A high-strength and tough oil well pipe for shale gas and its manufacturing process
Through the high-strength oil well pipe manufacturing process, combined with self-healing polyurethane emulsion and composite silica coating, the corrosion resistance problem of carbon steel pipes in shale gas wells has been solved, and a high-strength and long-life oil well pipe design has been achieved.
Patent Information
- Application Number
- CN202410608983.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-16
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-05-16
AI Technical Summary
Existing carbon steel pipes cannot meet the long-term service and corrosion resistance requirements of shale gas wells. How to develop a pipeline with high strength, toughness and high corrosion resistance.
High-strength oil well pipe manufacturing processes are adopted, including refining, vacuum degassing, continuous casting, rolling, annealing, drilling, hot continuous rolling, tension reduction, segmented heat treatment, and the surface of the pipe body is coated with self-healing polyurethane emulsion and Protective coating prepared from composite silica.
The prepared oil well pipe has high mechanical strength, self-healing super-hydrophobic, corrosion-resistant, and anti-fouling surfaces. Its mechanical properties meet the requirements of oil fields and extends its service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil well pipes, in particular to a high-strength and tough oil well pipe for shale gas and a manufacturing process thereof. Background Art
[0002] With the advancement of science and technology, human beings are paying more and more attention to clean energy. Among them, shale gas as a kind of clean energy has become more and more eye-catching. The vertical depth of shale gas wells in my country is generally 2000-4500 meters. The formations in some well areas contain high concentrations of corrosive media such as carbon dioxide and chloride ions. Therefore, there are higher requirements for the pipelines used in shale gas extraction.
[0003] At present, conventional carbon steel pipes can no longer meet the long-term service and corrosion resistance requirements of shale gas wells. How to develop a pipeline with both high strength and high corrosion resistance is a research hotspot in this industry and has practical significance and economic value. Summary of the invention
[0004] The object of the present invention is to provide a high-strength and tough oil well pipe for shale gas and a manufacturing process thereof, so as to solve the problems in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A manufacturing process of high-strength and tough oil well pipe for shale gas, comprising the following steps:
[0007] S1: Put the raw materials into an electric furnace, and perform refining, vacuum degassing, continuous casting, rolling, and annealing in sequence to obtain a round tube billet;
[0008] S2: Punching is performed at the tail of the round tube billet, followed by heating, punching, hot rolling, tension reducing treatment, and cooling to obtain a tube body;
[0009] S3: performing segmented heat treatment on the tube body to obtain a heat-treated tube body;
[0010] S4: Preparation of protective coatings using self-healing polyurethane emulsion and composite silica;
[0011] S5: coating the protective coating on the heat-treated pipe body, coupling threading and threaded surface, drying, and assembling to obtain a high-strength and tough oil well pipe for shale gas.
[0012] Furthermore, in terms of mass percentage, the raw material composition is: Si: 0.15-0.4, Mn: 0.3-0.5, Cr: 11.5-13.5, Mo: 1.9-2.1, Ni: 4.8-6, Cu: 0-0.2, V: 0.07-0.11, Nb: 0.01-0.03, Al: 0.01-0.05, N: 0.03-0.06, Ti: 0-0.02, C0-0.03, P: 0-0.018, S: 0-0.003, and the balance is Fe.
[0013] Furthermore, in step S1, the rolling ratio of the rolling treatment is 3-3.2; the working conditions of the annealing treatment are: keeping warm at 760-770°C for 8-9h.
[0014] Furthermore, in step S2, the working conditions of the punching treatment are: the punching diameter is 60-80mm, and the punching depth is 80mm; the working conditions of the heating treatment are: the temperature is 1210-1230℃; the working conditions of the perforation treatment are: the temperature is 1180-1220℃; the working conditions of the hot rolling treatment are: pressing with a PQF three-roller rolling mill, a preheating temperature of 90-100℃, a graphite lubrication speed of 0.8m / s, and a lubrication pressure of 45-48bar.
[0015] Furthermore, in step S3, the working conditions of the staged heat treatment are: keeping at 955-965°C for 25-30 min, then cooling to 600-620°C for 55-60 min, and air cooling.
[0016] Furthermore, the mass ratio of the self-healing polyurethane emulsion and the composite silica is 50:(3-4).
[0017] Further, the preparation of composite silicon dioxide comprises the following steps:
[0018] 1) Mix ethanol and deionized water, add tetraethyl silicate, hexadecyltrimethylammonium bromide and ammonia water, stir for 2-3 hours, centrifuge, wash, dry, keep at 200°C for 2 hours, heat to 600°C for 6 hours, and obtain pretreated silica microspheres; mix 2-mercaptobenzothiazole and ethanol, add silica microspheres, ultrasonically treat for 20-30 minutes, then stir for 46-48 hours, centrifuge and dry to obtain silica microspheres;
[0019] 2) Mix n-butanol, micronized silica, silica microspheres, ammonia water and deionized water, perform ultrasonic oscillation for 10-20 minutes, heat to 78-82°C in an oil bath and keep warm for 5-6 hours, add composite siloxane and γ-aminopropyltriethoxysilane, keep warm for 1-2 hours, centrifuge, wash, dry and grind to obtain composite silica.
[0020] Furthermore, the preparation of the self-repairing polyurethane emulsion comprises the following steps:
[0021] In a nitrogen atmosphere, poly(1,4-butylene adipate) ester diol and polyether polyol are mixed, the temperature is raised to 68-72°C and kept for 20-30 minutes, isophorone diisocyanate, dibutyltin dilaurate and N,N-dimethylformamide are added, the temperature is raised to 78-82°C and kept for 2-3 hours to obtain a prepolymer; in a nitrogen atmosphere, 2,2-bis(hydroxymethyl)propionic acid is added to the prepolymer, the temperature is lowered to 58-62°C and kept for 2 hours, 1,4-butanediol, composite siloxane and N,N-dimethylformamide are added, the temperature is kept for 1-2 hours, the temperature is lowered to 38-42°C, triethylamine is added and kept for 20-30 minutes, and then the mixture is poured into a mixed solution of ethylenediamine, diethylenetriamine and deionized water, emulsified in an ice water bath for 8-10 minutes, and rotary evaporated to obtain a self-healing polyurethane emulsion.
[0022] Furthermore, in the preparation of composite silica, the mass ratio of micron silica, silica microspheres, composite siloxane, and γ-aminopropyltriethoxysilane is 2:3:4:1.
[0023] Further, the preparation of the composite siloxane comprises the following steps:
[0024] (1) Under a nitrogen atmosphere, 4-vinylbenzeneboronic acid, anhydrous sodium sulfate and tetrahydrofuran are mixed, kept at 48-52° C. for 22-24 hours, and rotary evaporated and dried to obtain tri(vinylbenzene)boroxane;
[0025] (2) Vinyl polydimethylsiloxane, dodecafluoroheptyl methacrylate, pentaerythritol triacrylate and tetrahydrofuran are mixed, tri(vinylbenzene)boroxane, benzoyl peroxide and 2,2-azobisisobutyronitrile are added, the mixture is heated at 18-25°C for 10-12 hours, rotary evaporated, heated at 160°C for 2-3 minutes, toluene is added, and the mixture is precipitated with petroleum ether for 3-5 times and dried to obtain a composite siloxane.
[0026] Beneficial effects of the present invention:
[0027] The present invention provides a high-strength and tough oil well pipe for shale gas and a manufacturing process thereof. By adjusting the composition and process, the prepared oil well pipe has high mechanical strength and a self-repairing super-hydrophobic, corrosion-resistant and anti-fouling surface.
[0028] The present invention adopts a hot rolling process to produce oil well pipes. In step S1, the rolling ratio is controlled to be 3-3.2 to improve the core quality of the ingot and reduce the inner surface defects after rolling. By controlling the working conditions of the annealing treatment, cracking of the ingot is prevented. Through process design, the yield rate is above 90%, the tensile strength is above 998MPa, and the mechanical properties fully meet the requirements of oil field use. Compared with the common hot extrusion process on the market, the processing efficiency is high and the dimensional accuracy is high.
[0029] In order to improve the corrosion resistance of the oil well pipe surface and give it excellent resistance to mechanical damage, a protective coating prepared from self-repairing polyurethane emulsion and composite silica is coated on the surface of the oil well pipe components, giving the oil well pipe a corrosion-resistant, super-hydrophobic and anti-fouling surface that can self-repair at room temperature, thereby extending its service life.
[0030] At present, the industry generally selects water-based polyurethane coatings that are environmentally friendly, safe in storage and transportation, have good wear resistance, and strong adhesion as anti-corrosion coatings. However, due to the introduction of some hydrophilic groups, its water resistance will be affected to a certain extent. In order to solve this problem, the present invention uses isophorone diisocyanate as a hard segment, and poly(1,4-butylene adipate diol) partially replaces polyether polyol as a soft segment. The prepolymer is synthesized under the action of a catalyst, 2,2-bis(hydroxymethyl)propionic acid is used as a hydrophilic group, 1,4-butylene glycol is used as a chain extender, composite siloxane is used as a capping agent, and triethylamine is used as a neutralizing agent. The invention relates to a novel self-repairing aqueous polyurethane emulsion, wherein ethylenediamine and diethylenetriamine are used as amine cross-linking agents, and a self-healing aqueous polyurethane emulsion is synthesized. The composite siloxane is formed by free radical polymerization of a monomer formed by dehydration of 4-vinylbenzeneboronic acid and vinyl silicone oil, dodecafluoroheptyl methacrylate, and pentaerythritol triacrylate. The composite siloxane having a BO six-membered ring dynamic cross-linking network, a fluorinated group, and a hydroxyl group is prepared and introduced into the aqueous polyurethane emulsion, thereby enabling the coating to achieve rapid self-repairing at room temperature, in water environment, and at low temperature. At the same time, the "sacrificial bond" effect of the dynamic bond gives the coating good impact resistance and water resistance.
[0031] In order to further improve the corrosion resistance of the coating, composite silica is introduced as a coating filler and coated on the surface of the component to form a super hydrophobic, wear-resistant and anti-fouling protective layer. The mass ratio of silica nanospheres and micron silica coated with 2-mercaptobenzothiazole is controlled to form a micro-nano structure on the coating surface to improve the hydrophobicity of the coating. In order to improve the uniformity of dispersion of silica nanospheres and micron silica in the coating, silica nanospheres and micron silica are treated with composite siloxane and γ-aminopropyltriethoxysilane to improve their dispersibility while further improving their hydrophobicity and corrosion resistance. When the coating is scratched, while it is self-repairing, 2-mercaptobenzothiazole will be slowly released and strongly chemically adsorbed on the surface of the substrate, thereby blocking the corrosion of the substrate by the corrosive medium in the external environment, effectively extending the service life of the coating. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] It should be noted that if the embodiments of the present invention involve directional indications such as up, down, left, right, front, and back, the directional indication is only used to explain a specific posture such as the relative position relationship between the components, the movement status, etc. If the specific posture changes, the directional indication will also change accordingly. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.
[0034] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0035] Embodiment 1: A manufacturing process of a high-strength and tough oil well pipe for shale gas, comprising the following steps:
[0036] S1: Put the raw materials into an electric furnace, and perform refining, vacuum degassing, continuous casting, rolling, and annealing in sequence to obtain a round tube billet;
[0037] In step S1, the rolling ratio of the rolling treatment is 3; the working conditions of the annealing treatment are: keeping at 760°C for 9 hours;
[0038] S2: Punching is performed at the tail of the round tube billet, followed by heating, punching, hot rolling, tension reducing treatment, and cooling to obtain a tube body;
[0039] In step S2, the working conditions of the punching treatment are: the punching diameter is 60 mm, the punching depth is 80 mm; the working conditions of the heating treatment are: the temperature is 1210°C; the working conditions of the perforation treatment are: the temperature is 1180°C; the working conditions of the hot rolling treatment are: pressing by a PQF three-roller continuous rolling unit, the preheating temperature is 90°C, the graphite lubrication speed is 0.8 m / s, and the lubrication pressure is 45 bar;
[0040] S3: performing segmented heat treatment on the tube body to obtain a heat-treated tube body;
[0041] The working conditions of the staged heat treatment are: keep at 955℃ for 30min, then cool to 600℃ for 60min, and air cool;
[0042] S4: Preparation of protective coatings using self-healing polyurethane emulsion and composite silica;
[0043] The mass ratio of self-repairing polyurethane emulsion and composite silica is 50:3;
[0044] The preparation of the composite silicon dioxide comprises the following steps:
[0045] 1) Mix 2 mL of ethanol and 50 mL of deionized water, add 1 mL of tetraethyl silicate, 0.16 g of hexadecyltrimethylammonium bromide, and 1 mL of ammonia water, stir at 100 r / min for 2 h, centrifuge, wash, dry, keep at 200 ° C for 2 h, heat to 600 ° C for 6 h, and obtain pretreated silica microspheres; mix 8 mg of 2-mercaptobenzothiazole and 200 mL of ethanol, add 0.8 g of silica microspheres, ultrasonically treat for 20 min, then stir for 46 h, centrifuge, and dry to obtain silica microspheres;
[0046] 2) 50g of n-butanol, 2g of micronized silica, 3g of silica microspheres, 6g of ammonia water, and 4g of deionized water were mixed, ultrasonically vibrated for 10min, placed in an oil bath and heated to 78°C for 6h, 4g of composite siloxane and 1g of γ-aminopropyltriethoxysilane were added, and the mixture was kept warm for 1h, centrifuged, washed, dried, and ground to obtain composite silica;
[0047] The preparation of the self-repairing polyurethane emulsion comprises the following steps:
[0048] In a nitrogen atmosphere, 8 g of poly(1,4-butylene adipate) diol and 16 g of polyether polyol were mixed, the temperature was raised to 68 ° C for 30 min, 9.6 g of isophorone diisocyanate, 2 drops of dibutyltin dilaurate, and 6 mL of N,N-dimethylformamide were added, the temperature was raised to 78 ° C for 3 h to obtain a prepolymer; in a nitrogen atmosphere, 0.8 g of 2,2-bis(hydroxymethyl)propionic acid was added to the prepolymer, the temperature was lowered to 58 ° C for 3 h, and the mixture was heated to 78 ° C for 3 h. 2h, add 0.5g 1,4-butanediol, 2g composite siloxane, 6mL N,N-dimethylformamide, continue to keep warm for 1h, cool to 38°C, add 0.1g triethylamine and keep warm for 20min, then pour it into a mixed solution of 0.1g ethylenediamine, 0.3g diethylenetriamine, and 100mL deionized water, emulsify at 8000r / min for 8min in an ice water bath, and rotary evaporate to obtain a self-repairing polyurethane emulsion;
[0049] The preparation of the composite siloxane comprises the following steps:
[0050] (1) Under a nitrogen atmosphere, 13.5 mmol 4-vinylbenzene boronic acid, 42.2 mmol anhydrous sodium sulfate, and 20 mL tetrahydrofuran were mixed, kept at 48 °C for 24 h, and rotary evaporated and dried to obtain tri(vinylbenzene)boroxane;
[0051] (2) 3 g of vinyl polydimethylsiloxane, 0.06 g of dodecafluoroheptyl methacrylate, 0.1 g of pentaerythritol triacrylate, and 3 mL of tetrahydrofuran were mixed, and 0.07 g of tri(vinylbenzene)boroxane, 10 mg of benzoyl peroxide, and 10 mg of 2,2-azobisisobutyronitrile were added. The mixture was kept at 18°C for 12 h, and then rotary evaporated. The mixture was kept at 160°C for 2 min, and 20 mL of toluene was added. The mixture was precipitated with petroleum ether for 3 times, and dried to obtain a composite siloxane.
[0052] S5: coating the protective coating on the heat-treated pipe body, coupling threading and threaded surface, drying, and assembling to obtain a high-strength and tough oil well pipe for shale gas.
[0053] Embodiment 2: A manufacturing process of a high-strength and tough oil well pipe for shale gas, comprising the following steps:
[0054] S1: Put the raw materials into an electric furnace, and perform refining, vacuum degassing, continuous casting, rolling, and annealing in sequence to obtain a round tube billet;
[0055] In step S1, the rolling ratio of the rolling treatment is 3.1; the working conditions of the annealing treatment are: keeping at 765°C for 8.5h;
[0056] S2: Punching is performed at the tail of the round tube billet, followed by heating, punching, hot rolling, tension reducing treatment, and cooling to obtain a tube body;
[0057] In step S2, the working conditions of the punching treatment are: the punching diameter is 70 mm, the punching depth is 80 mm; the working conditions of the heating treatment are: the temperature is 1220°C; the working conditions of the perforation treatment are: the temperature is 1200°C; the working conditions of the hot rolling treatment are: pressing by a PQF three-roller continuous rolling unit, the preheating temperature is 95°C, the graphite lubrication speed is 0.8 m / s, and the lubrication pressure is 47 bar;
[0058] S3: performing segmented heat treatment on the tube body to obtain a heat-treated tube body;
[0059] The working conditions of the staged heat treatment are: keep at 960℃ for 28min, then cool to 610℃ for 58min, and air cool;
[0060] S4: Preparation of protective coatings using self-healing polyurethane emulsion and composite silica;
[0061] The mass ratio of self-repairing polyurethane emulsion and composite silica is 50:3.5;
[0062] The preparation of the composite silicon dioxide comprises the following steps:
[0063] 1) Mix 2 mL of ethanol and 50 mL of deionized water, add 1 mL of tetraethyl silicate, 0.16 g of hexadecyltrimethylammonium bromide, and 1 mL of ammonia water, stir at 100 r / min for 2.5 h, centrifuge, wash, dry, keep at 200 ° C for 2 h, heat to 600 ° C for 6 h, and obtain pretreated silica microspheres; mix 8 mg of 2-mercaptobenzothiazole and 200 mL of ethanol, add 0.8 g of silica microspheres, ultrasonically treat for 25 min, then stir for 47 h, centrifuge, and dry to obtain silica microspheres;
[0064] 2) 50g of n-butanol, 2g of micronized silica, 3g of silica microspheres, 6g of ammonia water, and 4g of deionized water were mixed, ultrasonically vibrated for 15min, placed in an oil bath and heated to 80°C for 5.5h, 4g of composite siloxane and 1g of γ-aminopropyltriethoxysilane were added, and the mixture was kept warm for 1.5h, centrifuged, washed, dried, and ground to obtain composite silica;
[0065] The preparation of the self-repairing polyurethane emulsion comprises the following steps:
[0066] In a nitrogen atmosphere, 8 g of poly(1,4-butylene adipate) diol and 16 g of polyether polyol were mixed, the temperature was raised to 70 ° C and kept for 25 min, 9.6 g of isophorone diisocyanate, 2 drops of dibutyltin dilaurate, and 6 mL of N,N-dimethylformamide were added, the temperature was raised to 80 ° C and kept for 2.5 h to obtain a prepolymer; in a nitrogen atmosphere, 0.8 g of 2,2-bis(hydroxymethyl)propionic acid was added to the prepolymer, the temperature was lowered to 60 ° C and kept for 1.5 h, add 0.5g 1,4-butanediol, 2g composite siloxane, 6mL N,N-dimethylformamide, continue to keep warm for 1.5h, cool to 40°C, add 0.1g triethylamine and keep warm for 25min, then pour into a mixture of 0.1g ethylenediamine, 0.3g diethylenetriamine, and 100mL deionized water, emulsify at 8000r / min for 8-10min in an ice water bath, and rotary evaporate to obtain a self-repairing polyurethane emulsion;
[0067] The preparation of the composite siloxane comprises the following steps:
[0068] (1) Under a nitrogen atmosphere, 13.5 mmol 4-vinylbenzene boronic acid, 42.2 mmol anhydrous sodium sulfate, and 20 mL tetrahydrofuran were mixed, kept at 50°C for 23 h, and rotary evaporated and dried to obtain tri(vinylbenzene)boroxane;
[0069] (2) 3 g of vinyl polydimethylsiloxane, 0.06 g of dodecafluoroheptyl methacrylate, 0.1 g of pentaerythritol triacrylate, and 3 mL of tetrahydrofuran were mixed, and 0.07 g of tri(vinylbenzene)boroxane, 10 mg of benzoyl peroxide, and 10 mg of 2,2-azobisisobutyronitrile were added. The mixture was kept at 20 °C for 11 h, and then rotary evaporated. The mixture was kept at 160 °C for 2.5 min, and 20 mL of toluene was added. The mixture was precipitated with petroleum ether for 4 times, and dried to obtain a composite siloxane.
[0070] S5: coating the protective coating on the heat-treated pipe body, coupling threading and threaded surface, drying, and assembling to obtain a high-strength and tough oil well pipe for shale gas.
[0071] Embodiment 3: A manufacturing process of a high-strength and tough oil well pipe for shale gas, comprising the following steps:
[0072] S1: Put the raw materials into an electric furnace, and perform refining, vacuum degassing, continuous casting, rolling, and annealing in sequence to obtain a round tube billet;
[0073] In step S1, the rolling ratio of the rolling treatment is 3.2; the working conditions of the annealing treatment are: keeping at 770°C for 8 hours;
[0074] S2: Punching is performed at the tail of the round tube billet, followed by heating, punching, hot rolling, tension reducing treatment, and cooling to obtain a tube body;
[0075] In step S2, the working conditions of the punching treatment are: the punching diameter is 80 mm, the punching depth is 80 mm; the working conditions of the heating treatment are: the temperature is 1230°C; the working conditions of the perforation treatment are: the temperature is 1220°C; the working conditions of the hot rolling treatment are: pressing by a PQF three-roller continuous rolling unit, the preheating temperature is 100°C, the graphite lubrication speed is 0.8 m / s, and the lubrication pressure is 48 bar;
[0076] S3: performing segmented heat treatment on the tube body to obtain a heat-treated tube body;
[0077] The working conditions of the staged heat treatment are: keep at 965℃ for 25min, then cool to 620℃ for 55min, and air cool;
[0078] S4: Preparation of protective coatings using self-healing polyurethane emulsion and composite silica;
[0079] The mass ratio of self-repairing polyurethane emulsion and composite silica is 50:4;
[0080] The preparation of the composite silicon dioxide comprises the following steps:
[0081] 1) Mix 2 mL of ethanol and 50 mL of deionized water, add 1 mL of tetraethyl silicate, 0.16 g of hexadecyltrimethylammonium bromide, and 1 mL of ammonia water, stir at 100 r / min for 3 h, centrifuge, wash, dry, keep at 200 ° C for 2 h, heat to 600 ° C for 6 h, and obtain pretreated silica microspheres; mix 8 mg of 2-mercaptobenzothiazole and 200 mL of ethanol, add 0.8 g of silica microspheres, ultrasonically treat for 30 min, then stir for 48 h, centrifuge, and dry to obtain silica microspheres;
[0082] 2) 50g of n-butanol, 2g of micronized silica, 3g of silica microspheres, 6g of ammonia water and 4g of deionized water were mixed, ultrasonically vibrated for 20min, placed in an oil bath and heated to 82°C for 5h, 4g of composite siloxane and 1g of γ-aminopropyltriethoxysilane were added, and the mixture was kept warm for 2h, centrifuged, washed, dried and ground to obtain composite silica;
[0083] The preparation of the self-repairing polyurethane emulsion comprises the following steps:
[0084] In a nitrogen atmosphere, 8 g of poly(1,4-butylene adipate) diol and 16 g of polyether polyol were mixed, the temperature was raised to 72 ° C and kept for 20 min, 9.6 g of isophorone diisocyanate, 2 drops of dibutyltin dilaurate, and 6 mL of N,N-dimethylformamide were added, the temperature was raised to 82 ° C and kept for 2 h to obtain a prepolymer; in a nitrogen atmosphere, 0.8 g of 2,2-bis(hydroxymethyl)propionic acid was added to the prepolymer, the temperature was lowered to 62 ° C and kept for 1 h, add 0.5g 1,4-butanediol, 2g composite siloxane, 6mL N,N-dimethylformamide, continue to keep warm for 2h, cool down to 42°C, add 0.1g triethylamine and keep warm for 30min, then pour it into a mixed solution of 0.1g ethylenediamine, 0.3g diethylenetriamine, and 100mL deionized water, emulsify at 8000r / min for 10min in an ice water bath, and rotary evaporate to obtain a self-repairing polyurethane emulsion;
[0085] The preparation of the composite siloxane comprises the following steps:
[0086] (1) Under nitrogen atmosphere, 13.5 mmol 4-vinylbenzene boronic acid, 42.2 mmol anhydrous sodium sulfate, and 20 mL tetrahydrofuran were mixed, kept at 52 °C for 22 h, and rotary evaporated and dried to obtain tri(vinylbenzene)boroxane;
[0087] (2) 3 g of vinyl polydimethylsiloxane, 0.06 g of dodecafluoroheptyl methacrylate, 0.1 g of pentaerythritol triacrylate, and 3 mL of tetrahydrofuran were mixed, and 0.07 g of tri(vinylbenzene)boroxane, 10 mg of benzoyl peroxide, and 10 mg of 2,2-azobisisobutyronitrile were added. The mixture was kept at 25 °C for 10 h, and then rotary evaporated. The mixture was kept at 160 °C for 3 min, and 20 mL of toluene was added. The mixture was precipitated with petroleum ether for 5 times and dried to obtain a composite siloxane.
[0088] S5: coating the protective coating on the heat-treated pipe body, coupling threading and threaded surface, drying, and assembling to obtain a high-strength and tough oil well pipe for shale gas.
[0089] Comparative Example 1: Taking Example 3 as the control group, no composite siloxane was added when preparing the self-repairing polyurethane emulsion, and other processes were normal.
[0090] Comparative Example 2: Taking Example 3 as the control group, micron silicon dioxide was used to replace the composite silicon dioxide, and other processes were normal.
[0091] Comparative Example 3: Taking Example 3 as the control group, vinyl polydimethylsiloxane was used to replace the composite siloxane, and the other processes were normal.
[0092] In the embodiments and comparative examples, the raw material compositions are, by mass percentage, Si: 0.26, Mn: 0.41, Cr: 11.92, Mo: 1.94, Ni: 5.51, Cu: 0.06, V: 0.072, Nb: 0.02, Al: 0.03, N: 0.045, Ti: 0.01, P: 0.012, S: 0.001, and the balance is Fe; the size of the heat-treated pipe body is φ139.7 mm and the wall thickness is 12.7 mm. The protective coating is applied to the surface of the heat-treated pipe body for 50 µm, the protective coating is applied to the threaded surface of the coupling for 10 µm, and the protective coating is applied to the threaded surface for 10 µm.
[0093] The sources of raw materials used in the above examples and comparative examples are:
[0094] Polyether polyol 9003-11-6: Hubei Xinhongli Chemical Co., Ltd.; Vinyl polydimethylsiloxane 53529-60-5: Tianmen Hengchang Chemical Co., Ltd.; Tetraethyl silicate T110593, hexadecyltrimethylammonium bromide H108983, 2-mercaptobenzothiazole M104864, micronized silica S104574, γ-aminopropyltriethoxysilane A107147, poly(1,4-butylene adipate) diol B302960, isophorone diisocyanate I109582, dibutyltin dilaurate D100274, N,N-dimethylformamide D1 11999, 2,2-bis(hydroxymethyl)propionic acid B104539, 1,4-butanediol B110391, triethylamine T103285, ethylenediamine E112132, diethylenetriamine D100059, 4-vinylbenzeneboronic acid V684264, tetrahydrofuran T103263, dodecafluoroheptyl methacrylate D301595, pentaerythritol triacrylate P192936, benzoyl peroxide B104630, 2,2-azobisisobutyronitrile A104255: Aladdin reagent; ethanol, ammonia water, n-butanol, sodium sulfate, toluene, petroleum ether, analytical grade: Sinopharm reagent.
[0095] Performance test: The heat-treated tube with a size of φ139.7 mm and a wall thickness of 12.7 mm coated with 50 µm protective coating prepared in the embodiment and comparative example was subjected to performance test; Tensile strength test: The sample size was 20 mm long and tested using a universal tensile testing machine with a tensile rate of 60 mm / min; Self-repair rate: A scratch with a length of 80 µm, a width of 2 µm, and a depth of 50 µm was drawn on the surface of the sample, and the scratch was kept at 18°C for 2 hours. The scratch length was observed using an electron microscope, and the self-repair rate = (L0-L1) / L0×100% (L0-initial scratch length, L1-scratch length after insulation); Water contact angle: Tested using a contact angle tester with a 4 μL deionized water droplet; Adhesion grade: Refer to GB / T 1720-2020 circle test, load 200g, 1 level is the best; Corrosion resistance: refer to GB / T1771-2007 for salt spray resistance test, temperature is 37℃, pH is 6.3, sodium chloride concentration is 60g / L, after 60d of exposure, if the sample does not show discoloration and rust, it is excellent, otherwise it is unqualified; the results are shown in Table 1;
[0096] Table 1
[0097]
[0098] The present invention provides a high-strength and tough oil well pipe for shale gas and a manufacturing process thereof. By adjusting the composition and process, the prepared oil well pipe has high mechanical strength and a self-repairing super-hydrophobic, corrosion-resistant and anti-fouling surface. In Table 1, / indicates that the item has not been tested.
[0099] Comparing Example 3 with Comparative Example 1 and Comparative Example 3, the industry generally selects water-based polyurethane coatings that are environmentally friendly, safe in storage and transportation, have good wear resistance, and strong adhesion as anti-corrosion coatings. However, due to the introduction of some hydrophilic groups, its water resistance will be affected to a certain extent. In order to solve this problem, the present invention uses isophorone diisocyanate as a hard segment, and poly(1,4-butylene adipate diol) partially replaces polyether polyol as a soft segment. The prepolymer is synthesized under the action of a catalyst, 2,2-bis(hydroxymethyl)propionic acid is used as a hydrophilic group, 1,4-butylene glycol is used as a chain extender, and composite siloxane is used as a prepolymer. The end-capping agent, triethylamine is used as a neutralizing agent, and ethylenediamine and diethylenetriamine are used as amine cross-linking agents to synthesize a water-based polyurethane emulsion with self-healing properties, wherein the composite siloxane is formed by free radical polymerization of a monomer formed by dehydration of 4-vinylbenzeneboronic acid and vinyl silicone oil, dodecafluoroheptyl methacrylate, and pentaerythritol triacrylate to prepare a composite siloxane with a BO six-membered ring dynamic cross-linking network, a fluorinated group, and a hydroxyl group, which is introduced into the water-based polyurethane emulsion to enable it to achieve rapid self-healing at room temperature, water environment, and low temperature. At the same time, the "sacrificial bond" effect of the dynamic bond gives the coating good impact resistance and water resistance.
[0100] Example 3 is compared with Comparative Example 2 and Comparative Example 3. In order to further improve the corrosion resistance of the coating, composite silica is introduced as a coating filler and coated on the surface of the component to form a super hydrophobic, wear-resistant and anti-fouling protective layer. The mass ratio of silica nanospheres and micron silica coated with 2-mercaptobenzothiazole is controlled to form a micro-nano structure on the coating surface to improve the hydrophobicity of the coating. In order to improve the uniformity of dispersion of silica nanospheres and micron silica in the coating, the silica nanospheres and micron silica are treated with composite siloxane and γ-aminopropyltriethoxysilane to further improve their hydrophobicity and corrosion resistance while improving their dispersibility. When the coating is scratched, while it is self-repairing, 2-mercaptobenzothiazole will be released and strongly chemically adsorbed on the surface of the substrate, thereby blocking the corrosion of the substrate by the corrosive medium in the external environment, and effectively extending the service life of the coating.
[0101] The above description is only an embodiment of the present invention and does not limit the patent scope of the present invention. All equivalent structural changes made by using the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A manufacturing process for high-strength and tough oil well pipe for shale gas, characterized in that: The following steps are involved: S1: Put the raw materials into an electric furnace, and perform refining, vacuum degassing, continuous casting, rolling, and annealing in sequence to obtain a round tube billet; S2: Punching is performed at the tail of the round tube billet, followed by heating, punching, hot rolling, tension reducing treatment, and cooling to obtain a tube body; S3: performing segmented heat treatment on the tube body to obtain a heat-treated tube body; S4: preparing a protective coating using a self-healing polyurethane emulsion and composite silica, wherein the mass ratio of the self-healing polyurethane emulsion to the composite silica is 50:(3-4); S5: coating the protective coating on the heat-treated pipe body, the threaded coupling and the threaded surface, drying, and assembling to obtain a high-strength and tough oil well pipe for shale gas; The preparation of the composite silicon dioxide comprises the following steps: 1) Mix ethanol and deionized water, add tetraethyl silicate, hexadecyltrimethylammonium bromide and ammonia water, stir for 2-3 hours, centrifuge, wash, dry, keep at 200°C for 2 hours, heat to 600°C for 6 hours, and obtain pretreated silica microspheres; mix 2-mercaptobenzothiazole and ethanol, add silica microspheres, ultrasonically treat for 20-30 minutes, then stir for 46-48 hours, centrifuge and dry to obtain silica microspheres; 2) Mix n-butanol, micronized silica, silica microspheres, ammonia water and deionized water, perform ultrasonic oscillation for 10-20 minutes, place in an oil bath and heat to 78-82°C for 5-6 hours, add composite siloxane and γ-aminopropyltriethoxysilane, continue to heat for 1-2 hours, centrifuge, wash, dry and grind to obtain composite silica; The preparation of the self-repairing polyurethane emulsion comprises the following steps: In a nitrogen atmosphere, poly(1,4-butylene adipate) ester diol and polyether polyol are mixed, heated to 68-72°C and kept warm for 20-30 minutes, isophorone diisocyanate, dibutyltin dilaurate and N,N-dimethylformamide are added, and the temperature is raised to 78-82°C and kept warm for 2-3 hours to obtain a prepolymer; in a nitrogen atmosphere, 2,2-bis(hydroxymethyl)propionic acid is added to the prepolymer, the temperature is lowered to 58-62°C and kept warm for 1-2 hours, 1,4-butanediol, composite siloxane and N,N-dimethylformamide are added, and the temperature is kept warm for 1-2 hours, the temperature is lowered to 38-42°C, triethylamine is added and kept warm for 20-30 minutes, and then the mixture is poured into a mixed solution of ethylenediamine, diethylenetriamine and deionized water, emulsified in an ice water bath for 8-10 minutes, and rotary evaporated to obtain a self-repairing polyurethane emulsion; The preparation of the composite siloxane comprises the following steps: (1) Under a nitrogen atmosphere, 4-vinylbenzeneboronic acid, anhydrous sodium sulfate and tetrahydrofuran are mixed, kept at 48-52° C. for 22-24 hours, and rotary evaporated and dried to obtain tri(vinylbenzene)boroxane; (2) Vinyl polydimethylsiloxane, dodecafluoroheptyl methacrylate, pentaerythritol triacrylate and tetrahydrofuran are mixed, tri(vinylbenzene)boroxane, benzoyl peroxide and 2,2-azobisisobutyronitrile are added, the mixture is heated at 18-25°C for 10-12 hours, rotary evaporated, heated at 160°C for 2-3 minutes, toluene is added, and the mixture is precipitated with petroleum ether for 3-5 times and dried to obtain a composite siloxane.
2. The manufacturing process of a high-strength and tough oil well pipe for shale gas according to claim 1, characterized in that: The raw material composition is, in mass percentage, Si: 0.15-0.4, Mn: 0.3-0.5, Cr: 11.5-13.5, Mo: 1.9-2.1, Ni: 4.8-6, Cu: 0-0.2, V: 0.07-0.11, Nb: 0.01-0.03, Al: 0.01-0.05, N: 0.03-0.06, Ti: 0-0.02, C: 0-0.03, P: 0-0.018, S: 0-0.003, and the balance is Fe.
3. The manufacturing process of a high-strength and tough oil well pipe for shale gas according to claim 1, characterized in that: In step S1, the rolling ratio of the rolling treatment is 3-3.2; the working conditions of the annealing treatment are: keeping warm at 760-770°C for 8-9h.
4. The manufacturing process of a high-strength and tough oil well pipe for shale gas according to claim 1, characterized in that: In step S3, the working conditions of the staged heat treatment are: keeping at 955-965°C for 25-30 min, then cooling to 600-620°C for 55-60 min, and cooling by air cooling.
5. The manufacturing process of a high-strength and tough oil well pipe for shale gas according to claim 1, characterized in that: In the preparation of composite silica, the mass ratio of micron silica, silica microspheres, composite siloxane and γ-aminopropyltriethoxysilane is 2:3:4:
1.
6. A high-strength and tough oil well pipe for shale gas, characterized in that: The invention is manufactured by the manufacturing process according to any one of claims 1 to 5.