A TOPCon battery structure and preparation method thereof

By introducing inorganic oxide layer and laser groove technology into TOPCon cells, the problem of reduced light absorption and interface defects caused by the thickness of the doped polysilicon layer is solved, the current and light absorption rate are increased, and the production cost is reduced.

CN118380497BActive Publication Date: 2024-10-22HUAIAN JIETAI NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410806978.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-22
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

The thicker doped polysilicon layer in TOPCon cells causes parasitic absorption to reduce light absorption, and the interface defect density of the doped polysilicon film is large, resulting in serious minority carrier recombination.

Method used

An inorganic oxide layer is introduced between the doped polysilicon layer and the back anti-reflection layer, and local contact is formed through laser grooving to improve the passivation effect, reduce minority carrier recombination on the surface of the polysilicon film, and reduce the thickness of the doped polysilicon layer.

Benefits of technology

The parasitic absorption is improved, the light absorption rate is increased, the production cost is reduced, and the current and passivation quality are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118380497B_ABST
    Figure CN118380497B_ABST
Patent Text Reader

Abstract

The invention discloses a TOPCon cell structure and a preparation method thereof, belonging to the field of TOPCon cells, comprising a silicon substrate, wherein the front side of the substrate is sequentially composed of a p+ emitter, an aluminum oxide dielectric layer, a front anti-reflection layer and a front conductive metal electrode from the inside to the outside; and the back side of the substrate is sequentially composed of an ultra-thin tunneling oxide layer, a back doped polysilicon layer, an oxide dielectric layer, a back anti-reflection layer and a back conductive metal electrode from the inside to the outside. The beneficial effects of the invention are as follows: an inorganic oxide layer is introduced between the doped polysilicon layer and the back anti-reflection layer, which has a field passivation effect on the doped polysilicon layer, and local contact is formed by laser grooving, so that phosphorus or boron can be further doped into the polysilicon layer to improve the passivation effect, and the oxide layer can reduce the minority carrier recombination on the surface of the polysilicon film; at the same time, the thickness of the doped polysilicon layer can be reduced, which is beneficial to the increase of current.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of TOPCon batteries, and in particular to a TOPCon battery structure and a preparation method thereof. Background Art

[0002] A solar cell is a device that converts solar energy directly into electrical energy. Its working principle is based on the photovoltaic effect. Among them, TOPCon solar cells are highly efficient solar cells. Their characteristics are that they passivate the back surface field by forming an ultra-thin oxide layer and a doped polysilicon layer on the back of the silicon wafer, thereby improving the conversion efficiency of the cell.

[0003] The structure of the current mass-produced TOPCon cell includes an n-type silicon substrate, a pn junction, a front anti-reflection layer, and a conductive metal electrode on the front side from the inside out, and an ultra-thin tunneling oxide layer, a doped polysilicon layer, a back anti-reflection layer, and a conductive metal electrode on the back side from the inside out. The structure of the tunneling oxide layer / doped polysilicon layer allows the majority carriers to be transmitted to the doped polysilicon layer while the minority carriers are basically blocked by the tunneling oxide layer. Therefore, there is basically no loss of metal-semiconductor recombination when the metal electrode and the doped polysilicon layer are in contact, which greatly improves the open circuit voltage of the solar cell. However, the disadvantage is that in order to achieve the passivation effect, the thickness of the doped polysilicon layer is between 100-200nm, which will produce parasitic absorption and reduce light absorption. In addition, the defect density at the interface of the doped polysilicon film is large, and the minority carrier recombination is more serious.

[0004] In view of this, the inventor conducted in-depth research on this demand, and thus the present case was produced. Summary of the invention

[0005] In view of the problems that the thickness of the doped polysilicon layer in the TOPCon cell in the prior art is large, which will produce parasitic absorption and reduce light absorption, and the defect density at the interface of the doped polysilicon film is large, and the minority carrier recombination is serious, the present invention provides a TOPCon cell structure and a preparation method thereof, by introducing an inorganic oxide layer between the doped polysilicon layer and the back anti-reflection layer, and forming a local contact by laser grooving, a certain field passivation effect is achieved, thereby improving the passivation quality of the TOPCon structure. The specific technical scheme is as follows:

[0006] A TOPCon cell structure includes a silicon substrate, wherein the front side of the substrate is composed of a p+ emitter, an aluminum oxide dielectric layer, a front anti-reflection layer, and a front conductive metal electrode from the inside to the outside; and the back side of the substrate is composed of an ultra-thin tunneling oxide layer, a back doped polysilicon layer, an oxide dielectric layer, a back anti-reflection layer, and a back conductive metal electrode from the inside to the outside.

[0007] The back conductive metal electrode penetrates the back anti-reflection layer and contacts the oxidized dielectric layer; the front conductive metal electrode penetrates the front anti-reflection layer and the aluminum oxide dielectric layer and contacts the p+ emitter.

[0008] An inorganic oxide layer is introduced between the doped polysilicon layer and the back anti-reflection layer to have a field passivation effect on the doped polysilicon layer, reduce the minority carrier recombination on the surface of the polysilicon film, and at the same time reduce the thickness of the doped polysilicon layer, which is beneficial to the increase of current.

[0009] Preferably, the thickness of the back doped polysilicon layer is 30-90nm, preferably 40-70nm, the thickness of the oxidizing medium layer is 20-50nm, the thickness of the oxidizing medium layer is preferably 30-40nm, and the sum of the thicknesses of the back doped polysilicon layer and the oxidizing medium layer is not less than 60nm. Here, the thickness of the back doped polysilicon layer is reduced from 100-200nm to 30-90nm, and the combination of the back doped polysilicon layer and the oxidizing medium layer not only improves parasitic absorption, increases light absorption rate, reduces production costs, but also has a good passivation effect.

[0010] Preferably, the silicon substrate is an N-type silicon substrate, the back-doped polysilicon layer is phosphorus-doped polysilicon, and the oxide dielectric layer is a phosphorus oxide dielectric layer.

[0011] Preferably, the silicon substrate is a P-type silicon substrate, the back-doped polysilicon layer is boron-doped polysilicon, and the oxide dielectric layer is a boron oxide dielectric layer.

[0012] Preferably, the thickness of the front anti-reflection layer is 70-120nm, the comprehensive refractive index is 1.9-2.1, and the refractive index of the film layer decreases in the direction away from the silicon substrate; the thickness of the back anti-reflection layer is 70-120nm, the comprehensive refractive index is 1.9-2.1, and the refractive index of the film layer decreases in the direction away from the silicon substrate. The front anti-reflection layer and the back anti-reflection layer are one or more combinations of SiNx, SiOxNy, and SiOx, preferably SiNx thin film.

[0013] Preferably, the thickness of the aluminum oxide dielectric layer is 3-5nm, and the thickness of the p+ emitter is 0.5-0.8µm. The p+ emitter preferably includes a heavily doped region with low square resistance located in the metal contact area and a lightly doped region with high square resistance located in the non-metal contact area, and the junction depth of the lightly doped region is less than or equal to 0.4µm, and the surface concentration is 9E+18 cm -3 , while the junction depth of the heavily doped region is less than or equal to 0.6µm, and the surface doping concentration is 5E+18 cm -3 .

[0014] Preferably, the ultra-thin tunneling oxide layer has a thickness of 1-3 nm.

[0015] Preferably, the front conductive metal electrode is an Ag / Al gate line electrode, and the back conductive metal electrode is an Ag gate line electrode, and the widths of both electrodes are 22-25 μm.

[0016] The present invention also provides a method for preparing the TOPCon battery structure, comprising:

[0017] After the silicon substrate is textured, boron is diffused and laser doped to form a selective emitter;

[0018] An ultra-thin tunnel oxide layer and an intrinsic polysilicon layer are prepared on the back side by LPCVD process, and a back-doped polysilicon layer is prepared by phosphorus diffusion or boron diffusion;

[0019] An oxide dielectric layer is prepared on the surface of the back-doped polysilicon layer by atomic layer deposition, and then laser grooving is performed to form a local contact, and then an anti-reflection layer and a conductive metal electrode are prepared.

[0020] Preferably, the present invention also provides a method for preparing a TOPCon battery structure, comprising the following steps:

[0021] Step 1: Texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um;

[0022] Step 2: Boron diffusion and laser doping to form a selective emitter, using BCl3 or BBr3 as the boron source, diffusion temperature 900-1100℃, diffusion square resistance 100-300Ω / □, and forming a surface concentration of 9E+18 cm on the front of the silicon substrate. 3 Then, a continuous laser was used to locally dope the metal contact area on the surface of the silicon substrate. Through the thermal effect of the laser grooving, the boron atoms in the borosilicate glass were simultaneously pushed into the silicon wafer to form a local heavily doped area inside the silicon wafer. The surface concentration of the metal contact area of ​​the borosilicate glass film was reduced to 5E+18 cm -3 , the junction depth is pushed to 0.6 µm, the laser power is preferably 20-45W, and the wavelength is 355-1064nm. The silicon substrate after laser doping is subjected to high temperature annealing, and after oxidation annealing, a p+ emitter is formed, which has a lightly doped region with high square resistance and a heavily doped region with low square resistance; the lightly doped region is located in the non-metallic contact region, and the heavily doped region is located in the metal contact region.

[0023] Step 3: Single-sided HF etching to remove the back BSG;

[0024] Step 4: Etch the back side doping layer, use the front BSG as a barrier layer, and use an alkaline solution to etch and remove the back side doping layer;

[0025] Step 5, depositing a tunnel oxide layer and an intrinsic polysilicon layer. First, in an LPCVD furnace tube, using O2 as an oxidant and an oxidation temperature of 550-650° C., an in-situ oxidation growth tunnel oxide layer is performed on the back of the silicon wafer. Second, after the growth of the tunnel oxide layer is completed, SiH4 is used as a reaction gas and N2 is used as a diluent gas at a deposition temperature of 550-650° C. to continue to use LPCVD technology to deposit an intrinsic polysilicon film on the surface of the tunnel oxide layer.

[0026] Step 6: Phosphorus diffusion, using POCl3 as the diffusion source, the diffusion temperature is 800-900℃, and the intrinsic polysilicon layer is doped with n-type phosphorus, with a doping concentration of 1~5E20cm -3 , forming a back-doped polysilicon layer;

[0027] Step 7: single-sided HF etching to remove PSG on the surface of the front polysilicon layer after diffusion;

[0028] Step 8: etching the front side polysilicon, using alkaline solution to remove the polysilicon layer on the front BSG surface, and using hydrofluoric acid to remove the front BSG and the back PSG;

[0029] Step nine, alternately introducing a first precursor and a second precursor oxygen source into the process chamber, wherein the first precursor is a phosphorus-containing precursor; after the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to generate an oxide, and this is repeated to form an oxidizing medium layer of a desired thickness; wherein the phosphorus-containing precursor includes but is not limited to trimethyl phosphate, triethyl phosphate, etc.; the second precursor oxygen source is used to react with the first precursor to generate an oxidizing medium layer, including but not limited to oxygen, ozone, laughing gas N2O, etc.

[0030] The metal contact area on the surface of the oxide medium layer is grooved by laser, with a laser pulse width range of 1-1000ns, a power range of 1%-100%, a frequency range of 100-3000kHz, and a laser scanning speed range of 1-30000mm / s. The metal contact area on the surface of the oxide medium layer is grooved by adjusting the above parameters, with a power of preferably 40%-60%, a pulse width of 30-60 µs, a frequency of 500kHz, and a scanning speed of 30000mm / s. At this time, the light spots are tangent, and the surface damage of the oxide medium layer is low. The laser beam with a higher energy density is irradiated on the surface to produce melting, ablation and evaporation, thereby achieving the purpose of grooving.

[0031] Step 10, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition method, using TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5nm;

[0032] Step 11, depositing a front anti-reflection layer and a back anti-reflection layer, using a tubular or plate PECVD to deposit an anti-reflection layer on the front and back of the silicon wafer, wherein the anti-reflection layer is one or more combinations of SiNx, SiOxNy, and SiOx;

[0033] Step 12: print Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sinter to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; and inject light to repair defects inside and on the surface of the battery.

[0034] Preferably, the present invention also provides a method for preparing a TOPCon battery structure, comprising the following steps:

[0035] Step 1: Texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a boron-doped P-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um;

[0036] Step 2: Phosphorus diffusion and laser doping to form a selective emitter, using POCl3 as the phosphorus source, diffusion temperature 700-1000℃, diffusion square resistance 100-300Ω / □, and forming a doping concentration of 1E+20 cm on the front of the silicon substrate. 3 Then, a continuous laser is used to locally dope the metal contact area on the surface of the silicon substrate. Through the thermal effect of laser grooving, the phosphorus atoms in the phosphorus silicate glass are simultaneously pushed into the silicon wafer to form a local heavily doped area inside the silicon wafer. The laser power is preferably 20-45W and the wavelength is 355-1064nm. The laser-doped silicon substrate is subjected to high-temperature annealing, and an n+ emitter is formed after oxidation annealing, which has a lightly doped area with high square resistance and a heavily doped area with low square resistance; the lightly doped area is located in the non-metal contact area, and the heavily doped area is located in the metal contact area.

[0037] Step 3: single-sided HF etching to remove the back PSG;

[0038] Step 4: etching the back side doping layer, using the front PSG as a barrier layer, and using an alkaline solution to etch and remove the back side doping layer;

[0039] Step 5, depositing a tunnel oxide layer and an intrinsic polysilicon layer. First, in an LPCVD furnace tube, using O2 as an oxidant, the oxidation temperature is 550-650°C, and the tunnel oxide layer is in-situ oxidized and grown on the back of the silicon wafer. Secondly, after the growth of the tunnel oxide layer is completed, SiH4 is used as a reaction gas, N2 is used as a dilution gas, and the deposition temperature is 550-650°C. LPCVD technology is continued to be used to deposit an intrinsic polysilicon film on the surface of the tunnel oxide layer, and the thickness thereof is 100-150nm.

[0040] Step 6: Boron diffusion, using boron trichloride or boron tribromide as the boron diffusion source, and introducing nitrogen and oxygen as reaction gases; the flow rate of the boron source is 50-500sccm, the flow rate of nitrogen is 1000-10000sccm, and the flow rate of oxygen is 500-4000sccm; the intrinsic polysilicon layer is diffused with boron, and the square resistance after boron diffusion is 120-300ohm / sq, and the diffusion concentration is 7E19-1E20cm -3 , forming a back-doped polysilicon layer;

[0041] Step 7: etching the front side polysilicon, using alkaline solution to remove the polysilicon layer on the front BSG surface, and using hydrofluoric acid to remove the BSG on the front and back sides;

[0042] Step eight, alternately introducing a first precursor and a second precursor oxygen source into the process chamber, wherein the first precursor is a boron-containing precursor. After the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to generate an oxide, and this process is repeated to form an oxidizing medium layer of a desired thickness; the second precursor oxygen source is used to react with the first precursor to generate an oxidizing medium layer, including but not limited to oxygen, ozone, laughing gas N2O, etc.

[0043] The metal contact area on the surface of the oxide medium layer is grooved by laser, with a laser pulse width range of 1-1000ns, a power range of 1%-100%, a frequency range of 100-3000kHz, and a laser scanning speed range of 1-30000mm / s. The metal contact area on the surface of the oxide medium layer is grooved by adjusting the above parameters, with a power of preferably 40%-60%, a pulse width of 30-60 µs, a frequency of 500kHz, and a scanning speed of 30000mm / s. At this time, the light spots are tangent, and the surface damage of the oxide medium layer is low. The laser beam with a higher energy density is irradiated on the surface to produce melting, ablation and evaporation, thereby achieving the purpose of grooving.

[0044] Step nine, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition method, using TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5nm;

[0045] Step 10, depositing a front anti-reflection layer and a back anti-reflection layer, using tubular or plate PECVD to deposit anti-reflection layers on the front and back of the silicon wafer, wherein the anti-reflection layers are one or more combinations of SiNx, SiOxNy, and SiOx;

[0046] Step 11: print Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sinter to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; and inject light to repair defects inside and on the surface of the battery.

[0047] Beneficial effects:

[0048] The beneficial effects produced by the technical solution of the present invention are as follows:

[0049] (1) An inorganic oxide layer is introduced between the doped polysilicon layer and the back anti-reflection layer to achieve field passivation on the doped polysilicon layer. Local contact is formed by laser grooving, and phosphorus or boron can be further doped into the polysilicon layer to enhance the passivation effect. The oxide layer can also reduce minority carrier recombination on the surface of the polysilicon film. At the same time, the thickness of the doped polysilicon layer can be reduced, which is beneficial to the increase of current.

[0050] (2) A layer of phosphorus oxide or boron oxide with a thickness of 20-50 nm is deposited on the doped polysilicon by atomic layer deposition, and laser grooving is performed to form local contact to reduce the minority carrier recombination in the contact area between the metal and the semiconductor. At the same time, the positive charge it carries has a field passivation effect, effectively improving the minority carrier recombination on the surface of doped polysilicon, thereby improving the passivation quality of the TOPcon structure.

[0051] (3) The thickness of the back-doped polysilicon layer is reduced from the previous 100-200nm to 30-90nm. Its combination with the oxide dielectric layer not only improves parasitic absorption, increases light absorption rate, and reduces production costs, but also has a good passivation effect.

[0052] (4) Atomic layer deposition (ALD) is used to prepare an oxide dielectric layer, which has the same positive charge as the minority carriers in the doped polysilicon layer and can play a field passivation role, reducing surface minority carrier recombination.

[0053] (5) Laser grooving of the phosphorus oxide film extends the concept of selective contact to the oxide dielectric layer and doped polysilicon layer, which can achieve higher conductivity in the contact area, reduce contact resistance, and achieve higher efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0055] Figure 1 Schematic diagram of the TOPCon solar cell layer structure in the present invention

[0056] Figure 2 is a process flow chart for preparing an N-type TOPCon solar cell structure in the present invention;

[0057] Figure 3 It is a process flow chart of the preparation process of the P-type TOPCon solar cell structure in the present invention. DETAILED DESCRIPTION

[0058] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0059] In this embodiment, an inorganic oxide layer is introduced between the doped polysilicon layer and the back anti-reflection layer to play a field passivation effect on the doped polysilicon layer, and local contact is formed by laser grooving, phosphorus or boron can be further doped into the polysilicon layer to improve the passivation effect, and the oxide layer can reduce the minority carrier recombination on the surface of the polysilicon film; at the same time, the thickness of the doped polysilicon layer can be reduced, which is conducive to the increase of current. The specific implementation is as follows:

[0060] like Figure 1 As shown, a TOPCon cell structure includes a silicon substrate 1, on the front side of which, from inside to outside, are a p+ emitter 2, an aluminum oxide dielectric layer 3, a front anti-reflection layer 4, and a front conductive metal electrode 5; on the back side of which, from inside to outside, are an ultra-thin tunneling oxide layer 6, a back doped polysilicon layer 7, an oxide dielectric layer 8, a back anti-reflection layer 9, and a back conductive metal electrode 10;

[0061] The back conductive metal electrode 10 penetrates the back anti-reflection layer 9 and contacts the oxide dielectric layer 8 ; the front conductive metal electrode 5 penetrates the front anti-reflection layer 4 and the aluminum oxide dielectric layer 3 and contacts the p+ emitter 2 .

[0062] An inorganic oxide layer is introduced between the doped polysilicon layer and the back anti-reflection layer to have a field passivation effect on the doped polysilicon layer, reduce the minority carrier recombination on the surface of the polysilicon film, and at the same time reduce the thickness of the doped polysilicon layer, which is beneficial to the increase of current.

[0063] As a preferred embodiment, the thickness of the back doped polysilicon layer is 30-90nm, preferably 40-70nm, the thickness of the oxidizing medium layer is 20-50nm, the thickness of the oxidizing medium layer is preferably 30-40nm, and the sum of the thicknesses of the back doped polysilicon layer and the oxidizing medium layer is not less than 60nm. Here, the thickness of the back doped polysilicon layer is reduced from 100-200nm to 30-90nm, and the combination of the back doped polysilicon layer and the oxidizing medium layer not only improves parasitic absorption, increases light absorption rate, reduces production costs, but also has a good passivation effect.

[0064] As a preferred implementation, the silicon substrate is an N-type silicon substrate, the back-doped polysilicon layer is phosphorus-doped polysilicon, and the oxide dielectric layer is a phosphorus oxide dielectric layer.

[0065] As a preferred implementation, the silicon substrate is a P-type silicon substrate, the back-doped polysilicon layer is boron-doped polysilicon, and the oxide dielectric layer is a boron oxide dielectric layer.

[0066] As a preferred embodiment, the thickness of the front anti-reflection layer is 70-120nm, the comprehensive refractive index is 1.9-2.1, and the refractive index of the film layer decreases in the direction away from the silicon substrate; the thickness of the back anti-reflection layer is 70-120nm, the comprehensive refractive index is 1.9-2.1, and the refractive index of the film layer decreases in the direction away from the silicon substrate. The front anti-reflection layer and the back anti-reflection layer are one or more combinations of SiNx, SiOxNy, and SiOx, preferably SiNx thin film.

[0067] As a preferred embodiment, the thickness of the aluminum oxide dielectric layer is 3-5nm, and the thickness of the p+ emitter is 0.5-0.8µm. The p+ emitter preferably includes a heavily doped region with low square resistance located in the metal contact area and a lightly doped region with high square resistance located in the non-metal contact area, and the junction depth of the lightly doped region is less than or equal to 0.4µm, and the surface concentration is 9E+18 cm 3 , while the junction depth of the heavily doped region is less than or equal to 0.6µm, and the surface doping concentration is 5E+18 cm 3.

[0068] As a preferred implementation, the thickness of the ultra-thin tunneling oxide layer is 1-3 nm.

[0069] As a preferred implementation, the front conductive metal electrode is an Ag / Al gate line electrode, and the back conductive metal electrode is an Ag gate line electrode, and the widths of both electrodes are 22-25 µm.

[0070] This embodiment also provides a method for preparing the TOPCon battery structure, including:

[0071] After the silicon substrate is textured, boron is diffused and laser doped to form a selective emitter;

[0072] An ultra-thin tunnel oxide layer and an intrinsic polysilicon layer are prepared on the back side by LPCVD process, and a back-doped polysilicon layer is prepared by phosphorus diffusion or boron diffusion;

[0073] An oxide dielectric layer is prepared on the surface of the back-doped polysilicon layer by atomic layer deposition, and then laser grooving is performed to form a local contact, and then an anti-reflection layer and a conductive metal electrode are prepared.

[0074] As a preferred embodiment, this embodiment also provides a method for preparing a TOPCon battery structure, such as Figure 2 As shown, the following steps are included:

[0075] Step S101, texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um;

[0076] Step S102, boron diffusion and laser doping to form a selective emitter, using BCl3 or BBr3 as a boron source, diffusion temperature 900-1100°C, diffusion square resistance 100-300Ω / □, forming a surface concentration of 9E+18 cm on the front of the silicon substrate 3 A borosilicate glass film is formed; then a continuous laser is used to locally dope the metal contact area on the surface of the silicon substrate. Through the thermal effect of laser grooving, the boron atoms in the borosilicate glass are simultaneously pushed into the silicon wafer to form a local heavily doped area inside the silicon wafer. The laser power is preferably 20-45W and the wavelength is 355-1064nm. The laser-doped silicon substrate is subjected to high-temperature annealing, and after oxidation annealing, a p+ emitter is formed, which has a lightly doped area with high square resistance and a heavily doped area with low square resistance; the lightly doped area is located in the non-metallic contact area, and the heavily doped area is located in the metal contact area.

[0077] Step S103, single-side HF etching to remove backside BSG;

[0078] Step S104, etching the back side doping layer, using the front side BSG as a barrier layer, and using an alkaline solution to etch and remove the back side doping layer;

[0079] Step S105, depositing a tunnel oxide layer and an intrinsic polysilicon layer, first, in an LPCVD furnace tube, using O2 as an oxidant, the oxidation temperature is 550-650° C., and the tunnel oxide layer is in-situ oxidized and grown on the back of the silicon wafer. Secondly, after the growth of the tunnel oxide layer is completed, SiH4 is used as a reaction gas, N2 is used as a diluent gas, and the deposition temperature is 550-650° C., and the intrinsic polysilicon film is continuously deposited on the surface of the tunnel oxide layer using the LPCVD technology;

[0080] Step S106: Phosphorus diffusion, using POCl3 as the diffusion source, the diffusion temperature is 800-900°C, and the intrinsic polysilicon layer is doped with n-type phosphorus, with a doping concentration of 1~5E20cm -3 , forming a back-doped polysilicon layer;

[0081] Step S107, single-sided HF etching to remove PSG on the surface of the front-side plated polysilicon layer after diffusion;

[0082] Step S108, etching the front side polysilicon, using alkaline solution to etch away the polysilicon layer on the front BSG surface, and using hydrofluoric acid to clean and remove the front BSG and the back PSG;

[0083] Step S109, alternately introducing a first precursor and a second precursor oxygen source into the process chamber, wherein the first precursor is a phosphorus-containing precursor; after the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to generate an oxide, and this is repeated to form an oxidizing medium layer of a desired thickness; wherein the phosphorus-containing precursor includes but is not limited to trimethyl phosphate, triethyl phosphate, etc.; the second precursor oxygen source is used to react with the first precursor to generate a phosphorus oxide medium layer, including but not limited to oxygen, ozone, laughing gas N2O, etc.

[0084] The metal contact area on the surface of the phosphorus oxide dielectric layer is laser grooved, with a laser pulse width range of 1-1000ns, a power range of 1%-100%, a frequency range of 100-3000kHz, and a laser scanning speed range of 1-30000mm / s. The metal contact area on the surface of the oxide dielectric layer is grooved by adjusting the above parameters, with a power of preferably 40%-60%, a pulse width of 30-60 µs, a frequency of 500kHz, and a scanning speed of 30000mm / s. At this time, the light spots are tangent, and the surface damage of the oxide dielectric layer is relatively low. The laser beam with a higher energy density is irradiated on the surface to produce melting, ablation and evaporation, thereby achieving the purpose of grooves.

[0085] Step S110, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition, TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C, to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5 nm;

[0086] Step S111, depositing a front anti-reflection layer and a back anti-reflection layer, using tubular or plate PECVD to deposit anti-reflection layers on the front and back of the silicon wafer, wherein the anti-reflection layers are one or more combinations of SiNx, SiOxNy, and SiOx;

[0087] Step S112, printing Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sintering to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; light injection to repair defects inside and on the surface of the battery.

[0088] As a preferred embodiment, this embodiment also provides a method for preparing a TOPCon battery structure, such as Figure 3 As shown, the following steps are included:

[0089] Step S101, texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a boron-doped P-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um;

[0090] Step S102: Phosphorus diffusion and laser doping to form a selective emitter, using POCl3 as the phosphorus source, a diffusion temperature of 700-900°C, a diffusion square resistance of 100-300Ω / □, and a doping concentration of 1E+21 cm -3 Then, a continuous laser is used to locally dope the metal contact area on the surface of the silicon substrate. Through the thermal effect of laser grooving, the phosphorus atoms in the phosphorus silicate glass are simultaneously pushed into the silicon wafer to form a local heavily doped area inside the silicon wafer. The laser power is preferably 20-45W and the wavelength is 355-1064nm. The laser-doped silicon substrate is subjected to high-temperature annealing, and an n+ emitter is formed after oxidation annealing, which has a lightly doped area with high square resistance and a heavily doped area with low square resistance; the lightly doped area is located in the non-metal contact area, and the heavily doped area is located in the metal contact area.

[0091] Step S103, single-side HF etching to remove backside BSG;

[0092] Step S104, etching the back side doping layer, using the front side BSG as a barrier layer, and using an alkaline solution to etch and remove the back side doping layer;

[0093] Step S105, depositing a tunnel oxide layer and an intrinsic polysilicon layer, first, in an LPCVD furnace tube, using O2 as an oxidant, the oxidation temperature is 550-650° C., and the tunnel oxide layer is in-situ oxidized and grown on the back of the silicon wafer. Secondly, after the growth of the tunnel oxide layer is completed, SiH4 is used as a reaction gas, N2 is used as a diluent gas, and the deposition temperature is 550-650° C., and the intrinsic polysilicon film is continuously deposited on the surface of the tunnel oxide layer using the LPCVD technology;

[0094] Step S106, boron diffusion, using boron trichloride or boron tribromide as a diffusion boron source, while introducing nitrogen and oxygen as reaction gases; the flow rate of the boron source is 50-500sccm, the flow rate of nitrogen is 1000-10000sccm, and the flow rate of oxygen is 500-4000sccm; the intrinsic polysilicon layer is subjected to boron diffusion, and the square resistance after boron diffusion is 120-300ohm / sq, and the diffusion concentration is 7E19-1E20cm -3 , forming a back-doped polysilicon layer;

[0095] Step S107, etching the front side polysilicon, using an alkaline solution to etch away the polysilicon layer on the front PSG surface, and using hydrofluoric acid to clean and remove the PSG on the front and back sides;

[0096] Step S108, alternately introducing a first precursor and a second precursor oxygen source into the process chamber, wherein the first precursor is a boron-containing precursor. After the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to generate an oxide, and this process is repeated to form an oxide medium layer of a desired thickness; the second precursor oxygen source is used to react with the first precursor to generate a boron oxide medium layer, including but not limited to oxygen, ozone, nitrous oxide N2O, etc.

[0097] The metal contact area on the surface of the boron oxide dielectric layer is laser grooved, with a laser pulse width range of 1-1000ns, a power range of 1%-100%, a frequency range of 100-3000kHz, and a laser scanning speed range of 1-30000mm / s; by adjusting the above parameters, the metal contact area on the surface of the oxide dielectric layer is grooved, with a power of preferably 40%-60%, a pulse width of 30-60 µs, a frequency of 500kHz, and a scanning speed of 30000mm / s. At this time, the light spots are tangent, the surface damage of the oxide dielectric layer is low, and a laser beam with a higher energy density is irradiated on the surface to produce melting, ablation and evaporation, thereby achieving the purpose of grooving.

[0098] Step S109, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition, TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C, to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5 nm;

[0099] Step S110, depositing a front anti-reflection layer and a back anti-reflection layer, using tubular or plate PECVD to deposit anti-reflection layers on the front and back of the silicon wafer, wherein the anti-reflection layers are one or more combinations of SiNx, SiOxNy, and SiOx;

[0100] Step S111, printing Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sintering to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; light injection to repair defects inside and on the surface of the battery.

[0101] The beneficial effects of the TOPCon battery structure and its preparation process in this embodiment are further reviewed below through several groups of examples.

[0102] Embodiment 1:

[0103] A method for preparing an N-type TOPCon battery structure comprises the following steps:

[0104] Step S101, texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um;

[0105] Step S102, boron diffusion and laser doping to form a selective emitter, using BCl3 or BBr3 as a boron source, diffusion temperature 900-1100°C, diffusion square resistance 100-300Ω / □, forming a surface concentration of 9E+18 cm on the front of the silicon substrate -3 Then, a continuous laser was used to locally dope the metal contact area on the surface of the silicon substrate. Through the thermal effect of the laser grooving, the boron atoms in the borosilicate glass were simultaneously pushed into the silicon wafer to form a local heavily doped area inside the silicon wafer. The surface concentration of the metal contact area of ​​the borosilicate glass film was reduced to 5E+18 cm -3 The laser power is preferably 20-45W, and the wavelength is 355-1064nm. The laser-doped silicon substrate is subjected to high-temperature annealing, and after oxidation annealing, a p+ emitter is formed, which has a lightly doped region with high square resistance and a heavily doped region with low square resistance; wherein the lightly doped region is located in the non-metallic contact region, and the heavily doped region is located in the metal contact region.

[0106] Step S103, single-side HF etching to remove backside BSG;

[0107] Step S104, etching the back side doping layer, using the front side BSG as a barrier layer, and using an alkaline solution to etch and remove the back side doping layer;

[0108] Step S105, depositing a tunnel oxide layer and an intrinsic polysilicon layer, first, in an LPCVD furnace tube, using O2 as an oxidant, the oxidation temperature is 550-650° C., and the tunnel oxide layer is in-situ oxidized and grown on the back of the silicon wafer. Secondly, after the growth of the tunnel oxide layer is completed, SiH4 is used as a reaction gas, N2 is used as a diluent gas, and the deposition temperature is 550-650° C., and the intrinsic polysilicon film is continuously deposited on the surface of the tunnel oxide layer using the LPCVD technology;

[0109] Step S106: Phosphorus diffusion, using POCl3 as the diffusion source, the diffusion temperature is 800-900°C, and the intrinsic polysilicon layer is doped with n-type phosphorus, with a doping concentration of 1-5E20cm -3 , forming a back-doped polysilicon layer; the thickness of which is 40nm;

[0110] Step S107, single-sided HF etching to remove PSG on the surface of the front-side plated polysilicon layer after diffusion;

[0111] Step S108, etching the front side polysilicon, using alkaline solution to etch away the polysilicon layer on the front BSG surface, and using hydrofluoric acid to clean and remove the front BSG and the back PSG;

[0112] Step S109, alternately introducing a first precursor and a second precursor oxygen source into the process chamber, wherein the first precursor is a phosphorus-containing precursor; after the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to form an oxide, and this is repeated to form an oxidizing medium layer of a desired thickness; wherein the phosphorus-containing precursor is trimethyl phosphate, and the second precursor oxygen source is oxygen, which is used to react with the first precursor to form an oxidizing medium layer, and the thickness of the oxidizing medium layer is 35 nm;

[0113] The surface metal contact area of ​​the oxide dielectric layer is laser grooved with a laser power of 40%-60%, a pulse width of 30-60µs, a frequency of 500kHz, and a scanning speed of 30000mm / s.

[0114] Step S110, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition, TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C, to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5 nm;

[0115] Step S111, depositing a front anti-reflection layer and a back anti-reflection layer, using tubular or plate PECVD to deposit anti-reflection layers on the front and back of the silicon wafer, wherein the anti-reflection layers are one or more combinations of SiNx, SiOxNy, and SiOx;

[0116] Step S112, printing Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sintering to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; light injection to repair defects inside and on the surface of the battery.

[0117] Embodiment 2:

[0118] A method for preparing an N-type TOPCon battery structure comprises the following steps:

[0119] Step S101, texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um;

[0120] Step S102, boron diffusion and laser doping to form a selective emitter, using BCl3 or BBr3 as a boron source, diffusion temperature 900-1100°C, diffusion square resistance 100-300Ω / □, forming a surface concentration of 9E+18 cm on the front of the silicon substrate -3 Then, a continuous laser was used to locally dope the metal contact area on the surface of the silicon substrate. Through the thermal effect of the laser grooving, the boron atoms in the borosilicate glass were simultaneously pushed into the silicon wafer to form a local heavily doped area inside the silicon wafer. The doping concentration of the metal contact area of ​​the borosilicate glass film was reduced to 5E+18 cm -3 The laser power is preferably 20-45W, and the wavelength is 355-1064nm. The laser-doped silicon substrate is subjected to high-temperature annealing, and after oxidation annealing, a p+ emitter is formed, which has a lightly doped region with high square resistance and a heavily doped region with low square resistance; wherein the lightly doped region is located in the non-metallic contact region, and the heavily doped region is located in the metal contact region.

[0121] Step S103, single-side HF etching to remove backside BSG;

[0122] Step S104, etching the back side doping layer, using the front side BSG as a barrier layer, and using an alkaline solution to etch and remove the back side doping layer;

[0123] Step S105, depositing a tunnel oxide layer and an intrinsic polysilicon layer, first, in an LPCVD furnace tube, using O2 as an oxidant, the oxidation temperature is 550-650° C., and the tunnel oxide layer is in-situ oxidized and grown on the back of the silicon wafer. Secondly, after the growth of the tunnel oxide layer is completed, SiH4 is used as a reaction gas, N2 is used as a diluent gas, and the deposition temperature is 550-650° C., and the intrinsic polysilicon film is continuously deposited on the surface of the tunnel oxide layer using the LPCVD technology;

[0124] Step S106: Phosphorus diffusion, using POCl3 as the diffusion source, the diffusion temperature is 800-900°C, and the intrinsic polysilicon layer is doped with n-type phosphorus, with a doping concentration of 1-5E20cm -3 , forming a back-doped polysilicon layer; the thickness of which is 60nm;

[0125] Step S107, single-sided HF etching to remove PSG on the surface of the front-side plated polysilicon layer after diffusion;

[0126] Step S108, etching the front side polysilicon, using alkaline solution to etch away the polysilicon layer on the front BSG surface, and using hydrofluoric acid to clean and remove the front BSG and the back PSG;

[0127] Step S109, alternately introducing a first precursor and a second precursor oxygen source into the process chamber, wherein the first precursor is a phosphorus-containing precursor; after the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to form an oxide, and this process is repeated to form an oxidizing medium layer of a desired thickness; wherein the phosphorus-containing precursor is trimethyl phosphate, and the second precursor oxygen source is ozone, which is used to react with the first precursor to form an oxidizing medium layer with a thickness of 30 nm;

[0128] The surface metal contact area of ​​the oxide dielectric layer is laser grooved with a laser power of 40%-60%, a pulse width of 30-60µs, a frequency of 500kHz, and a scanning speed of 30000mm / s.

[0129] Step S110, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition, TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C, to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5 nm;

[0130] Step S111, depositing a front anti-reflection layer and a back anti-reflection layer, using tubular or plate PECVD to deposit anti-reflection layers on the front and back of the silicon wafer, wherein the anti-reflection layers are one or more combinations of SiNx, SiOxNy, and SiOx;

[0131] Step S112, printing Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sintering to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; light injection to repair defects inside and on the surface of the battery.

[0132] Embodiment 3:

[0133] A method for preparing an N-type TOPCon battery structure comprises the following steps:

[0134] Step S101, texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um;

[0135] Step S102, boron diffusion and laser doping to form a selective emitter, using BCl3 or BBr3 as a boron source, diffusion temperature 900-1100°C, diffusion square resistance 100-300Ω / □, forming a surface concentration of 9E+18 cm on the front of the silicon substrate -3 Then, a continuous laser was used to locally dope the metal contact area on the surface of the silicon substrate. Through the thermal effect of the laser grooving, the boron atoms in the borosilicate glass were simultaneously pushed into the silicon wafer to form a local heavily doped area inside the silicon wafer. The doping concentration of the metal contact area of ​​the borosilicate glass film was reduced to 5E+18 cm -3 The laser power is preferably 20-45W, and the wavelength is 355-1064nm. The laser-doped silicon substrate is subjected to high-temperature annealing, and after oxidation annealing, a p+ emitter is formed, which has a lightly doped region with high square resistance and a heavily doped region with low square resistance; wherein the lightly doped region is located in the non-metallic contact region, and the heavily doped region is located in the metal contact region.

[0136] Step S103, single-side HF etching to remove backside BSG;

[0137] Step S104, etching the back side doping layer, using the front side BSG as a barrier layer, and using an alkaline solution to etch and remove the back side doping layer;

[0138] Step S105, depositing a tunnel oxide layer and an intrinsic polysilicon layer, first, in an LPCVD furnace tube, using O2 as an oxidant, the oxidation temperature is 550-650° C., and the tunnel oxide layer is in-situ oxidized and grown on the back of the silicon wafer. Secondly, after the growth of the tunnel oxide layer is completed, SiH4 is used as a reaction gas, N2 is used as a diluent gas, and the deposition temperature is 550-650° C., and the intrinsic polysilicon film is continuously deposited on the surface of the tunnel oxide layer using the LPCVD technology;

[0139] Step S106: Phosphorus diffusion, using POCl3 as the diffusion source, the diffusion temperature is 800-900°C, and the intrinsic polysilicon layer is doped with n-type phosphorus, with a doping concentration of 1-5E20cm -3 , forming a back-doped polysilicon layer; the thickness of which is 70nm;

[0140] Step S107, single-sided HF etching to remove PSG on the surface of the front-side plated polysilicon layer after diffusion;

[0141] Step S108, etching the front side polysilicon, using alkaline solution to etch away the polysilicon layer on the front BSG surface, and using hydrofluoric acid to clean and remove the front BSG and the back PSG;

[0142] Step S109, alternately introducing a first precursor and a second precursor oxygen source into the process chamber, wherein the first precursor is a phosphorus-containing precursor; after the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to form an oxide, and this is repeated to form an oxidizing medium layer of a desired thickness; wherein the phosphorus-containing precursor is triethyl phosphate, and the second precursor oxygen source is nitrous oxide N2O, which is used to react with the first precursor to form an oxidizing medium layer, and the thickness of the oxidizing medium layer is 30 nm;

[0143] The surface metal contact area of ​​the oxide dielectric layer is laser grooved with a laser power of 40%-60%, a pulse width of 30-60µs, a frequency of 500kHz, and a scanning speed of 30000mm / s.

[0144] Step S110, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition, TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C, to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5 nm;

[0145] Step S111, depositing a front anti-reflection layer and a back anti-reflection layer, using tubular or plate PECVD to deposit anti-reflection layers on the front and back of the silicon wafer, wherein the anti-reflection layers are one or more combinations of SiNx, SiOxNy, and SiOx;

[0146] Step S112, printing Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sintering to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; light injection to repair defects inside and on the surface of the battery.

[0147] Embodiment 4:

[0148] A method for preparing a P-type TOPCon battery structure comprises the following steps:

[0149] Step S101, texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a boron-doped P-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um;

[0150] Step S102: Phosphorus diffusion and laser doping to form a selective emitter, using POCl3 as the phosphorus source, a diffusion temperature of 700-1000°C, a diffusion square resistance of 100-300Ω / □, and a surface concentration of 1E+20 cm -3Then, a continuous laser is used to locally dope the metal contact area on the surface of the silicon substrate. Through the thermal effect of laser grooving, the phosphorus atoms in the phosphorus silicate glass are simultaneously pushed into the silicon wafer to form a local heavily doped area inside the silicon wafer. The laser power is preferably 20-45W and the wavelength is 355-1064nm. The laser-doped silicon substrate is subjected to high-temperature annealing, and after oxidation annealing, a p+ emitter is formed, which has a lightly doped area with high square resistance and a heavily doped area with low square resistance; the lightly doped area is located in the non-metallic contact area, and the heavily doped area is located in the metal contact area.

[0151] Step S103, single-sided HF etching to remove the back PSG;

[0152] Step S104, etching the back side doping layer, using the front PSG as a barrier layer, and using an alkaline solution to etch and remove the back side doping layer;

[0153] Step S105, depositing a tunnel oxide layer and an intrinsic polysilicon layer, first, in an LPCVD furnace tube, using O2 as an oxidant, the oxidation temperature is 550-650° C., and the tunnel oxide layer is in-situ oxidized and grown on the back of the silicon wafer. Secondly, after the growth of the tunnel oxide layer is completed, SiH4 is used as a reaction gas, N2 is used as a diluent gas, and the deposition temperature is 550-650° C., and the intrinsic polysilicon film is continuously deposited on the surface of the tunnel oxide layer using the LPCVD technology;

[0154] Step S106, boron diffusion, using boron trichloride or boron tribromide as a diffusion boron source, while introducing nitrogen and oxygen as reaction gases; the flow rate of the boron source is 50-500sccm, the flow rate of nitrogen is 1000-10000sccm, and the flow rate of oxygen is 500-4000sccm; the intrinsic polysilicon layer is subjected to boron diffusion, and the square resistance after boron diffusion is 120-300ohm / sq, and the diffusion concentration is 7E19-1E20cm -3 , forming a back-doped polysilicon layer with a thickness of 70nm;

[0155] Step S107, etching the front side polysilicon, using an alkaline solution to remove the polysilicon layer on the front BSG surface, and using hydrofluoric acid to remove the BSG on the front and back sides;

[0156] Step S108, alternately introducing the first precursor and the second precursor oxygen source into the process chamber, the first precursor is a boron-containing precursor, boron trichloride is used, after the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to form an oxide, and this process is repeated to form an oxidizing medium layer of the required thickness; the second precursor oxygen source is oxygen gas, which is used to react with the first precursor to form an oxidizing medium layer, and the thickness of the oxidizing medium layer is 30nm.

[0157] The surface metal contact area of ​​the oxide dielectric layer is laser grooved with a laser power of 40%-60%, a pulse width of 30-60µs, a frequency of 500kHz, and a scanning speed of 30000mm / s.

[0158] Step S109, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition, TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C, to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5 nm;

[0159] Step S110, depositing a front anti-reflection layer and a back anti-reflection layer, using tubular or plate PECVD to deposit anti-reflection layers on the front and back of the silicon wafer, wherein the anti-reflection layers are one or more combinations of SiNx, SiOxNy, and SiOx;

[0160] Step S111, printing Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sintering to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; light injection to repair defects inside and on the surface of the battery.

[0161] Embodiment 5:

[0162] A method for preparing a P-type TOPCon battery structure comprises the following steps:

[0163] Step S101, texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a boron-doped P-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um;

[0164] Step S102: Phosphorus diffusion and laser doping to form a selective emitter, using POCl3 as a boron source, a diffusion temperature of 700-1000°C, a diffusion square resistance of 100-300Ω / □, and a surface concentration of 1E+20 cm -3 Then, a continuous laser was used to locally dope the metal contact area on the surface of the silicon substrate. Through the thermal effect of laser grooving, the phosphorus atoms in the phosphosilicate glass were simultaneously pushed into the silicon wafer to form a local heavily doped area inside the silicon wafer. The doping concentration of the metal contact area of ​​the phosphosilicate glass film was reduced to 5E+18 cm 3 The laser power is preferably 20-45W, and the wavelength is 355-1064nm. The laser-doped silicon substrate is subjected to high-temperature annealing, and an n+ emitter is formed after oxidation annealing, which has a lightly doped region with high square resistance and a heavily doped region with low square resistance; the lightly doped region is located in the non-metal contact region, and the heavily doped region is located in the metal contact region.

[0165] Step S103, single-sided HF etching to remove the back PSG;

[0166] Step S104, etching the back side doping layer, using the front PSG as a barrier layer, and using an alkaline solution to etch and remove the back side doping layer;

[0167] Step S105, depositing a tunnel oxide layer and an intrinsic polysilicon layer, first, in an LPCVD furnace tube, using O2 as an oxidant, the oxidation temperature is 550-650° C., and the tunnel oxide layer is in-situ oxidized and grown on the back of the silicon wafer. Secondly, after the growth of the tunnel oxide layer is completed, SiH4 is used as a reaction gas, N2 is used as a diluent gas, and the deposition temperature is 550-650° C., and the intrinsic polysilicon film is continuously deposited on the surface of the tunnel oxide layer using the LPCVD technology;

[0168] Step S106, boron diffusion, using boron trichloride or boron tribromide as a diffusion boron source, while introducing nitrogen and oxygen as reaction gases; the flow rate of the boron source is 50-500sccm, the flow rate of nitrogen is 1000-10000sccm, and the flow rate of oxygen is 500-4000sccm; the intrinsic polysilicon layer is subjected to boron diffusion, and the square resistance after boron diffusion is 120-300ohm / sq, and the diffusion concentration is 7E19-1E20cm -3 , forming a back-doped polysilicon layer with a thickness of 40nm;

[0169] Step S107, etching the front side polysilicon, using an alkaline solution to remove the polysilicon layer on the front BSG surface, and using hydrofluoric acid to remove the BSG on the front and back sides;

[0170] Step S108, alternately introducing the first precursor and the second precursor oxygen source into the process chamber, wherein the first precursor is a boron-containing precursor, such as boron tribromide. After the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to form an oxide, and this process is repeated to form an oxidizing medium layer of a desired thickness; the second precursor oxygen source is ozone, which is used to react with the first precursor to form an oxidizing medium layer, and the thickness of the oxidizing medium layer is 40nm.

[0171] The surface metal contact area of ​​the oxide dielectric layer is laser grooved with a laser power of 40%-60%, a pulse width of 30-60µs, a frequency of 500kHz, and a scanning speed of 30000mm / s.

[0172] Step S109, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition, TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C, to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5 nm;

[0173] Step S110, depositing a front anti-reflection layer and a back anti-reflection layer, using tubular or plate PECVD to deposit anti-reflection layers on the front and back of the silicon wafer, wherein the anti-reflection layers are one or more combinations of SiNx, SiOxNy, and SiOx;

[0174] Step S111, printing Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sintering to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; light injection to repair defects inside and on the surface of the battery.

[0175] The above five groups of embodiments and conventional TOPCon solar cells were subjected to performance tests, and the results are as follows:

[0176] Table 1 TOPCon solar cell performance test results in each group of examples

[0177] As shown in Table 1, after the introduction of the oxide dielectric layer, the efficiency of both P-type and N-type TOPCon cells has been improved, mainly in terms of the improvement in open circuit voltage (Voc), indicating that the dielectric layer has a certain passivation effect. However, due to the increase in series resistance, the fill factor has deteriorated. The laser grooving process will be optimized in the future to improve the ohmic contact and reduce the impact of series resistance.

[0178] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A TOPCon battery structure, It is characterized in that It includes a silicon substrate, whose front side is composed of a p+ emitter, an aluminum oxide dielectric layer, a front anti-reflection layer and a front conductive metal electrode from the inside to the outside; and whose back side is composed of an ultra-thin tunneling oxide layer, a back doped polysilicon layer, an oxide dielectric layer, a back anti-reflection layer and a back conductive metal electrode from the inside to the outside; The back conductive metal electrode penetrates the back anti-reflection layer and contacts the oxidized dielectric layer; the front conductive metal electrode penetrates the front anti-reflection layer and the aluminum oxide dielectric layer and contacts the p+ emitter; The silicon substrate is an N-type silicon substrate, the back-doped polysilicon layer is phosphorus-doped polysilicon, and the oxide medium layer is a phosphorus oxide medium layer; The silicon substrate may also be a P-type silicon substrate, the back-doped polysilicon layer may be a boron-doped polysilicon layer, and the oxide dielectric layer may be a boron oxide dielectric layer; The surface metal contact area of ​​the oxide medium layer has a notch formed by laser etching; The thickness of the back doped polysilicon layer is 30-90 nm, the thickness of the oxidized dielectric layer is 20-50 nm, and the sum of the thicknesses of the back doped polysilicon layer and the oxidized dielectric layer is not less than 60 nm; The thickness of the front anti-reflection layer is 70-120nm, the comprehensive refractive index is 1.9-2.1, and the refractive index of the film layer decreases in the direction away from the silicon substrate; the thickness of the back anti-reflection layer is 70-120nm, the comprehensive refractive index is 1.9-2.1, and the refractive index of the film layer decreases in the direction away from the silicon substrate.

2. A TOPCon battery structure according to claim 1, It is characterized in that The thickness of the aluminum oxide dielectric layer is 3-5 nm, the thickness of the p+ emitter is 0.5-0.8 nm; and the thickness of the ultra-thin tunneling oxide layer is 1-3 nm.

3. A TOPCon battery structure according to claim 1, It is characterized in that The front conductive metal electrode is an Ag / Al gate line electrode, and the back conductive metal electrode is an Ag gate line electrode, and the widths of both electrodes are 22-25 μm.

4. A method for preparing a TOPCon battery structure according to any one of claims 1 to 3, It is characterized in that After the silicon substrate is textured, boron is diffused and laser doped to form a selective emitter; An ultra-thin tunnel oxide layer and an intrinsic polysilicon layer are prepared on the back side by LPCVD process, and a back-doped polysilicon layer is prepared by phosphorus diffusion or boron diffusion; An oxide dielectric layer is prepared on the surface of the back-doped polysilicon layer by atomic layer deposition, and then laser grooving is performed to form a local contact, and then an anti-reflection layer and a conductive metal electrode are prepared.

5. A method for preparing a TOPCon battery structure according to any one of claims 1 to 3, It is characterized in that The steps include: Step 1: Texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um; Step 2: Boron diffusion and laser doping to form a selective emitter, using BCl 3 or BBr 3 It is a boron source, with a diffusion temperature of 900-1100℃, a diffusion square resistance of 100-300Ω / □, and a doping concentration of 9E+18cm on the front of the silicon substrate. -3 borosilicate glass film; then use continuous laser to locally dope the metal contact area on the surface of the silicon substrate, perform high-temperature annealing on the laser-doped silicon substrate, and form a p+ emitter after oxidation annealing, which has a lightly doped area with high square resistance and a heavily doped area with low square resistance; Step 3: Single-sided HF etching to remove the back BSG; Step 4: Etch the back side doping layer, use the front BSG as a barrier layer, and use an alkaline solution to etch and remove the back side doping layer; Step 5: Deposit tunnel oxide layer and intrinsic polysilicon layer. First, in the LPCVD furnace, 2 As an oxidant, the oxidation temperature is 550-650℃, and the tunnel oxide layer is grown in situ on the back of the silicon wafer. Secondly, after the tunnel oxide layer is grown, SiH 4 is the reaction gas, N 2 The gas is used for dilution, and the deposition temperature is 550-650°C. The intrinsic polysilicon film is deposited on the surface of the tunnel oxide layer by LPCVD technology. Step 6: Phosphorus diffusion, using POCl3 as the diffusion source, the diffusion temperature is 800-900℃, and the intrinsic polysilicon layer is doped with n-type phosphorus, with a doping concentration of 1~5E20cm -3 , forming a back-doped polysilicon layer; Step 7: single-sided HF etching to remove PSG on the surface of the front polysilicon layer after diffusion; Step 8: etching the front polysilicon, using alkaline solution to remove the polysilicon layer on the front PSG surface, and using hydrofluoric acid to remove the BSG on the front and the PSG on the back; Step nine, alternately introducing a first precursor and a second precursor oxygen source into the process chamber, wherein the first precursor is a phosphorus-containing precursor. After the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to form an oxide, and this process is repeated to form an oxide medium layer of a desired thickness; Laser grooving is performed on the surface metal contact area of ​​the oxide dielectric layer, with a laser pulse width range of 1-1000ns, a power range of 1%-100%, a frequency range of 100-3000kHz, and a laser scanning speed range of 1-30000mm / s; Step 10, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition method, using TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5nm; Step 11, depositing a front anti-reflection layer and a back anti-reflection layer, using a tubular or plate PECVD to deposit an anti-reflection layer on the front and back of the silicon wafer, wherein the anti-reflection layer is one or more combinations of SiNx, SiOxNy, and SiOx; Step 12: print Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sinter to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; and inject light to repair defects inside and on the surface of the battery.

6. A method for preparing a TOPCon battery structure according to any one of claims 1 to 3, It is characterized in that The steps include: Step 1: Texturing, using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the front of the silicon substrate to increase the absorption of sunlight and reduce reflection; the silicon substrate is a boron-doped P-type single crystal silicon wafer with a resistivity of 0.1-10Ωcm and a thickness of 100-200um; Step 2: Phosphorus diffusion and laser doping to form a selective emitter using POCl 3 It is a phosphorus source, with a diffusion temperature of 700-1000℃, a diffusion square resistance of 100-300Ω / □, and a doping concentration of 1E+20cm on the front of the silicon substrate. -3 Then, a continuous laser is used to locally dope the metal contact area on the surface of the silicon substrate, and the laser-doped silicon substrate is subjected to high-temperature annealing. After oxidation annealing, an n+ emitter is formed, which has a lightly doped area with high square resistance and a heavily doped area with low square resistance. Step 3: single-sided HF etching to remove the back PSG; Step 4: etching the back side doping layer, using the front PSG as a barrier layer, and using an alkaline solution to etch and remove the back side doping layer; Step 5: Deposit tunnel oxide layer and intrinsic polysilicon layer. First, in the LPCVD furnace, 2 As an oxidant, the oxidation temperature is 550-650℃, and the tunnel oxide layer is grown in situ on the back of the silicon wafer. Secondly, after the tunnel oxide layer is grown, SiH 4 is the reaction gas, N 2 The gas is used for dilution, and the deposition temperature is 550-650°C. The intrinsic polysilicon film is deposited on the surface of the tunnel oxide layer by LPCVD technology. Step 6: Boron diffusion, using boron trichloride or boron tribromide as the boron diffusion source, and introducing nitrogen and oxygen as reaction gases; the flow rate of the boron source is 50-500sccm, the flow rate of nitrogen is 1000-10000sccm, and the flow rate of oxygen is 500-4000sccm; the intrinsic polysilicon layer is diffused with boron, and the square resistance after boron diffusion is 120-300ohm / sq, and the diffusion concentration is 7E19-1E20cm -3 , forming a back-doped polysilicon layer; Step 7: etching the front side polysilicon, using alkaline solution to remove the polysilicon layer on the front BSG surface, and using hydrofluoric acid to remove the BSG on the front and back sides; Step eight, alternately introducing a first precursor and a second precursor oxygen source into the process chamber, wherein the first precursor is a boron-containing precursor, and after the first precursor is deposited on the polysilicon, the second precursor oxygen source is introduced and reacts with the first precursor to form an oxide, and this process is repeated to form an oxide medium layer of a desired thickness; Laser grooving is performed on the surface metal contact area of ​​the oxide dielectric layer, with a laser pulse width range of 1-1000ns, a power range of 1%-100%, a frequency range of 100-3000kHz, and a laser scanning speed range of 1-30000mm / s; Step nine, depositing an aluminum oxide dielectric layer on the front side, using ALD atomic layer deposition method, using TMA as a precursor, H2O as an oxidant, and controlling the reaction temperature at 200-350°C to deposit an aluminum oxide dielectric layer on the front p+ emitter surface with a thickness of 1-5nm; Step 10, depositing a front anti-reflection layer and a back anti-reflection layer, using tubular or plate PECVD to deposit anti-reflection layers on the front and back of the silicon wafer, wherein the anti-reflection layers are one or more combinations of SiNx, SiOxNy, and SiOx; Step 11: print Ag / Al paste for the front electrode and Ag paste for the back electrode; co-sinter to form a good ohmic contact to obtain a front conductive metal electrode and a back conductive metal electrode; and inject light to repair defects inside and on the surface of the battery.