As an example, a solution containing a hole transport layer material may be coated on the substrate to obtain the hole transport layer.

[0063] According to some embodiments of the present application, before forming the electrode layer, the method may further include: forming an electron transport layer on a side of the perovskite layer away from the hole transport layer, and forming a hole blocking layer on a side of the electron transport layer away from the perovskite layer.

[0064] The fifth aspect of the present application provides a photovoltaic module, including the perovskite solar cell provided in the third aspect of the present application or the perovskite solar cell prepared by the method provided in the fourth aspect of the present application.

[0065] The embodiments of the present application are described in detail below. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific technology or conditions are indicated in the embodiments, the technology or conditions described in the document in this area or the product specification are used. The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained commercially.

[0066] Example 1

[0067] 1. Preparation of ionic liquids

[0068] Under nitrogen protection, 4-(bromomethyl)thiopheneboronic acid (440 mg, 2 mmol) in a double-necked flask was dissolved in ethyl acetate (15 mL). Subsequently, 1-vinyl imidazole (0.226 mL, 2.5 mmol) was added to the above solution and refluxed at 70°C for 24 hours. After the reaction was completed, the unreacted reactants were washed with ethyl acetate and vacuum dried at 45°C for 12 hours to obtain ionic liquid IL-1 (508 mg, 1.6 mmol) with a yield of 81%.

[0069]

[0070] 1 H NMR (500 MHz, Chloroform- d ) δ 9.88 (t, J = 1.7 Hz, 1H), 7.85 (dd, J =1.8, 2.8 Hz, 1H), 7.79 (dd, J = 1.7, 2.7 Hz, 1H), 7.56 (d, J = 7.1 Hz, 1H), 7.23(t, J = 9.1 Hz, 1H), 6.94 (d, J = 7.1 Hz, 1H), 6.07 (s, 2H), 5.11 (dd, J= 2.0, 9.2Hz, 1H), 4.98 (dd, J = 2.1, 9.1 Hz, 1H). HRMS (ESI / Q-TOF, m / z): Calcd for [M-Br - ] + C 10 H 12 BN2O2S + : 235.0707, found: 235.0699.

[0071] 2. Preparation of perovskite solar cells

[0072] The TCO conductive glass was ultrasonically cleaned with deionized water, acetone and isopropanol for 15 minutes respectively, and finally dried in a drying oven at 75°C for later use; the dried TCO conductive glass substrate was placed in a UV ozone machine for 5 minutes to remove organic impurities on its surface and optimize its surface wettability;

[0073] Dissolve 1 mg of [2-(9H-carbazole-9-yl)ethyl]phosphoric acid in 1 mL of ethanol and stir at room temperature until completely dissolved to obtain an organic hole transport material solution; take 30 μL of the organic hole transport material solution, drop it on the treated TCO conductive glass, spin coat it at 5000 rpm for 30 s, and place the TCO conductive glass coated with the hole transport material on a hot stage for heating and annealing at 100°C for 10 min to form a hole transport layer;

[0074] Dissolve 722.08 mg of lead iodide, 238.50 mg of iodomethylamine and ionic liquid IL-1 in 1 mL of N, N-dimethylformamide (DMF), and stir at room temperature until completely dissolved to obtain a perovskite precursor solution. The mass proportion of the ionic liquid is 1.5 mg / mL.

[0075] In a nitrogen glove box, 30 μL of perovskite precursor solution was added dropwise to the TCO conductive glass that formed the hole transport layer. The solution was first spin-coated at 1000 rpm for 10 s and then at 5000 rpm for 30 s. During this process, 125 μL of chlorobenzene was quickly added dropwise after 25 s. The TCO conductive glass was then placed on a hot stage and heated and annealed at 100 °C for 40 min to form a perovskite layer.

[0076] 20 mg of methanefullerene phenyl-C 61 -Butyric acid-methyl ester (PCBM) was dissolved in 1 mL of chlorobenzene and stirred at room temperature to obtain [6,6]-phenyl-C 61 -Methyl butyrate solution;

[0077] Take 30 μL [6,6]-phenyl-C61 -Methyl butyrate solution was added dropwise onto the TCO conductive glass with the perovskite layer formed thereon, and spin-coated at 3000 rpm for 60 s to form an electron transport layer;

[0078] Dissolve 0.5 mg of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP) in 1 mL of isopropanol and stir at room temperature to obtain a hole blocking layer solution; take 40 μL of the hole blocking layer solution and drop it onto the electron transport layer, and spin-coat at 5000 rpm for 35 s to form a hole blocking layer;

[0079] The TCO conductive glass with hole blocking layer, electron transport layer, perovskite layer and hole transport layer was transferred to the vacuum coating instrument and the vacuum degree was drawn to 3×10 -4 A silver electrode was evaporated at 100 nm in thickness to obtain an electrode layer.

[0080] Example 2

[0081] The preparation method of the perovskite solar cell is the same as that of Example 1, except that the preparation method of the ionic liquid is:

[0082] Under nitrogen protection, 4-(bromomethyl)-2-fluorophenylboronic acid (464 mg, 2 mmol) in a double-necked flask was dissolved in ethyl acetate (15 mL). Subsequently, 1-vinyl imidazole (0.226 mL, 2.5 mmol) was added to the above solution and refluxed at 70°C for 24 hours. After the reaction was completed, the unreacted reactants were washed with ethyl acetate and vacuum dried at 45°C for 12 hours to obtain the ionic liquid IL-2 (580 mg, 1.8 mmol) with a yield of 89%.

[0083]

[0084] 1 H NMR (500 MHz, Chloroform- d ) δ 7.82 (dt, J = 1.5, 3.0 Hz, 2H), 7.66(dd, J = 4.9, 8.4 Hz, 1H), 7.61 (s, 1H), 7.23 (t, J = 14.5 Hz, 1H), 7.05 (dq, J =1.1, 8.4 Hz, 1H), 6.80 (dq, J = 1.1, 8.1 Hz, 1H), 6.05 (t, J= 1.0 Hz, 2H), 5.21(dd, J = 2.0, 14.7 Hz, 1H), 4.98 (dd, J = 2.0, 14.5 Hz, 1H). HRMS (ESI / Q-TOF, m / z): Calcd for [M-Br - ] + C 12 H 13 BFN2O2 + : 247.1049, found: 247.1053.

[0085] Example 3

[0086] The preparation method of the perovskite solar cell is the same as that of Example 1, except that the preparation method of the ionic liquid is:

[0087] Under nitrogen protection, 4-(bromomethyl)-2-fluorophenylboronic acid (500 mg, 2 mmol) in a double-necked flask was dissolved in ethyl acetate (15 mL). Subsequently, 1-vinyl imidazole (0.226 mL, 2.5 mmol) was added to the above solution and refluxed at 70°C for 24 hours. After the reaction was completed, the unreacted reactants were washed with ethyl acetate and vacuum dried at 45°C for 12 hours to obtain the ionic liquid IL-3 (480 mg, 1.4 mmol) with a yield of 71%.

[0088]

[0089] 1 H NMR (500 MHz, Chloroform- d ) δ 7.85 – 7.79 (m, 2H), 7.52 (s, 2H),7.27 – 7.18 (m, 2H), 6.85 (ddt, J = 0.9, 4.9, 7.9 Hz, 1H), 6.07 (d, J = 1.0 Hz,2H), 5.21 (dd, J = 2.0, 14.6 Hz, 1H), 4.98 (dd, J = 2.0, 14.5 Hz, 1H). HRMS (ESI / Q-TOF, m / z): Calcd for [M-Br - ] + C 12 H 12 BF2N2O2+ : 265.0954, found: 265.0950.

[0090] Example 4

[0091] The preparation method of the perovskite solar cell is the same as that of Example 1, and the preparation method of the ionic liquid is the same as that of Example 2, except that the raw material 4-(bromomethyl)-2-fluorophenylboric acid is replaced by The obtained ionic liquid IL-4 is .

[0092] 1 H NMR (500 MHz, Chloroform- d ) δ 9.63 (t, J = 1.7 Hz, 1H), 8.50 (dd, J =2.5, 1.7 Hz, 1H), 7.88 – 7.83 (m, 1H), 7.75 (s, 2H), 7.22 (t, J = 9.1 Hz, 1H),5.11 (dd, J = 9.2, 2.0 Hz, 1H), 4.98 (dd, J = 9.1, 2.1 Hz, 1H), 4.41 (ddd, J = 7.4,5.1, 2.4 Hz, 2H), 4.32 (dd, J = 5.2, 2.4 Hz, 2H). HRMS (ESI / Q-TOF, m / z): Calcdfor [M-Br - ] + C 11 H 12 BN2O4S + : 279.0605, found: 279.0601.

[0093] Example 5

[0094] The preparation method of the perovskite solar cell is the same as that of Example 1, and the preparation method of the ionic liquid is the same as that of Example 2, except that the raw material 4-(bromomethyl)-2-fluorophenylboric acid is replaced by The obtained ionic liquid IL-5 is .

[0095] 1 H NMR (500 MHz, Chloroform- d ) δ 8.90 (dd, J= 2.9, 1.6 Hz, 2H), 7.90(dd, J = 3.1, 1.7 Hz, 1H), 7.66 (d, J = 10.1 Hz, 1H), 7.33 (s, 2H), 7.27 (d, J =10.1 Hz, 1H), 7.21 (t, J = 9.1 Hz, 1H), 5.11 (dd, J = 9.2, 2.0 Hz, 1H), 4.98 (dd, J = 9.1, 2.1 Hz, 1H). HRMS (ESI / Q-TOF, m / z): Calcd for [M-Br - ] + C 11 H 10 BN4O2S + :273.0612, found: 273.0604.

[0096] Example 6

[0097] The preparation method of the perovskite solar cell is the same as that of Example 1, and the preparation method of the ionic liquid is the same as that of Example 2, except that the raw material 4-(bromomethyl)-2-fluorophenylboric acid is replaced by The obtained ionic liquid IL-6 is .

[0098] 1 H NMR (500 MHz, Chloroform- d ) δ 9.97 (d, J = 1.8 Hz, 1H), 8.78 (dd, J =2.5, 1.7 Hz, 1H), 8.23 ​​(s, 1H), 7.89 (dd, J = 2.5, 1.7 Hz, 1H), 7.25 – 7.18 (m,2H), 6.97 (s, 2H), 5.11 (dd, J = 9.2, 2.0 Hz, 1H), 4.98 (dd, J = 9.1, 2.1 Hz,1H). HRMS (ESI / Q-TOF, m / z): Calcd for [M-Br - ] + C 11 H 10 BN2O2S2+ : 273.0271, found:273.0265.

[0099] Example 7

[0100] The preparation method of the perovskite solar cell is the same as that of Example 1, and the preparation method of the ionic liquid is the same as that of Example 2, except that the raw material 4-(bromomethyl)-2-fluorophenylboric acid is replaced by The obtained ionic liquid IL-7 is .

[0101] 1 H NMR (500 MHz, Chloroform- d ) δ 9.97 (t, J = 1.8 Hz, 1H), 8.78 (dd, J =2.5, 1.7 Hz, 1H), 8.41 (s, 1H), 7.92 – 7.88 (m, 1H), 7.22 (t, J = 9.1 Hz, 1H), 7.07 (s, 1H), 6.99 (s, 2H), 5.11 (dd, J = 9.2, 2.0 Hz, 1H), 4.98 (dd, J = 9.1,2.1 Hz, 1H). HRMS (ESI / Q-TOF, m / z): Calcd for [M-Br - ] + C 13 H 10 BN2O2S3 + : 332.9992,found: 332.9995.

[0102] Example 8

[0103] The preparation method of the perovskite solar cell is the same as that of Example 1, and the preparation method of the ionic liquid is the same as that of Example 2, except that the raw material 4-(bromomethyl)-2-fluorophenylboric acid is replaced by The obtained ionic liquid IL-8 is .

[0104] 1 H NMR (500 MHz, Chloroform- d ) δ 8.53 (dd, J = 2.9, 1.6 Hz, 1H), 7.89(dd, J= 3.0, 1.7 Hz, 1H), 7.85 (s, 3H), 7.28 (s, 2H), 7.20 (t, J = 9.1 Hz, 1H),5.11 (dd, J = 9.2, 2.0 Hz, 1H), 4.98 (dd, J = 9.1, 2.1 Hz, 1H). HRMS (ESI / Q-TOF,m / z): Calcd for [M-Br - ] + C 11 H 12 N2O3P + : 251.0580, found: 251.0577.

[0105] Comparative Example 1

[0106] Making perovskite solar cells

[0107] The TCO conductive glass was ultrasonically cleaned with deionized water, acetone and isopropanol for 15 minutes respectively, and finally dried in a drying oven at 75°C for later use; the dried TCO conductive glass substrate was placed in a UV ozone machine for 5 minutes to remove organic impurities on its surface and optimize its surface wettability;

[0108] Dissolve 1 mg of [2-(9H-carbazole-9-yl)ethyl]phosphoric acid in 1 mL of ethanol and stir at room temperature until completely dissolved to obtain an organic hole transport material solution; take 30 μL of the organic hole transport material solution, drop it on the treated TCO conductive glass, spin coat it at 5000 rpm for 30 s, and place the TCO conductive glass coated with the hole transport material on a hot stage for heating and annealing at 100°C for 10 min to form a hole transport layer;

[0109] Dissolve 722.08 mg of lead iodide and 238.50 mg of iodomethylamine in 1 mL of N, N-dimethylformamide (DMF) and stir at room temperature until completely dissolved to obtain a perovskite precursor solution;

[0110] In a nitrogen glove box, 30 μL of perovskite precursor solution was added dropwise to the TCO conductive glass that formed the hole transport layer. The solution was first spin-coated at 1000 rpm for 10 s and then at 5000 rpm for 30 s. During this process, 125 μL of chlorobenzene was quickly added dropwise after 25 s. The TCO conductive glass was then placed on a hot stage and heated and annealed at 100 °C for 40 min to form a perovskite layer.

[0111] 20 mg of methanefullerene phenyl-C 61-Butyric acid-methyl ester (PCBM) was dissolved in 1 mL of chlorobenzene and stirred at room temperature to obtain [6,6]-phenyl-C 61 -Methyl butyrate solution;

[0112] Take 30 μL [6,6]-phenyl-C 61 -Methyl butyrate solution was added dropwise onto the TCO conductive glass with the perovskite layer formed thereon, and spin-coated at 3000 rpm for 60 s to form an electron transport layer;

[0113] Dissolve 0.5 mg of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP) in 1 mL of isopropanol and stir at room temperature to obtain a hole blocking layer solution; take 40 μL of the hole blocking layer solution and drop it onto the electron transport layer, and spin-coat at 5000 rpm for 35 s to form a hole blocking layer;

[0114] The TCO conductive glass with hole blocking layer, electron transport layer, perovskite layer and hole transport layer was transferred to the vacuum coating instrument and the vacuum degree was drawn to 3×10 -4 A silver electrode was evaporated at 100 nm in thickness to obtain an electrode layer.

[0115] Performance Testing

[0116] 1. Test methods for short-circuit current (Jsc), open-circuit voltage (Voc), fill factor (FF) and photoelectric conversion efficiency (Eff): GB 11009-1989 is used for solar cell spectral response test, GB 12632-1990 is used for single crystal cell test, and GBT 6495.1-1996 is used for photovoltaic current-voltage characteristic test of solar cells. The specific conditions are 25°C, AM1.5G spectrum, 1000 W / cm 2 Light intensity polarity test.

[0117] 2. Stability test method: ISOS-L-2 is used for maximum power point tracking (MPPT) to test the stability of solar cells. The specific conditions are 85°C, AM1.5 G spectrum, 100 mW / cm 2 Light intensity.

[0118] The test results of the perovskite solar cells in Examples 1 to 8 and Comparative Example 1 are shown in Table 1.

[0119] Table 1

[0120]

[0121] Conclusion: Compared with Comparative Example 1, the perovskite solar cells prepared in Examples 1-8 have higher open circuit voltage, short circuit current, fill factor and photoelectric conversion efficiency, and have excellent high temperature stability, indicating that the present application can improve the quality of the perovskite layer and improve the stability of the perovskite layer under high temperature conditions by adding ionic liquids to the perovskite layer.

[0122] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. An ionic liquid, It is characterized in that include: , Among them, R 1 is an alkyl chain of 1 to 18 carbon atoms; R 2 -COOH, -B(OH) 2 、-PO(OH) 2 , -CF 3 、-NH 2 、-SO 3 At least one of H; Ar Formula 1, Formula 2: Formula 3, Formula 4: Formula 5, Formula 6, Formula 7, At least one of Formula 8.

2. The ionic liquid according to claim 1, It is characterized in that R 2 -B(OH) 2 or -PO(OH) 2 At least one of .

3. The ionic liquid according to claim 2, It is characterized in that Satisfy at least one of the following conditions: (1) R 1 is one of the alkyl chains of 1 to 4 carbon atoms; (2) Ar is Formula 1.

4. A method for preparing the ionic liquid according to any one of claims 1 to 3, It is characterized in that include: Vinyl imidazole, R 2 -Ar-R 1 -Br and a solvent are mixed, heated to reflux, and dried to obtain the ionic liquid.

5. The method according to claim 4, It is characterized in that The vinyl imidazole and the R 2 -Ar-R 1 The molar ratio of -Br is 1:(1.1-2).

6. The method according to claim 5, It is characterized in that The vinyl imidazole and the R 2 -Ar-R 1 The molar ratio of -Br is 1:(1.1-1.5).

7. The method according to claim 4, It is characterized in that The heating reflux temperature is 50°C-70°C, and the heating reflux time is 12h-24h.

8. A perovskite solar cell, It is characterized in that include: substrate; A perovskite layer, wherein the perovskite layer is disposed on one side of the substrate, the perovskite layer comprises a perovskite material and an additive, wherein the additive comprises the ionic liquid according to any one of claims 1 to 3 and a polymer formed by the ionic liquid; An electrode layer is disposed on a side of the perovskite layer away from the substrate.

9. The perovskite solar cell according to claim 8, It is characterized in that The molar ratio of the additive to the perovskite material is (1-10):

150.

10. The perovskite solar cell according to claim 9, It is characterized in that The molar ratio of the additive to the perovskite material is (3-5):

150.

11. The perovskite solar cell according to claim 9, It is characterized in that The perovskite solar cell further comprises: a hole transport layer, the hole transport layer being located between the substrate and the perovskite layer; An electron transport layer, the electron transport layer being located on a side of the perovskite layer away from the hole transport layer; A hole blocking layer is provided, wherein the hole blocking layer is located on a side of the electron transport layer away from the perovskite layer, and the electrode layer is located on a side of the hole blocking layer away from the electron transport layer.

12. The perovskite solar cell according to claim 11, It is characterized in that Satisfy at least one of the following conditions: The perovskite material is ABX 3 , where A is Cs + 、MA + (CH 3 NH 3 + ), FA + (CH(NH 2 ) 2 + ), Rb + At least one of the following, B is Pb 2+ Sn 2+ , Mn 2+ At least one of, X is at least one of the halogen ions; The material forming the hole transport layer is at least one of [2-(9H-carbazole-9-yl)ethyl]phosphoric acid, [4-(9H-carbazole-9-yl)butyl]phosphoric acid, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid, [2-(3,6-dimethyl-9H-carbazole-9-yl)ethyl]phosphoric acid, [2-(3,6-di-tert-butyl-9H-carbazole-9-yl)ethyl]phosphoric acid, [4-(3,6-dibromo-9H-carbazole-9-yl)butyl]phosphoric acid, poly[bis(4-phenyl) (2,4,6-trimethylphenyl)amine], poly(3-hexylthiophene-2,5-diyl), and polyethylenedioxythiophene-poly(styrene sulfonate); The material forming the electron transport layer is [6,6]-phenyl-C 61 -Methyl butyrate, C 60 , at least one of tin oxide; The material forming the hole blocking layer is at least one of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline or zirconium acetylacetonate; The material forming the electrode layer is at least one of silver, copper, oxide and carbon electrode.

13. A method for preparing the perovskite solar cell according to any one of claims 8 to 12, It is characterized in that include: Mixing an ionic liquid, an A source, a B source, an X source, and a solvent to form a precursor solution, forming the precursor solution on one side of the substrate, and heating and annealing to form the perovskite layer; An electrode layer is formed on a side of the perovskite layer away from the substrate.

14. The method according to claim 13, It is characterized in that The mass proportion of the ionic liquid in the precursor solution is 0.5 mg / mL-3 mg / mL.

15. The method according to claim 13, It is characterized in that The temperature of the heating annealing is 100° C.-150° C., and the time of the heating annealing is 30 min-40 min.

16. The method according to claim 13, It is characterized in that Also includes: forming a hole transport layer between the substrate and the perovskite layer; forming an electron transport layer on a side of the perovskite layer away from the hole transport layer; forming a hole blocking layer on a side of the electron transport layer away from the perovskite layer; The electrode layer is formed on a side of the hole blocking layer away from the electron transport layer.

17. A photovoltaic module, It is characterized in that A perovskite solar cell comprising the perovskite solar cell described in any one of claims 8 to 12 or a perovskite solar cell prepared by the method described in any one of claims 13 to 16.