A PET additive masterbatch and its preparation method and application
By preparing modified titanium dioxide nanospheres and glassy carbon deposition nanospheres, combined with aminosilane and quaternization treatment, a PET additive masterbatch is formed, which solves the problem of static electricity hazards of PET sheets and improves the antistatic and mechanical properties. The safety and environmental protection of the materials are ensured.
Patent Information
- Application Number
- CN202410662299.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-05-27
AI Technical Summary
Due to the lack of conductive properties of PET sheets, it is easy to cause static electricity hazards, leading to accidents such as static electricity accumulation, dust collection, discharge, short circuits and fires. The addition of existing antistatic agents has problems such as complex processes, uneven dispersion, and insufficient durability.
Prepare PET additive masterbatch by preparing titanium dioxide nanospheres and performing surface modification, depositing doped glassy carbon, aminosilane modification, quaternization, mixing and adding into PET resin for melt mixing, extrusion and granulation to form a product with good resistance. Additive masterbatch for electrostatic properties.
It significantly improves the antistatic performance and environmental protection of PET resin, while improving the mechanical properties and ensuring the safety and reliability of the material.
Smart Images

Figure BDA0004860065830000151 
Figure BDA0004860065830000161 
Figure BDA0004860065830000162
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of additive masterbatch, and in particular to a PET additive masterbatch and a preparation method and application thereof. Background Art
[0002] PET, the full name of which is polyethylene terephthalate, is a thermoplastic polymer with the advantages of low cost and easy molding. It is widely used in additive masterbatch, packaging, printing and other industries. In daily production and use, due to friction, static electricity will accumulate on the surface of plastic film. A large amount of static electricity accumulation causes dust to be absorbed on the surface of plastic packaging film, discharge, short circuit of electronic devices, and even fire, explosion and other accidents. Due to the lack of certain properties of PET sheets, such as conductivity, it is easy to cause static electricity hazards, and the modification cost is high and difficult, which limits its wider application.
[0003] In order to avoid the above problems and improve the safety of plastic packaging films, it is necessary to improve the antistatic performance of plastic packaging materials. Adding organic antistatic agents or inorganic conductive fillers is a common method in industry. Directly adding antistatic agents can prevent the hazards of static electricity, but there are also problems such as complex processes, uneven dispersion, and insufficient durability. Masterbatch technology is often used in industry to solve the above problems, that is, antistatic agents are mixed with resin carriers and other additives and pelletized to form antistatic masterbatches, which improves compatibility with resins and is easier to disperse than directly adding liquid, powdered or paste antistatic agents to achieve the ideal antistatic effect. Summary of the invention
[0004] The purpose of the present invention is to provide a PET additive masterbatch and a preparation method and application thereof. The preparation method is simple and the raw material source is wide. The antistatic property of PET resin can be significantly improved, the environmental protection property can be improved, and the mechanical properties of the resin can be improved to a certain extent. The present invention has broad application prospects.
[0005] The technical solution of the present invention is achieved in this way:
[0006] The invention provides a method for preparing a PET additive masterbatch. The method comprises the following steps: preparing titanium dioxide nanospheres, modifying the surfaces by tannic acid polymerization, depositing N / S-doped glassy carbon, modifying the nanospheres by aminosilane, quaternizing the amino groups, mixing the nanospheres with a plasticizer, adding the nanospheres to a PET resin, melting and mixing the nanospheres, and extruding and granulating the nanospheres to obtain the PET additive masterbatch.
[0007] As a further improvement of the present invention, the following steps are included:
[0008] S1. Preparation of titanium dioxide nanospheres: tetrabutyl titanate was dissolved in ethanol, ammonia water was added dropwise, stirred for reaction, centrifuged, washed, dried, ball-milled, and calcined to obtain titanium dioxide nanospheres;
[0009] S2. Preparation of modified titanium dioxide nanospheres: adding titanium dioxide nanospheres to water, adding tannic acid and a catalyst, heating and stirring to react, centrifuging, washing, and drying to obtain modified titanium dioxide nanospheres;
[0010] S3. Preparation of N / S-doped glassy carbon-deposited titanium dioxide nanospheres: The phenolic resin, cellulose, modified titanium dioxide nanospheres, melamine and thiourea were mixed and ball-milled uniformly, and vacuum carbonized to obtain N / S-doped glassy carbon-deposited titanium dioxide nanospheres;
[0011] S4. Preparation of aminosilane-modified nanospheres: adding the N / S-doped glassy carbon-deposited titanium dioxide nanospheres obtained in step S3 to ethanol, adding aminosilane, heating and stirring to react, centrifuging, washing, and drying to obtain aminosilane-modified nanospheres;
[0012] S5. Quaternization reaction: adding the aminosilane-modified nanospheres obtained in step S4 to water, adding formic acid and formaldehyde solution, heating and stirring the reaction, centrifuging, washing, drying, adding N-methyl-2-pyrrolidone, adding iodomethane, stirring the reaction, centrifuging, washing, drying, to obtain quaternary ammonium-modified nanospheres;
[0013] S6. Preparation of PET additive masterbatch: melt-mix the quaternary ammonium modified nanospheres, plasticizer and PET resin obtained in step S5, and extrude and granulate to obtain PET additive masterbatch.
[0014] As a further improvement of the present invention, the mass ratio of tetrabutyl titanate, ethanol and ammonia water in step S1 is 15-20:60-70:5-7, the concentration of ammonia water is 20-25wt%, the stirring reaction time is 20-40min, the ball milling time is 1-3h, the calcination temperature is 450-550°C, and the time is 1-3h.
[0015] As a further improvement of the present invention, the mass ratio of the titanium dioxide nanospheres, tannic acid and catalyst in step S2 is 15-20:7-10:1-2, the catalyst is a Tris-HCl solution with a pH of 8.5-9, the temperature of the heating and stirring reaction is 40-50°C, and the time is 1-3h.
[0016] As a further improvement of the present invention, the mass ratio of the phenolic resin, cellulose, modified titanium dioxide nanospheres, melamine and thiourea in step S3 is 15-20:5-7:27-32:2-4:1-2, and the vacuum degree of the vacuum carbonization is 2-5×10 -2 Pa, heating rate is 10-15℃ / min, carbonization temperature is 1000-1200℃, and holding time is 1-3h.
[0017] As a further improvement of the present invention, the mass ratio of the N / S doped glassy carbon deposited titanium dioxide nanospheres and the aminosilane in step S4 is 10:1-2, and the aminosilane is selected from at least one of aminopropyltrimethoxysilane, aminopropyltriethoxysilane, N-β (aminoethyl) -γ-aminopropyltrimethoxysilane, and γ-aminoethylaminopropyltrimethoxysilane, preferably, it is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, and the mass ratio is 3-5:2. The temperature of the heating and stirring reaction is 40-50°C, and the time is 2-4h.
[0018] As a further improvement of the present invention, the mass ratio of the aminosilane-modified nanospheres, formic acid, formaldehyde solution, water, and methyl iodide in step S5 is 10:3-5:5-7:10-15:1-2, the concentration of the formaldehyde solution is 35-40wt%, the temperature of the heating and stirring reaction is 65-75°C, the time is 20-24h, and the stirring reaction time is 12-15h.
[0019] As a further improvement of the present invention, the mass ratio of the quaternized modified nanospheres, the plasticizer and the PET resin in step S6 is 10-12:2-4:100, the plasticizer is selected from at least one of epoxy soybean oil, epoxy acetyl linolenic acid methyl ester, epoxy furoate butyl ester, epoxy silkworm pupa oleic acid butyl ester, epoxy soybean oleate octyl ester, 9,10-epoxy stearic acid octyl ester, dioctyl adipate, dioctyl sebacate, and diisononyl adipate, and the melting temperature is 250-260°C.
[0020] The present invention further protects a PET auxiliary agent masterbatch prepared by the above preparation method.
[0021] The present invention further protects the use of the above PET auxiliary agent masterbatch in the preparation of antistatic PET resin.
[0022] The present invention has the following beneficial effects:
[0023] TiO2 nanoparticles have good photocatalytic and conductive properties. After the surface is modified with tannic acid, it has abundant active groups such as hydroxyl and carboxyl groups with good viscosity. It can be bonded with phenolic resin, cellulose, melamine and thiourea through electrostatic adsorption. After heating and carbonization, N / S-doped glassy carbon deposited titanium dioxide nanospheres were obtained. After N and S doping, the catalytic ability of TiO2 in the visible light wavelength range is improved, and the formaldehyde and organic catalytic performance and antibacterial performance of the product are greatly improved, which has good environmental protection. Glassy carbon has good conductive properties, and after deposition, it further improves the antistatic modification of nanospheres to PET resin. The surface is further modified with aminosilane and has abundant amino groups. The nanospheres with abundant quaternized groups on the surface obtained by quaternization reaction have good electrostatic elimination effect and strong adsorption capacity. At the same time, the antibacterial properties of the material are improved, and good effects can be exerted at low concentrations.
[0024] The invention mixes the prepared quaternary ammonium modified nanospheres, a plasticizer and a PET resin. Active groups such as hydroxyl groups and amino groups on the surfaces of the nanospheres can be combined with the PET resin by forming hydrogen bonds, thereby promoting the dispersion of the nanospheres in the PET resin. The addition of the plasticizer further improves the dispersibility of the nanospheres, is beneficial to optimizing the processing performance of the masterbatch, and improves the antistatic and conductive modification effects of the masterbatch on the PET resin.
[0025] The invention prepares PET auxiliary agent masterbatch, has a simple preparation method, and has a wide source of raw materials. It can significantly improve the antistatic property of PET resin, improve its environmental protection, and also improve the mechanical properties of the resin to a certain extent, and has broad application prospects. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The phenolic resin is 2130 phenolic resin purchased from Wuxi Jiunai Anticorrosion Materials Co., Ltd.
[0028] Cellulose, content 95-96%, density 0.66-0.68g / cm 3 , purchased from Shijiazhuang Xinyuan Cellulose Co., Ltd.
[0029] PET resin was purchased from Haozheng New Materials Technology (Dongguan) Co., Ltd.
[0030] Example 1
[0031] This embodiment provides a method for preparing a PET additive masterbatch, comprising the following steps:
[0032] S1. Preparation of titanium dioxide nanospheres: 15 parts by weight of tetrabutyl titanate was dissolved in 60 parts by weight of ethanol, 5 parts by weight of 20 wt% ammonia water was added dropwise, the reaction was stirred for 20 min, centrifuged, washed, dried, ball milled for 1 h, and calcined at 450 ° C for 1 h to obtain titanium dioxide nanospheres;
[0033] S2. Preparation of modified titanium dioxide nanospheres: 15 parts by weight of the titanium dioxide nanospheres prepared in step S1 were added to 200 parts by weight of water, 7 parts by weight of tannic acid and 1 part by weight of a catalyst were added, heated to 40 ° C, stirred for 1 h, centrifuged, washed, and dried to obtain modified titanium dioxide nanospheres;
[0034] The catalyst is a Tris-HCl solution with a pH of 8.5;
[0035] S3. Preparation of N / S-doped glassy carbon deposited titanium dioxide nanospheres: 15 parts by weight of phenolic resin, 5 parts by weight of cellulose, 27 parts by weight of modified titanium dioxide nanospheres prepared in step S2, 2 parts by weight of melamine and 1 part by weight of thiourea were mixed and ball-milled uniformly, and vacuum carbonized at a vacuum degree of 2×10 -2 Pa, heating rate of 10 °C / min, carbonization temperature of 1000 °C, holding time of 1 h, and N / S-doped glassy carbon deposited titanium dioxide nanospheres were obtained;
[0036] S4. Preparation of aminosilane-modified nanospheres: 10 parts by weight of the N / S-doped glassy carbon-deposited titanium dioxide nanospheres prepared in step S3 were added to 100 parts by weight of ethanol, 1 part by weight of aminosilane was added, the mixture was heated to 40° C., stirred for reaction for 2 h, centrifuged, washed, and dried to obtain aminosilane-modified nanospheres;
[0037] The aminosilane is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, with a mass ratio of 3:2;
[0038] S5. Quaternization reaction: 10 parts by weight of the aminosilane-modified nanospheres prepared in step S4 were added to 10 parts by weight of water, 3 parts by weight of formic acid, 5 parts by weight of a 35wt% formaldehyde solution were added, heated to 65 ° C, stirred for 20 hours, centrifuged, washed, dried, added to 50 parts by weight of N-methyl-2-pyrrolidone, 1 part by weight of methyl iodide was added, stirred for 12 hours, centrifuged, washed, and dried to obtain quaternized modified nanospheres;
[0039] S6. Preparation of PET additive masterbatch: 10 parts by weight of the quaternized modified nanospheres prepared in step S5, 2 parts by weight of diisononyl adipate and 100 parts by weight of PET resin are melt-mixed at 250° C. and extruded into granules to prepare PET additive masterbatch.
[0040] Example 2
[0041] This embodiment provides a method for preparing a PET additive masterbatch, comprising the following steps:
[0042] S1. Preparation of titanium dioxide nanospheres: 20 parts by weight of tetrabutyl titanate was dissolved in 70 parts by weight of ethanol, 7 parts by weight of 25 wt% ammonia water was added dropwise, the reaction was stirred for 40 min, centrifuged, washed, dried, ball milled for 3 h, and calcined at 550 ° C for 3 h to obtain titanium dioxide nanospheres;
[0043] S2. Preparation of modified titanium dioxide nanospheres: 20 parts by weight of the titanium dioxide nanospheres prepared in step S1 were added to 200 parts by weight of water, 10 parts by weight of tannic acid and 2 parts by weight of a catalyst were added, heated to 50 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain modified titanium dioxide nanospheres;
[0044] The catalyst is a Tris-HCl solution with a pH of 9;
[0045] S3. Preparation of N / S-doped glassy carbon deposited titanium dioxide nanospheres: 20 parts by weight of phenolic resin, 7 parts by weight of cellulose, 32 parts by weight of modified titanium dioxide nanospheres prepared in step S2, 4 parts by weight of melamine and 2 parts by weight of thiourea were mixed and ball-milled uniformly, and vacuum carbonized at a vacuum degree of 5×10 -2 Pa, heating rate of 15 °C / min, carbonization temperature of 1200 °C, holding time of 3 h, and N / S-doped glassy carbon deposited titanium dioxide nanospheres were obtained;
[0046] S4. Preparation of aminosilane-modified nanospheres: 10 parts by weight of the N / S-doped glassy carbon-deposited titanium dioxide nanospheres prepared in step S3 were added to 100 parts by weight of ethanol, 2 parts by weight of aminosilane were added, the mixture was heated to 50° C., stirred for 4 h, centrifuged, washed, and dried to obtain aminosilane-modified nanospheres;
[0047] The aminosilane is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, with a mass ratio of 5:2;
[0048] S5. Quaternization reaction: 10 parts by weight of the aminosilane-modified nanospheres prepared in step S4 were added to 15 parts by weight of water, 5 parts by weight of formic acid, 7 parts by weight of a 40wt% formaldehyde solution were added, heated to 75 ° C, stirred for 24 hours, centrifuged, washed, dried, added to 50 parts by weight of N-methyl-2-pyrrolidone, 2 parts by weight of methyl iodide were added, stirred for 15 hours, centrifuged, washed, and dried to obtain quaternary ammonium modified nanospheres;
[0049] S6. Preparation of PET additive masterbatch: 12 parts by weight of the quaternary ammonium modified nanospheres prepared in step S5, 4 parts by weight of 9,10-epoxy stearate and 100 parts by weight of PET resin are melt-mixed at 260°C, extruded and granulated to prepare PET additive masterbatch.
[0050] Example 3
[0051] This embodiment provides a method for preparing a PET additive masterbatch, comprising the following steps:
[0052] S1. Preparation of titanium dioxide nanospheres: 17 parts by weight of tetrabutyl titanate was dissolved in 65 parts by weight of ethanol, 6 parts by weight of 22 wt% ammonia water was added dropwise, the reaction was stirred for 30 min, centrifuged, washed, dried, ball milled for 2 h, and calcined at 500 ° C for 2 h to obtain titanium dioxide nanospheres;
[0053] S2. Preparation of modified titanium dioxide nanospheres: 17 parts by weight of the titanium dioxide nanospheres prepared in step S1 were added to 200 parts by weight of water, 8.5 parts by weight of tannic acid and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified titanium dioxide nanospheres;
[0054] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0055] S3. Preparation of N / S-doped glassy carbon deposited titanium dioxide nanospheres: 17 parts by weight of phenolic resin, 6 parts by weight of cellulose, 30 parts by weight of modified titanium dioxide nanospheres prepared in step S2, 3 parts by weight of melamine and 1.5 parts by weight of thiourea were mixed and ball-milled uniformly, and vacuum carbonized at a vacuum degree of 3.5×10 -2 Pa, heating rate of 12 °C / min, carbonization temperature of 1100 °C, holding time of 2 h, and N / S-doped glassy carbon deposited titanium dioxide nanospheres were obtained;
[0056] S4. Preparation of aminosilane-modified nanospheres: 10 parts by weight of the N / S-doped glassy carbon-deposited titanium dioxide nanospheres prepared in step S3 were added to 100 parts by weight of ethanol, 1.5 parts by weight of aminosilane were added, the mixture was heated to 45° C., stirred for 3 h, centrifuged, washed, and dried to obtain aminosilane-modified nanospheres;
[0057] The aminosilane is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, with a mass ratio of 4:2;
[0058] S5. Quaternization reaction: 10 parts by weight of the aminosilane-modified nanospheres prepared in step S4 were added to 12 parts by weight of water, 4 parts by weight of formic acid, 6 parts by weight of a 37wt% formaldehyde solution were added, heated to 70°C, stirred for 22h, centrifuged, washed, dried, added to 50 parts by weight of N-methyl-2-pyrrolidone, 1.5 parts by weight of iodomethane were added, stirred for 13.5h, centrifuged, washed, and dried to obtain quaternized modified nanospheres;
[0059] S6. Preparation of PET additive masterbatch: 11 parts by weight of the quaternary ammonium modified nanospheres prepared in step S5, 3 parts by weight of epoxy soybean octyl ester and 100 parts by weight of PET resin are melt-mixed at 255°C, extruded and granulated to prepare PET additive masterbatch.
[0060] Example 4
[0061] Compared with Example 3, the difference is that the aminosilane is a single N-β (aminoethyl) -γ-aminopropyltrimethoxysilane.
[0062] Example 5
[0063] Compared with Example 3, the difference is that the aminosilane is a single γ-aminoethylaminopropyltrimethoxysilane.
[0064] Comparative Example 1
[0065] Compared with Example 3, the difference is that step S2 is not performed.
[0066] The details are as follows:
[0067] S1. Preparation of titanium dioxide nanospheres: 17 parts by weight of tetrabutyl titanate was dissolved in 65 parts by weight of ethanol, 6 parts by weight of 22 wt% ammonia water was added dropwise, the reaction was stirred for 30 min, centrifuged, washed, dried, ball milled for 2 h, and calcined at 500 ° C for 2 h to obtain titanium dioxide nanospheres;
[0068] S2. Preparation of N / S-doped glassy carbon deposited titanium dioxide nanospheres: 17 parts by weight of phenolic resin, 6 parts by weight of cellulose, 30 parts by weight of titanium dioxide nanospheres prepared in step S1, 3 parts by weight of melamine and 1.5 parts by weight of thiourea were mixed and ball-milled uniformly, and vacuum carbonized at a vacuum degree of 3.5×10 -2 Pa, heating rate of 12 °C / min, carbonization temperature of 1100 °C, holding time of 2 h, and N / S-doped glassy carbon deposited titanium dioxide nanospheres were obtained;
[0069] S3. Preparation of aminosilane-modified nanospheres: 10 parts by weight of the N / S-doped glassy carbon-deposited titanium dioxide nanospheres prepared in step S2 were added to 100 parts by weight of ethanol, 1.5 parts by weight of aminosilane were added, the mixture was heated to 45° C., stirred for reaction for 3 h, centrifuged, washed, and dried to obtain aminosilane-modified nanospheres;
[0070] The aminosilane is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, with a mass ratio of 4:2;
[0071] S4. Quaternization reaction: 10 parts by weight of the aminosilane-modified nanospheres prepared in step S3 were added to 12 parts by weight of water, 4 parts by weight of formic acid, 6 parts by weight of a 37wt% formaldehyde solution were added, heated to 70°C, stirred for 22h, centrifuged, washed, dried, added to 50 parts by weight of N-methyl-2-pyrrolidone, 1.5 parts by weight of iodomethane were added, stirred for 13.5h, centrifuged, washed, and dried to obtain quaternary ammonium modified nanospheres;
[0072] S5. Preparation of PET additive masterbatch: 11 parts by weight of the quaternary ammonium modified nanospheres prepared in step S4, 3 parts by weight of epoxy soybean octyl ester and 100 parts by weight of PET resin are melt-mixed at 255°C, extruded and granulated to prepare PET additive masterbatch.
[0073] Comparative Example 2
[0074] Compared with Example 3, the difference is that step S3 is not performed.
[0075] The details are as follows:
[0076] S1. Preparation of titanium dioxide nanospheres: 17 parts by weight of tetrabutyl titanate was dissolved in 65 parts by weight of ethanol, 6 parts by weight of 22 wt% ammonia water was added dropwise, the reaction was stirred for 30 min, centrifuged, washed, dried, ball milled for 2 h, and calcined at 500 ° C for 2 h to obtain titanium dioxide nanospheres;
[0077] S2. Preparation of modified titanium dioxide nanospheres: 17 parts by weight of the titanium dioxide nanospheres prepared in step S1 were added to 200 parts by weight of water, 8.5 parts by weight of tannic acid and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified titanium dioxide nanospheres;
[0078] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0079] S3. Preparation of aminosilane-modified nanospheres: 10 parts by weight of the modified titanium dioxide nanospheres prepared in step S2 were added to 100 parts by weight of ethanol, 1.5 parts by weight of aminosilane were added, heated to 45 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain aminosilane-modified nanospheres;
[0080] The aminosilane is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, with a mass ratio of 4:2;
[0081] S4. Quaternization reaction: 10 parts by weight of the aminosilane-modified nanospheres prepared in step S3 were added to 12 parts by weight of water, 4 parts by weight of formic acid, 6 parts by weight of a 37wt% formaldehyde solution were added, heated to 70°C, stirred for 22h, centrifuged, washed, dried, added to 50 parts by weight of N-methyl-2-pyrrolidone, 1.5 parts by weight of iodomethane were added, stirred for 13.5h, centrifuged, washed, and dried to obtain quaternary ammonium modified nanospheres;
[0082] S5. Preparation of PET additive masterbatch: 11 parts by weight of the quaternary ammonium modified nanospheres prepared in step S4, 3 parts by weight of epoxy soybean octyl ester and 100 parts by weight of PET resin are melt-mixed at 255°C, extruded and granulated to prepare PET additive masterbatch.
[0083] Comparative Example 3
[0084] Compared with Example 3, the difference is that melamine is not added in step S3.
[0085] The details are as follows:
[0086] S1. Preparation of titanium dioxide nanospheres: 17 parts by weight of tetrabutyl titanate was dissolved in 65 parts by weight of ethanol, 6 parts by weight of 22 wt% ammonia water was added dropwise, the reaction was stirred for 30 min, centrifuged, washed, dried, ball milled for 2 h, and calcined at 500 ° C for 2 h to obtain titanium dioxide nanospheres;
[0087] S2. Preparation of modified titanium dioxide nanospheres: 17 parts by weight of the titanium dioxide nanospheres prepared in step S1 were added to 200 parts by weight of water, 8.5 parts by weight of tannic acid and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified titanium dioxide nanospheres;
[0088] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0089] S3. Preparation of S-doped glassy carbon deposited titanium dioxide nanospheres: 17 parts by weight of phenolic resin, 6 parts by weight of cellulose, 30 parts by weight of modified titanium dioxide nanospheres prepared in step S2, and 4.5 parts by weight of thiourea were mixed and ball-milled uniformly, and vacuum carbonized at a vacuum degree of 3.5×10 -2 Pa, heating rate of 12 °C / min, carbonization temperature of 1100 °C, holding time of 2 h, S-doped glassy carbon deposited titanium dioxide nanospheres were obtained;
[0090] S4. Preparation of aminosilane-modified nanospheres: 10 parts by weight of the S-doped glassy carbon-deposited titanium dioxide nanospheres prepared in step S3 were added to 100 parts by weight of ethanol, 1.5 parts by weight of aminosilane were added, the mixture was heated to 45° C., stirred for reaction for 3 h, centrifuged, washed, and dried to obtain aminosilane-modified nanospheres;
[0091] The aminosilane is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, with a mass ratio of 4:2;
[0092] S5. Quaternization reaction: 10 parts by weight of the aminosilane-modified nanospheres prepared in step S4 were added to 12 parts by weight of water, 4 parts by weight of formic acid, 6 parts by weight of a 37wt% formaldehyde solution were added, heated to 70°C, stirred for 22h, centrifuged, washed, dried, added to 50 parts by weight of N-methyl-2-pyrrolidone, 1.5 parts by weight of iodomethane were added, stirred for 13.5h, centrifuged, washed, and dried to obtain quaternized modified nanospheres;
[0093] S6. Preparation of PET additive masterbatch: 11 parts by weight of the quaternary ammonium modified nanospheres prepared in step S5, 3 parts by weight of epoxy soybean octyl ester and 100 parts by weight of PET resin are melt-mixed at 255°C, extruded and granulated to prepare PET additive masterbatch.
[0094] Comparative Example 4
[0095] Compared with Example 3, the difference is that thiourea is not added in step S3.
[0096] The details are as follows:
[0097] S1. Preparation of titanium dioxide nanospheres: 17 parts by weight of tetrabutyl titanate was dissolved in 65 parts by weight of ethanol, 6 parts by weight of 22 wt% ammonia water was added dropwise, the reaction was stirred for 30 min, centrifuged, washed, dried, ball milled for 2 h, and calcined at 500 ° C for 2 h to obtain titanium dioxide nanospheres;
[0098] S2. Preparation of modified titanium dioxide nanospheres: 17 parts by weight of the titanium dioxide nanospheres prepared in step S1 were added to 200 parts by weight of water, 8.5 parts by weight of tannic acid and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified titanium dioxide nanospheres;
[0099] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0100] S3. Preparation of N-doped glassy carbon deposited titanium dioxide nanospheres: 17 parts by weight of phenolic resin, 6 parts by weight of cellulose, 30 parts by weight of modified titanium dioxide nanospheres obtained in step S2, and 4.5 parts by weight of melamine were mixed and ball-milled uniformly, and vacuum carbonized at a vacuum degree of 3.5×10 -2 Pa, heating rate of 12 °C / min, carbonization temperature of 1100 °C, holding time of 2 h, and N-doped glassy carbon deposited titanium dioxide nanospheres were obtained;
[0101] S4. Preparation of aminosilane-modified nanospheres: 10 parts by weight of the N-doped glassy carbon-deposited titanium dioxide nanospheres prepared in step S3 were added to 100 parts by weight of ethanol, 1.5 parts by weight of aminosilane were added, the mixture was heated to 45° C., stirred for 3 h, centrifuged, washed, and dried to obtain aminosilane-modified nanospheres;
[0102] The aminosilane is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, with a mass ratio of 4:2;
[0103] S5. Quaternization reaction: 10 parts by weight of the aminosilane-modified nanospheres prepared in step S4 were added to 12 parts by weight of water, 4 parts by weight of formic acid, 6 parts by weight of a 37wt% formaldehyde solution were added, heated to 70°C, stirred for 22h, centrifuged, washed, dried, added to 50 parts by weight of N-methyl-2-pyrrolidone, 1.5 parts by weight of iodomethane were added, stirred for 13.5h, centrifuged, washed, and dried to obtain quaternized modified nanospheres;
[0104] S6. Preparation of PET additive masterbatch: 11 parts by weight of the quaternary ammonium modified nanospheres prepared in step S5, 3 parts by weight of epoxy soybean octyl ester and 100 parts by weight of PET resin are melt-mixed at 255°C, extruded and granulated to prepare PET additive masterbatch.
[0105] Comparative Example 5
[0106] Compared with Example 3, the difference is that melamine and thiourea are not added in step S3.
[0107] The details are as follows:
[0108] S1. Preparation of titanium dioxide nanospheres: 17 parts by weight of tetrabutyl titanate was dissolved in 65 parts by weight of ethanol, 6 parts by weight of 22 wt% ammonia water was added dropwise, the reaction was stirred for 30 min, centrifuged, washed, dried, ball milled for 2 h, and calcined at 500 ° C for 2 h to obtain titanium dioxide nanospheres;
[0109] S2. Preparation of modified titanium dioxide nanospheres: 17 parts by weight of the titanium dioxide nanospheres prepared in step S1 were added to 200 parts by weight of water, 8.5 parts by weight of tannic acid and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified titanium dioxide nanospheres;
[0110] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0111] S3. Preparation of glassy carbon deposited titanium dioxide nanospheres: 21.5 parts by weight of phenolic resin, 6 parts by weight of cellulose, and 30 parts by weight of modified titanium dioxide nanospheres obtained in step S2 were mixed and ball-milled uniformly, and vacuum carbonized at a vacuum degree of 3.5×10 - 2 Pa, heating rate of 12 °C / min, carbonization temperature of 1100 °C, holding time of 2 h, glassy carbon deposited titanium dioxide nanospheres were obtained;
[0112] S4. Preparation of aminosilane-modified nanospheres: 10 parts by weight of the glassy carbon-deposited titanium dioxide nanospheres prepared in step S3 were added to 100 parts by weight of ethanol, 1.5 parts by weight of aminosilane were added, heated to 45° C., stirred for 3 h, centrifuged, washed, and dried to obtain aminosilane-modified nanospheres;
[0113] The aminosilane is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, with a mass ratio of 4:2;
[0114] S5. Quaternization reaction: 10 parts by weight of the aminosilane-modified nanospheres prepared in step S4 were added to 12 parts by weight of water, 4 parts by weight of formic acid, 6 parts by weight of a 37wt% formaldehyde solution were added, heated to 70°C, stirred for 22h, centrifuged, washed, dried, added to 50 parts by weight of N-methyl-2-pyrrolidone, 1.5 parts by weight of iodomethane were added, stirred for 13.5h, centrifuged, washed, and dried to obtain quaternized modified nanospheres;
[0115] S6. Preparation of PET additive masterbatch: 11 parts by weight of the quaternary ammonium modified nanospheres prepared in step S5, 3 parts by weight of epoxy soybean octyl ester and 100 parts by weight of PET resin are melt-mixed at 255°C, extruded and granulated to prepare PET additive masterbatch.
[0116] Comparative Example 6
[0117] Compared with the embodiment 3, the difference is that steps S4 and S5 are not performed.
[0118] The details are as follows:
[0119] S1. Preparation of titanium dioxide nanospheres: 17 parts by weight of tetrabutyl titanate was dissolved in 65 parts by weight of ethanol, 6 parts by weight of 22 wt% ammonia water was added dropwise, the reaction was stirred for 30 min, centrifuged, washed, dried, ball milled for 2 h, and calcined at 500 ° C for 2 h to obtain titanium dioxide nanospheres;
[0120] S2. Preparation of modified titanium dioxide nanospheres: 17 parts by weight of the titanium dioxide nanospheres prepared in step S1 were added to 200 parts by weight of water, 8.5 parts by weight of tannic acid and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified titanium dioxide nanospheres;
[0121] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0122] S3. Preparation of N / S-doped glassy carbon deposited titanium dioxide nanospheres: 17 parts by weight of phenolic resin, 6 parts by weight of cellulose, 30 parts by weight of modified titanium dioxide nanospheres prepared in step S2, 3 parts by weight of melamine and 1.5 parts by weight of thiourea were mixed and ball-milled uniformly, and vacuum carbonized at a vacuum degree of 3.5×10 -2 Pa, heating rate of 12 °C / min, carbonization temperature of 1100 °C, holding time of 2 h, and N / S-doped glassy carbon deposited titanium dioxide nanospheres were obtained;
[0123] S4. Preparation of PET additive masterbatch: 11 parts by weight of N / S-doped glassy carbon-deposited titanium dioxide nanospheres obtained in step S3, 3 parts by weight of epoxy soybean octyl ester and 100 parts by weight of PET resin are melt-mixed at 255°C, extruded and granulated to obtain PET additive masterbatch.
[0124] Comparative Example 7
[0125] Compared with Example 3, the difference is that no epoxy soybean octyl ester is added in step S6.
[0126] The details are as follows:
[0127] S1. Preparation of titanium dioxide nanospheres: 17 parts by weight of tetrabutyl titanate was dissolved in 65 parts by weight of ethanol, 6 parts by weight of 22 wt% ammonia water was added dropwise, the reaction was stirred for 30 min, centrifuged, washed, dried, ball milled for 2 h, and calcined at 500 ° C for 2 h to obtain titanium dioxide nanospheres;
[0128] S2. Preparation of modified titanium dioxide nanospheres: 17 parts by weight of the titanium dioxide nanospheres prepared in step S1 were added to 200 parts by weight of water, 8.5 parts by weight of tannic acid and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified titanium dioxide nanospheres;
[0129] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0130] S3. Preparation of N / S-doped glassy carbon deposited titanium dioxide nanospheres: 17 parts by weight of phenolic resin, 6 parts by weight of cellulose, 30 parts by weight of modified titanium dioxide nanospheres prepared in step S2, 3 parts by weight of melamine and 1.5 parts by weight of thiourea were mixed and ball-milled uniformly, and vacuum carbonized at a vacuum degree of 3.5×10 -2 Pa, heating rate of 12 °C / min, carbonization temperature of 1100 °C, holding time of 2 h, and N / S-doped glassy carbon deposited titanium dioxide nanospheres were obtained;
[0131] S4. Preparation of aminosilane-modified nanospheres: 10 parts by weight of the N / S-doped glassy carbon-deposited titanium dioxide nanospheres prepared in step S3 were added to 100 parts by weight of ethanol, 1.5 parts by weight of aminosilane were added, the mixture was heated to 45° C., stirred for 3 h, centrifuged, washed, and dried to obtain aminosilane-modified nanospheres;
[0132] The aminosilane is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, with a mass ratio of 4:2;
[0133] S5. Quaternization reaction: 10 parts by weight of the aminosilane-modified nanospheres prepared in step S4 were added to 12 parts by weight of water, 4 parts by weight of formic acid, 6 parts by weight of a 37wt% formaldehyde solution were added, heated to 70°C, stirred for 22h, centrifuged, washed, dried, added to 50 parts by weight of N-methyl-2-pyrrolidone, 1.5 parts by weight of iodomethane were added, stirred for 13.5h, centrifuged, washed, and dried to obtain quaternized modified nanospheres;
[0134] S6. Preparation of PET additive masterbatch: 14 parts by weight of the quaternary ammonium modified nanospheres obtained in step S5 and 100 parts by weight of PET resin are melt-mixed at 255° C. and extruded into granules to obtain PET additive masterbatch.
[0135] Test Example 1
[0136] The PET additive masterbatch prepared in Examples 1-5 and Comparative Examples 1-7 was added to PET resin in an amount of 8 wt %, and a 300 um thick PET sheet was obtained by extrusion for performance testing.
[0137] The tensile properties were tested according to the method in standard GB / T 1040-2018 "Determination of tensile properties of plastics".
[0138] The cantilever beam impact strength test was carried out according to the method in standard GB / T 1843-2008 "Determination of cantilever beam impact strength of plastics".
[0139] The transmittance and haze were measured according to the method in standard GB / T 2410-2008 “Determination of light transmittance and haze of transparent plastics”.
[0140] The surface resistance is tested in accordance with the standard GB / T 1410-2006 “Test methods for volume resistivity and surface resistivity of solid insulating materials”.
[0141] The results are shown in Table 1.
[0142] Table 1
[0143]
[0144]
[0145] It can be seen from the above table that the PET additive masterbatch prepared in Examples 1-3 of the present invention can significantly improve the comprehensive performance of PET resin, reduce surface resistance, and improve antistatic performance.
[0146] Test Example 2
[0147] The PET additive masterbatch prepared in Examples 1-5 and Comparative Examples 1-7 was added to the PET resin in an amount of 8 wt %, and extruded to obtain a 300 um thick PET sheet.
[0148] The antibacterial test was carried out according to the test method 1 film sticking method of the standard GB / T 31402-2015 "Test method for antibacterial performance of plastic surfaces".
[0149] The mildew resistance test was carried out according to the test method of standard QB / T 2591-2003 "Antibacterial plastics - Test methods for antibacterial properties and antibacterial effects".
[0150] Bacteria used for detection: Escherichia coli (ATCC25922), Aspergillus niger (ATCC20611) and Candida albicans (ATCC10231).
[0151] The results are shown in Table 2.
[0152] Table 2
[0153]
[0154]
[0155] It can be seen from the above table that the PET additive masterbatch prepared in Examples 1-3 of the present invention can significantly improve the antibacterial and anti-mildew properties of PET resin.
[0156] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a PET additive masterbatch, characterized in that: The following steps are involved: S1. Preparation of titanium dioxide nanospheres: tetrabutyl titanate was dissolved in ethanol, ammonia water was added dropwise, stirred for reaction, centrifuged, washed, dried, ball-milled, and calcined to obtain titanium dioxide nanospheres; S2. Preparation of modified titanium dioxide nanospheres: adding titanium dioxide nanospheres to water, adding tannic acid and a catalyst, heating and stirring to react, centrifuging, washing, and drying to obtain modified titanium dioxide nanospheres; S3. Preparation of N / S-doped glassy carbon-deposited titanium dioxide nanospheres: phenolic resin, cellulose, modified titanium dioxide nanospheres, melamine and thiourea were mixed and ball-milled uniformly, and vacuum carbonized to obtain N / S-doped glassy carbon-deposited titanium dioxide nanospheres; S4. Preparation of aminosilane-modified nanospheres: adding the N / S-doped glassy carbon-deposited titanium dioxide nanospheres obtained in step S3 to ethanol, adding aminosilane, heating and stirring the reaction, centrifuging, washing, and drying to obtain aminosilane-modified nanospheres; S5 quaternization reaction: the aminosilane-modified nanospheres obtained in step S4 were added to water, formic acid and formaldehyde solution were added, the reaction was heated and stirred, centrifuged, washed, dried, added to N-methyl-2-pyrrolidone, iodomethane was added, the reaction was stirred, centrifuged, washed, and dried to obtain quaternary ammonium modified nanospheres; S6. Preparation of PET additive masterbatch: The quaternary ammonium modified nanospheres, plasticizer and PET resin prepared in step S5 are melt-mixed and extruded into granules to prepare PET additive masterbatch.
2. The method for preparing the PET auxiliary agent masterbatch according to claim 1, characterized in that: In step S1, the mass ratio of tetrabutyl titanate, ethanol and ammonia water is 15-20:60-70:5-7, the concentration of ammonia water is 20-25wt%, the stirring reaction time is 20-40min, the ball milling time is 1-3h, the calcination temperature is 450-550°C, and the time is 1-3h.
3. The method for preparing the PET auxiliary agent masterbatch according to claim 1, characterized in that: The mass ratio of the titanium dioxide nanospheres, tannic acid and catalyst in step S2 is 15-20:7-10:1-2, the catalyst is a Tris-HCl solution with a pH of 8.5-9, the temperature of the heating and stirring reaction is 40-50° C., and the time is 1-3 hours.
4. The method for preparing the PET additive masterbatch according to claim 1, characterized in that: The mass ratio of the phenolic resin, cellulose, modified titanium dioxide nanospheres, melamine and thiourea in step S3 is 15-20:5-7:27-32:2-4:1-2, and the vacuum degree of the vacuum carbonization is 2-5×10 -2 Pa, heating rate is 10-15℃ / min, carbonization temperature is 1000-1200℃, and holding time is 1-3h.
5. The method for preparing PET additive masterbatch according to claim 1, characterized in that: The mass ratio of the N / S-doped glassy carbon-deposited titanium dioxide nanospheres and the aminosilane in step S4 is 10:1-2, and the aminosilane is selected from at least one of aminopropyltrimethoxysilane, aminopropyltriethoxysilane, N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, and γ-aminoethylaminopropyltrimethoxysilane. The temperature of the heating and stirring reaction is 40-50°C and the time is 2-4h.
6. The method for preparing the PET additive masterbatch according to claim 5, characterized in that: The aminosilane is a mixture of N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane, with a mass ratio of 3-5:
2.
7. The method for preparing the PET additive masterbatch according to claim 1, characterized in that: In step S5, the mass ratio of aminosilane-modified nanospheres, formic acid, formaldehyde solution, water, and methyl iodide is 10:3-5:5-7:10-15:1-2, the concentration of the formaldehyde solution is 35-40wt%, the temperature of the heating and stirring reaction is 65-75°C, the time is 20-24h, and the stirring reaction time is 12-15h.
8. The method for preparing PET additive masterbatch according to claim 1, characterized in that: The mass ratio of the quaternized modified nanospheres, the plasticizer and the PET resin in step S6 is 10-12:2-4:100, the plasticizer is selected from at least one of epoxy soybean oil, epoxy acetyl linolenic acid methyl ester, epoxy furoate butyl ester, epoxy silkworm pupa oleic acid butyl ester, epoxy soybean oleate octyl ester, 9,10-epoxy stearic acid octyl ester, dioctyl adipate, dioctyl sebacate and diisononyl adipate, and the melting temperature is 250-260°C.
9. A PET additive masterbatch obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the PET additive masterbatch as claimed in claim 9 in the preparation of antistatic PET resin.