Combined passivated back contact cell with specific passivation of the light-receiving surface and its preparation and application
By adopting an alternating semiconductor layer structure of silicon substrate and high-temperature deposition of ultra-thin amorphous silicon layer in the back-contact battery, the problems of high equipment cost and insufficient passivation layer thickness in the existing technology are solved, and the short-circuit current and conversion of the battery are improved. efficiency, reducing equipment costs.
Patent Information
- Application Number
- CN202410831505.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-26
AI Technical Summary
When existing jointly passivated back-contact cells use plate PECVD to deposit an amorphous silicon passivation layer on the light-receiving surface, the equipment cost is high and the thickness of the passivation layer is insufficient, which affects the short-circuit current and conversion efficiency of the cell.
A silicon substrate is used to alternately arrange the first semiconductor layer and the second semiconductor layer on the back side, and a second tunnel oxide layer, an ultra-thin amorphous silicon layer and an anti-reflection layer are formed on the light-receiving surface. The thickness of the ultra-thin amorphous silicon layer is 0.5 -3nm, deposited by tubular PECVD at a high temperature of 300-600°C, combining the structure of metal electrodes and conductive film layers to form a specific passivation layer on the light-receiving surface.
It significantly improves the short-circuit current and conversion efficiency of the battery, while significantly reducing equipment costs. It enhances the passivation effect through a passivation layer structure with an appropriate thickness ratio, replaces plate PECVD to reduce the absorption of the amorphous silicon layer, and improves battery performance.
Smart Images

Figure CN118398679B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of back contact batteries, and in particular relates to a combined passivation back contact battery with a light-receiving surface specifically passivated, and the manufacture and application thereof. Background Art
[0002] In the existing post-texturing method of the combined passivation back contact battery, a passivation layer and an anti-reflection layer are formed on the light-receiving surface. The passivation layer is generally an amorphous silicon passivation layer, and the thickness of the passivation layer is generally 5-15nm. The passivation layer and the anti-reflection layer are generally formed by plate-type PECVD, and the temperature during formation is about 200°C.
[0003] However, the amorphous silicon passivation layer and anti-reflection layer on the light-receiving surface generally need to be deposited using plate-type PECVD. Plate-type PECVD equipment is expensive, which greatly increases the equipment cost. At the same time, the light-receiving surface passivation layer is an amorphous silicon passivation layer with a thickness of about 7nm. A thicker thickness can ensure a certain passivation effect. The absorption coefficient of the amorphous silicon layer is relatively high, thus seriously affecting the short-circuit current of the battery.
[0004] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned defects of the prior art and to provide a combined passivated back contact cell with specific passivation on the light-receiving surface and its preparation and application, which can achieve a higher overall passivation effect, significantly improve the short-circuit current and cell conversion efficiency, and greatly reduce the equipment cost.
[0006] In order to achieve the above-mentioned objectives, in a first aspect, the present invention provides a combined passivated back contact cell with specific passivation on the light-receiving surface, comprising a silicon substrate, a first semiconductor layer and a second semiconductor layer alternately arranged on the back side of the silicon substrate, the two ends of the second semiconductor layer respectively extend outward to cover the outside of the partial back side of the adjacent first semiconductor layer, and a first semiconductor opening area not covering the second semiconductor layer is opened on the back side of the first semiconductor layer, wherein the first semiconductor layer comprises a first tunneling oxide layer and a first doped polycrystalline silicon layer, the second semiconductor layer comprises an intrinsic silicon layer and a second doped silicon layer, and also comprises a second tunneling oxide layer, an ultra-thin amorphous silicon layer and an anti-reflection layer sequentially arranged on the light-receiving surface of the silicon substrate, the thickness of the ultra-thin amorphous silicon layer is 0.5-3nm, and the ratio of the thickness of the second tunneling oxide layer to the ultra-thin amorphous silicon layer is 0.15-1:1.
[0007] In some preferred embodiments of the present invention, the ultra-thin amorphous silicon layer is hydrogenated amorphous silicon, intrinsic amorphous silicon, oxygen-doped amorphous silicon or N-type doped amorphous silicon, and the effective doping concentration of N-type doped amorphous silicon is 3e19cm -3 -3e20cm-3 .
[0008] In some preferred embodiments of the present invention, the ultra-thin amorphous silicon layer is hydrogenated amorphous silicon, and the hydrogen content of the hydrogenated amorphous silicon is 5-15 at.%.
[0009] In some specific embodiments, the ultra-thin amorphous silicon layer is oxygen-doped amorphous silicon, and the oxygen concentration of the oxygen-doped amorphous silicon is 5e18cm -3 -5e21cm -3 .
[0010] In some preferred embodiments of the present invention, the thickness of the ultra-thin amorphous silicon layer is 0.5-1 nm, and / or the thickness of the second tunneling oxide layer is 1-3 nm.
[0011] In some preferred embodiments of the present invention, the thickness ratio of the first tunneling oxide layer, the intrinsic silicon layer, the second tunneling oxide layer, and the ultra-thin amorphous silicon layer is 0.3-4:1.4-16:0.15-1:1.
[0012] In some preferred embodiments of the present invention, the thickness of the first tunneling oxide layer is 1.5-2.5 nm, the thickness of the first doped polysilicon layer is 50-150 nm, and the effective doping concentration is 5e19 cm -3 -5e20cm -3 The thickness of the intrinsic silicon layer is 4-15nm, the thickness of the second doped silicon layer is 8-15nm, and the effective doping concentration is 3e19cm -3 -3e20cm -3 .
[0013] In some preferred embodiments of the present invention, the anti-reflection layer is at least one of silicon nitride, silicon oxynitride and silicon oxide.
[0014] In some preferred embodiments of the present invention, a second semiconductor opening region is formed between adjacent first semiconductor layers, the second semiconductor opening region is arranged at intervals from the first semiconductor opening region, and the area between them is an overlapping region; in the overlapping region, a mask layer is set between the first semiconductor layer and the second semiconductor layer, or no mask layer is set.
[0015] In some preferred embodiments of the present invention, the combined passivated back contact cell with specific passivation on the light-receiving surface also includes a metal electrode and a conductive film layer laid on the outer surfaces of the first semiconductor layer and the second semiconductor layer, and an isolation groove is opened on the portion of the conductive film layer located in the overlapping area; the metal electrode is arranged on the outer surfaces of the conductive film layers corresponding to the second semiconductor opening area and the first semiconductor opening area.
[0016] In a second aspect, the present invention provides a method for manufacturing a combined passivation back contact cell, comprising the following steps:
[0017] S101, providing a double-sided polished silicon substrate;
[0018] S102, forming a first semiconductor layer and a mask layer in sequence on the back side of the silicon substrate, wherein the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer;
[0019] S103, performing a first etching on the back surface obtained in S102 to form a second semiconductor opening region;
[0020] S104, performing texturing cleaning to form a texturing surface on the front surface and the second semiconductor opening area, and then removing the mask layer outside the second semiconductor opening area on the back surface of the silicon substrate;
[0021] S105, forming a second tunneling oxide layer by oxidation on the light-receiving surface of the silicon substrate, and then depositing an ultra-thin amorphous silicon layer and an anti-reflection layer on the outer surface of the second tunneling oxide layer by tubular PECVD at a high temperature of 300-600° C., wherein the thickness of the ultra-thin amorphous silicon layer is 0.5-3 nm, and the ratio of the thickness of the second tunneling oxide layer to the ultra-thin amorphous silicon layer is 0.15-1:1;
[0022] S106, depositing a second semiconductor layer on the back surface obtained in S105, wherein the second semiconductor layer comprises an intrinsic silicon layer and a second doped silicon layer;
[0023] S107 , performing a second etching on a portion of the second semiconductor layer on the back side of the silicon substrate to form a first semiconductor opening region spaced apart from the second semiconductor opening region.
[0024] In some preferred embodiments of the present invention, the deposition conditions of the ultra-thin amorphous silicon layer include: a process pressure of 100-500 Pa and a power of 5-15 kW; and when the ultra-thin amorphous silicon layer is hydrogenated amorphous silicon, silane and hydrogen are introduced, and the flow ratio of silane to hydrogen is 0.1-1:1.
[0025] Preferably, the deposition conditions of the anti-reflection layer include: introducing at least silane and ammonia, a process pressure of 100-500 Pa, and a power of 10-30 kW.
[0026] In some preferred embodiments of the present invention, the method for manufacturing the combined passivation back contact cell further comprises the following steps:
[0027] S108, depositing a conductive film layer on the back surface obtained in S107;
[0028] S109, performing a third etching on a portion of the conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove;
[0029] S110 , forming metal electrodes on the outer surfaces of the corresponding conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
[0030] In a third aspect, the present invention provides a combined passivation back contact cell, which is manufactured by the manufacturing method of the combined passivation back contact cell described in the second aspect.
[0031] In a fourth aspect, the present invention provides a photovoltaic module, which includes the combined passivated back contact cell with specific passivation of the light-receiving surface as described in the first aspect, or includes the combined passivated back contact cell as described in the third aspect.
[0032] Beneficial effects:
[0033] The present invention adopts the above technical scheme, especially sets a second tunneling oxide layer on the light-receiving surface, passivates the interface of the crystalline silicon surface in the silicon substrate through the second tunneling oxide layer, cooperates with the ultra-thin amorphous silicon layer, obtains the passivation enhancement effect, makes up for the defect of reduced passivation effect of the ultra-thin amorphous silicon layer, and cooperates with the combined passivation structure to realize the high-temperature deposition of the ultra-thin amorphous silicon layer and the anti-reflection layer on the front of the battery, while maintaining a high transmittance, so that the overall passivation effect is at a high level, increases the short-circuit current of the battery, and significantly improves the battery conversion efficiency. Among them, the use of the second tunneling oxide layer and the ultra-thin amorphous silicon layer with a suitable thickness ratio enhances the passivation. One possible speculation is that the ultra-thin amorphous silicon layer is easy to carry H, which is conducive to the passivation of the interface between the crystalline silicon in the silicon substrate and the second tunneling oxide layer, and the synergistic passivation of the ultra-thin amorphous silicon layer, thereby promoting the significant enhancement of the passivation effect. Under the same conditions, if the amorphous silicon layer is thicker, the absorption coefficient will be higher, affecting the passivation.
[0034] According to research, in the prior art, there is no tunneling oxide layer between the interface of amorphous silicon and the surface of the silicon substrate. Under high temperature conditions, H overflow will occur at the interface between the silicon substrate and the amorphous silicon, which significantly reduces the passivation effect. Therefore, it can only be deposited at low temperature, and a tubular furnace cannot be used (because the defects of the tubular furnace are relatively large and the effect is poor when performing low-temperature deposition). In the manufacturing method of the present invention, due to the passivation structure of the light-receiving surface, an ultra-thin amorphous silicon layer (or a tunneling oxide layer and an ultra-thin amorphous silicon layer) can be formed at a high temperature of 400-600°C by using tubular PECVD, replacing the need to use plate PECVD to deposit a thicker amorphous silicon layer at a low temperature (about 200°C) in the traditional battery structure. The present invention greatly reduces the absorption of the amorphous silicon layer, thereby increasing the short-circuit current of the battery, thereby improving the battery conversion efficiency. In addition, the use of tubular PECVD to replace plate PECVD greatly reduces the equipment cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0036] Figure 1 is a schematic structural diagram of a silicon substrate provided in Example 1 of the present invention;
[0037] Figure 2 It is a schematic structural diagram of a first semiconductor layer and a mask layer formed sequentially on the back side of Embodiment 1 of the present invention;
[0038] Figure 3 is a schematic structural diagram of forming a second semiconductor opening region on the back side in Embodiment 1 of the present invention;
[0039] Figure 4 It is a schematic structural diagram of the embodiment 1 of the present invention in which the back surface is textured, cleaned and the mask layer is removed;
[0040] Figure 5 It is a schematic structural diagram of forming a second tunneling oxide layer, an ultra-thin amorphous silicon layer and an anti-reflection layer on the light-receiving surface in Embodiment 1 of the present invention;
[0041] Figure 6 is a schematic structural diagram of forming a second semiconductor layer on the back side of Embodiment 1 of the present invention;
[0042] Figure 7 is a schematic structural diagram of forming a first semiconductor opening region on the back side in Embodiment 1 of the present invention;
[0043] Figure 8 is a schematic structural diagram of forming a conductive film layer on the back side of Embodiment 1 of the present invention;
[0044] Fig. 9 is a schematic structural diagram of an isolation groove formed on the back side of Embodiment 1 of the present invention;
[0045] Fig.10 In the first embodiment of the present invention, a metal electrode is formed on the back side.
[0046] Description of Reference Numerals
[0047] 1. Silicon substrate, 2. First tunneling oxide layer, 3. First doped polysilicon layer, 4. Mask layer, 5. Second tunneling oxide layer, 6. Ultra-thin amorphous silicon layer, 7. Anti-reflection layer, 8. Intrinsic amorphous silicon layer, 9. Second doped amorphous silicon layer, 10. Conductive film layer, 11. Metal electrode, W1, second semiconductor opening region, W2, first semiconductor opening region, W3, isolation trench. DETAILED DESCRIPTION
[0048] In the present invention, unless otherwise specified, directional words such as "upper, lower, left, right" are generally understood in conjunction with the directions shown in the drawings and actual applications.
[0049] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0050] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0051] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).
[0052] In the present invention, the area close to the silicon substrate is referred to as the inner part, and the area far from the silicon substrate is referred to as the outer part.
[0053] In a first aspect, the present invention provides a combined passivated back contact cell with specific passivation on the light-receiving surface, comprising a silicon substrate, a first semiconductor layer and a second semiconductor layer alternately arranged on the back side of the silicon substrate, wherein both ends of the second semiconductor layer extend outward to cover the portion of the back side of the adjacent first semiconductor layer, and a first semiconductor opening area not covering the second semiconductor layer is opened on the back side of the first semiconductor layer, wherein the first semiconductor layer comprises a first tunneling oxide layer and a first doped polycrystalline silicon layer, the second semiconductor layer comprises an intrinsic silicon layer and a second doped silicon layer, and further comprises a second tunneling oxide layer, an ultra-thin amorphous silicon layer and an anti-reflection layer sequentially arranged on the light-receiving surface of the silicon substrate, the thickness of the ultra-thin amorphous silicon layer is 0.5-3nm, and the ratio of the thickness of the second tunneling oxide layer to the ultra-thin amorphous silicon layer is 0.15-1:1, preferably 0.40-1:1.
[0054] In some preferred embodiments of the present invention, the ultra-thin amorphous silicon layer is hydrogenated amorphous silicon, intrinsic amorphous silicon, oxygen-doped amorphous silicon or N-type doped amorphous silicon.
[0055] In some specific embodiments, the ultra-thin amorphous silicon layer is oxygen-doped amorphous silicon, and the oxygen concentration of the oxygen-doped amorphous silicon is 5e18cm -3 -5e21cm -3 , which can reduce the absorption of the amorphous silicon layer and is more conducive to improving the short-circuit current and battery efficiency of the battery.
[0056] Preferably, the effective doping concentration of N-type doped amorphous silicon is 3e19cm -3 -3e20cm -3 Using N-type doped amorphous silicon with a suitable doping concentration as the ultra-thin amorphous silicon layer can further enhance the effect of front field passivation and is more conducive to improving the battery conversion efficiency.
[0057] More preferably, the ultra-thin amorphous silicon layer is hydrogenated amorphous silicon, and the hydrogen content of hydrogenated amorphous silicon is 5-15 at.%, preferably 8-15 at.%, which can further improve the interface passivation and, combined with a suitable hydrogen doping concentration, is more conducive to improving the battery conversion efficiency.
[0058] In the present invention, at.% means atomic percentage. Since hydrogen in hydrogenated amorphous silicon is mainly saturated suspended atoms, the content is expressed in atomic percentage.
[0059] In some preferred embodiments of the present invention, the thickness of the ultra-thin amorphous silicon layer is 0.5-3 nm, and / or the thickness of the second tunnel oxide layer is 0.5-1.5 nm. The use of ultra-thin amorphous silicon layer and second tunnel oxide layer of appropriate thickness can take into account the passivation effect of the battery and the absorption of front light, which is more conducive to improving the battery conversion efficiency.
[0060] In some preferred embodiments of the present invention, the thickness ratio of the first tunneling oxide layer, the intrinsic silicon layer, the second tunneling oxide layer, and the ultra-thin amorphous silicon layer is 0.3-4:1.4-16:0.15-1:1, and each passivation layer adopts an appropriate thickness ratio, which is more conducive to improving the battery conversion efficiency.
[0061] In some preferred embodiments of the present invention, the thickness of the first tunneling oxide layer is 1-2 nm, the thickness of the first doped polysilicon layer is 50-150 nm, and the effective doping concentration is 5e19 cm -3 -5e20cm -3 .
[0062] Preferably, the thickness of the intrinsic silicon layer is 4-15 nm, the thickness of the second doped silicon layer is 8-15 nm, and the effective doping concentration is 3e19 cm -3-3e20cm -3 .
[0063] The second doped silicon layer may be doped amorphous silicon or microcrystalline silicon. The intrinsic silicon layer is preferably an intrinsic amorphous silicon layer.
[0064] One of the first doped polysilicon layer and the second doped silicon layer is N-type, and the other is P-type.
[0065] In some preferred embodiments of the present invention, the anti-reflection layer is at least one of silicon nitride, silicon oxynitride and silicon oxide.
[0066] Preferably, the thickness of the anti-reflection layer is 60-90 nm.
[0067] In some preferred embodiments of the present invention, a second semiconductor opening region is formed between adjacent first semiconductor layers, the second semiconductor opening region is arranged at intervals from the first semiconductor opening region, and the area between them is an overlapping region; in the overlapping region, a mask layer is set between the first semiconductor layer and the second semiconductor layer, or no mask layer is set.
[0068] In some preferred embodiments of the present invention, the combined passivated back contact cell with specific passivation on the light-receiving surface also includes a metal electrode and a conductive film layer laid on the outer surfaces of the first semiconductor layer and the second semiconductor layer, and an isolation groove is opened on the portion of the conductive film layer located in the overlapping area; the metal electrode is arranged on the outer surfaces of the conductive film layers corresponding to the second semiconductor opening area and the first semiconductor opening area.
[0069] In a second aspect, the present invention provides a method for manufacturing a combined passivation back contact cell, comprising the following steps:
[0070] S101, providing a double-sided polished silicon substrate;
[0071] S102, forming a first semiconductor layer and a mask layer in sequence on the back side of the silicon substrate, wherein the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer;
[0072] S103, performing a first etching on the back surface obtained in S102 to form a second semiconductor opening region;
[0073] S104, performing texturing cleaning to form a texturing surface on the front surface and the second semiconductor opening area; then removing the mask layer outside the second semiconductor opening area on the back surface of the silicon substrate;
[0074] S105, forming a second tunneling oxide layer by oxidizing the light-receiving surface of the silicon substrate, and then depositing an ultra-thin amorphous silicon layer and an anti-reflection layer on the outer surface of the second tunneling oxide layer by tubular PECVD at a high temperature of 300-600° C. (preferably 400-600° C.), wherein the thickness of the ultra-thin amorphous silicon layer is 0.5-3 nm, and the ratio of the thickness of the second tunneling oxide layer to the ultra-thin amorphous silicon layer is 0.15-1:1;
[0075] S106, depositing a second semiconductor layer on the back surface obtained in S105, wherein the second semiconductor layer comprises an intrinsic silicon layer and a second doped silicon layer;
[0076] S107 , performing a second etching on a portion of the second semiconductor layer on the back side of the silicon substrate to form a first semiconductor opening region spaced apart from the second semiconductor opening region.
[0077] The silicon substrate may be an N-type silicon substrate or a P-type silicon substrate.
[0078] In some preferred embodiments of the present invention, the deposition conditions of the ultra-thin amorphous silicon layer include: process pressure of 100-500 Pa, power of 5-15 kW. Adopting appropriate tubular PECVD deposition conditions to deposit the ultra-thin amorphous silicon layer is more conducive to improving the battery passivation effect.
[0079] Preferably, when the ultra-thin amorphous silicon layer is hydrogenated amorphous silicon, silane and hydrogen are introduced, and the flow ratio of silane to hydrogen is 0.1-1: 1. In the present invention, when the ultra-thin amorphous silicon layer is other types, phosphine, nitrous oxide and other required gases can be introduced as long as the target film layer can be formed.
[0080] Preferably, the deposition conditions of the anti-reflection layer include: introducing at least silane and ammonia, a process pressure of 100-500 Pa, and a power of 10-30 kW. When the anti-reflection layer is other types, nitrous oxide, nitrogen, hydrogen and other required gases can be introduced as long as the target film layer can be formed.
[0081] The formation of the first tunnel oxide layer and the second tunnel oxide layer in the present invention may refer to the prior art, for example, they may be formed by LPCVD, tubular PECVD or any other method.
[0082] It can be understood that in the texturing and cleaning process S104, the mask layer and the first semiconductor layer remaining in the second semiconductor opening region can be removed, and a texturing surface can be formed on the light-receiving surface of the silicon substrate and the second semiconductor opening region.
[0083] In some preferred embodiments of the present invention, the method for manufacturing the combined passivation back contact cell further comprises the following steps:
[0084] S108, depositing a conductive film layer on the back surface obtained in S107;
[0085] S109, performing a third etching on a portion of the conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove;
[0086] S110 , forming metal electrodes on the outer surfaces of the conductive film layers corresponding to the first semiconductor opening region and the second semiconductor opening region.
[0087] The type and thickness of the mask layer in S102 can refer to the prior art, for example, the type can be at least one of silicon nitride, silicon oxide, and silicon oxynitride. The thickness of the mask layer can be, for example, 30-90 nm.
[0088] In a third aspect, the present invention provides a combined passivation back contact cell, which is manufactured by the manufacturing method of the combined passivation back contact cell described in the second aspect.
[0089] In a fourth aspect, the present invention provides a photovoltaic module, which includes the combined passivated back contact cell with specific passivation of the light-receiving surface as described in the first aspect, or includes the combined passivated back contact cell as described in the third aspect.
[0090] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0091] Example 1
[0092] A combined passivation back contact cell is prepared by the following manufacturing method:
[0093] S101, such as Figure 1 As shown, a silicon substrate 1 is provided, and the silicon substrate 1 is polished and cleaned in sequence;
[0094] S102, such as Figure 2 As shown, a first semiconductor layer and a mask layer 4 are sequentially formed on the back of the silicon substrate 1, and the first semiconductor layer includes a first tunneling oxide layer 2 and a first doped polysilicon layer 3 sequentially formed on the back; the thickness of the first tunneling oxide layer 2 is 1.7nm, the thickness of the first doped polysilicon layer 3 is 100nm, and the effective doping concentration is 1e20cm -3 ; The thickness of the mask layer 4 is 60nm, and the mask layer is silicon nitride;
[0095] S103, such as Figure 3 As shown, the first semiconductor layer is first etched on the back surface obtained in S102 to form second semiconductor opening regions W1 distributed at intervals;
[0096] S104, such as Figure 4 As shown, a texture surface is formed in the second semiconductor opening region W1 on the front and back sides through texturing and cleaning, and then the mask layer 4 is removed;
[0097] S105, such as Figure 5 As shown, a second tunneling oxide layer 5, an ultra-thin amorphous silicon layer 6 and an anti-reflection layer 7 are formed on the light-receiving surface of the cell. The thickness of the second tunneling oxide layer 5 is 1nm, the thickness of the ultra-thin amorphous silicon layer 6 is 2nm, and the second tunneling oxide layer 5 is formed by high-temperature oxidation; the ultra-thin amorphous silicon layer 6 and the anti-reflection layer 7 are formed at one time by tubular PECVD, the formation temperature is 450°C, and the formation conditions include: introducing silane and hydrogen, the flow ratio of silane to hydrogen is 0.2:1, the process pressure is 300Pa, the power is 10kW, after deposition to a preset thickness, the power is turned off and the gas is evacuated; then silane and ammonia are introduced, the process pressure is 300Pa, the power is 20kW, and the anti-reflection layer 7 is formed. The ultra-thin amorphous silicon layer 6 is hydrogenated amorphous silicon, and the hydrogen atomic percentage content is 10 at.%, and the anti-reflection layer 7 is silicon nitride, with a thickness of 80nm.
[0098] S106, such as Figure 6 As shown, a second semiconductor layer is formed on the back surface obtained in S105, and the second semiconductor layer includes an intrinsic amorphous silicon layer 8 and a second doped amorphous silicon layer 9 sequentially formed on the back surface; the thickness of the intrinsic amorphous silicon layer 8 is 5nm, the thickness of the second doped amorphous silicon layer 9 is 8nm, and the effective doping concentration is 9e19cm -3 ;
[0099] S107, such as Figure 7 As shown, the polished area of the back surface obtained in S106 is then subjected to a second etching to expose the first semiconductor layer, thereby forming a first semiconductor opening region W2 spaced apart from the second semiconductor opening region W1;
[0100] S108, such as Figure 8 As shown, in S107, a conductive film layer 10 is formed to fully cover the back surface;
[0101] S109, such as Fig. 9 As shown, the conductive film layer 10 portion located between the second semiconductor opening region W1 and the first semiconductor opening region W2 on the back side obtained in S108 is subjected to a third etching to form an isolation groove W3;
[0102] S110, such as Fig.10 As shown, metal electrodes 11 are respectively formed on the outer surfaces of the corresponding regions of the second semiconductor opening region W1 and the first semiconductor opening region W2 on the back side obtained in S109 .
[0103] Example 2
[0104] The method of Example 1 is referred to, except that the ultra-thin amorphous silicon layer is intrinsic amorphous silicon. To meet this condition, the preparation process parameters need to be adjusted: when forming ultra-thin amorphous silicon in S105, only silane is introduced without hydrogen, and other conditions remain the same.
[0105] Example 3
[0106] The method of Example 1 is followed, except that the ultra-thin amorphous silicon layer is N-type doped amorphous silicon and the effective doping concentration is 1e20 cm -3 To meet this condition, the preparation process parameters need to be adjusted: when S105 forms ultra-thin amorphous silicon, silane and phosphine diluted with hydrogen are introduced, the volume flow content of the diluted phosphine is 2%, and the flow ratio of phosphine diluted with hydrogen to silane is 3:1. Other conditions remain the same.
[0107] Example 4
[0108] The method of Example 1 is referred to, except that the thickness of the ultra-thin amorphous silicon layer is 3 nm. According to calculation, the ratio of the thickness of the second tunneling oxide layer to the ultra-thin amorphous silicon layer is 0.33:1.
[0109] Example 5
[0110] The method of Example 1 is referred to, except that the thickness of the second tunneling oxide layer is 0.67 nm. According to calculation, the ratio of the thickness of the second tunneling oxide layer to the ultra-thin amorphous silicon layer is 0.335:1.
[0111] Example 6
[0112] The method of Example 1 is followed, except that the hydrogen atom content of hydrogenated amorphous silicon is 7 at.%, and the process parameters need to be adjusted to meet this condition: when S105 forms ultra-thin amorphous silicon, the flow ratio of silane to hydrogen is 0.4:1, and other conditions remain the same.
[0113] Example 7
[0114] The method of Example 1 is followed, except that the ultra-thin amorphous silicon layer is oxygen-doped amorphous silicon and the oxygen concentration of the oxygen-doped amorphous silicon is 9e20cm -3 To meet this condition, the preparation process parameters need to be adjusted: when S105 forms ultra-thin amorphous silicon, silane and nitrous oxide are introduced, and the flow ratio of silane to hydrogen is 3:1, and other conditions remain the same.
[0115] Comparative Example 1
[0116] The method of Example 1 is referred to, except that the structure of the light-receiving surface is different. Specifically, an ultra-thin amorphous silicon layer and an anti-reflection layer are sequentially formed on the light-receiving surface using a tube furnace, and only a tunneling oxide layer is not formed.
[0117] Comparative Example 2
[0118] The method of comparative example 1 is referred to, except that the ultra-thin amorphous silicon layer is replaced by an intrinsic amorphous silicon layer deposited by plate-type PECVD on the light-receiving surface and has a thickness of 7 nm. To meet this condition, the process parameters need to be adjusted: silane and hydrogen are introduced, the process temperature is 200°C, the process pressure is 100 Pa, and the power is 1 kW.
[0119] Comparative Example 3
[0120] The method of Example 1 is followed, except that the structure of the light-receiving surface is different. Specifically, a plate-type PECVD is used to sequentially form an intrinsic amorphous layer (thickness 4 nm), an N-type doped amorphous layer (thickness 7 nm, effective doping concentration 1e20 cm -3 ) and an anti-reflection layer (same as in Example 1).
[0121] Comparative Example 4
[0122] The method of Example 1 is followed, except that the structure of the light-receiving surface is different. Specifically, a tunneling oxide layer, an N-type doped polysilicon layer (with a thickness of 20 nm and an effective doping concentration of 8e19 cm-1) are sequentially formed on the light-receiving surface. -3 ) and the anti-reflection layer (same as in Example 1), the N-type doped polysilicon layer is formed by tubular PECVD.
[0123] Test Case
[0124] The combined passivated back contact cells obtained in the above embodiments and comparative examples were subjected to performance tests, and the results are shown in Table 1. The short-circuit current and equipment cost of each embodiment and comparative example were converted using embodiment 1 as a reference benchmark, the data of embodiment 1 was normalized benchmark 1, and other examples were converted based on embodiment 1, such as the short-circuit current of comparative example 1 / the raw short-circuit current of embodiment 1 was 0.98.
[0125] Table 1
[0126] Performance Indicators Short circuit current normalized data Battery conversion efficiency Normalized data of equipment cost Example 1 1 26.7% 1 Example 2 1 26.6% 1 Example 3 1 26.68% 1 Example 4 0.99 26.6% 1 Example 5 1 26.6% 1 Example 6 1 26.65% 1 Example 7 1.01 26.65% 1 Comparative Example 1 0.98 25% 0.96 Comparative Example 2 0.98 25.5% 1.15 Comparative Example 3 0.995 26.55% 1.4 Comparative Example 4 0.992 26.2% 1.05
[0127] It can be seen from the above results that, compared with the comparative example, the embodiment of the present invention can achieve a higher overall passivation effect, significantly improve the short-circuit current and battery conversion efficiency, and significantly reduce equipment costs.
[0128] Furthermore, according to Example 1 and Examples 2-6, it can be seen that the preferred battery structure of the present invention is more conducive to improving the short-circuit current and battery conversion efficiency.
[0129] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A combined passivated back contact cell with a light-receiving surface specifically passivated, comprising a silicon substrate, a first semiconductor layer and a second semiconductor layer alternately arranged on the back of the silicon substrate, the two ends of the second semiconductor layer respectively extending outward to cover the back of the adjacent first semiconductor layer, and a first semiconductor opening region not covering the second semiconductor layer is opened on the back of the first semiconductor layer, wherein: The first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer includes an intrinsic silicon layer and a second doped silicon layer. The invention is characterized in that it also includes a second tunneling oxide layer, an ultra-thin amorphous silicon layer and an anti-reflection layer which are sequentially arranged on the light-receiving surface of the silicon substrate, the thickness of the second tunneling oxide layer is 0.5-1.5nm, the thickness of the ultra-thin amorphous silicon layer is 0.5-3nm, and the ratio of the thickness of the second tunneling oxide layer to the ultra-thin amorphous silicon layer is 0.15-1:
1.
2. The combined passivated back contact cell with specific passivation of the light-receiving surface according to claim 1, characterized in that: The ultra-thin amorphous silicon layer is hydrogenated amorphous silicon, intrinsic amorphous silicon, oxygen-doped amorphous silicon or N-type doped amorphous silicon. The oxygen concentration of the oxygen-doped amorphous silicon is 5e18cm -3 -5e21cm -3 The effective doping concentration of N-type doped amorphous silicon is 3e19cm -3 -3e20cm -3 .
3. The combined passivated back contact cell with specific passivation of the light-receiving surface according to claim 2, characterized in that: The ultra-thin amorphous silicon layer is hydrogenated amorphous silicon, and the hydrogen content of the hydrogenated amorphous silicon is 5-15 at.%.
4. The combined passivated back contact cell with specific passivation of the light-receiving surface according to claim 1, characterized in that: The thickness ratio of the first tunneling oxide layer, the intrinsic silicon layer, the second tunneling oxide layer and the ultra-thin amorphous silicon layer is 0.3-4:1.4-16:0.15-1:
1.
5. The combined passivated back contact cell with specific passivation of the light-receiving surface according to claim 1, characterized in that: The thickness of the first tunnel oxide layer is 1-2 nm, the thickness of the first doped polysilicon layer is 50-150 nm, and the effective doping concentration is 5e19 cm -3 -5e20cm -3 The thickness of the intrinsic silicon layer is 4-15nm, the thickness of the second doped silicon layer is 8-15nm, and the effective doping concentration is 3e19cm -3 -3e20cm -3 .
6. The combined passivated back contact cell with specific passivation of the light-receiving surface according to claim 1, characterized in that: A second semiconductor opening region is formed between adjacent first semiconductor layers, the second semiconductor opening region is arranged at intervals from the first semiconductor opening region, and the region between them is an overlapping region; in the overlapping region, a mask layer is disposed between the first semiconductor layer and the second semiconductor layer, or no mask layer is disposed; The combined passivated back contact cell with specific passivation on the light-receiving surface also includes a metal electrode and a conductive film layer laid on the outer surfaces of the first semiconductor layer and the second semiconductor layer, and an isolation groove is opened on the portion of the conductive film layer located in the overlapping area; the metal electrode is arranged on the outer surfaces of the conductive film layers corresponding to the second semiconductor opening area and the first semiconductor opening area.
7. A method for manufacturing a combined passivation back contact battery, characterized in that: The steps include: S101, providing a double-sided polished silicon substrate; S102, forming a first semiconductor layer and a mask layer in sequence on the back side of the silicon substrate, wherein the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer; S103, performing a first etching on the back surface obtained in S102 to form a second semiconductor opening region; S104, performing texturing and cleaning to form a texturing surface on the front surface and the second semiconductor opening area; Then, removing the mask layer outside the second semiconductor opening region on the back side of the silicon substrate; S105, forming a second tunneling oxide layer by oxidation on the light-receiving surface of the silicon substrate, and then depositing an ultra-thin amorphous silicon layer and an anti-reflection layer on the outer surface of the second tunneling oxide layer by tubular PECVD at a high temperature of 300-600° C., wherein the thickness of the ultra-thin amorphous silicon layer is 0.5-3 nm, and the ratio of the thickness of the second tunneling oxide layer to the ultra-thin amorphous silicon layer is 0.15-1:1; S106, depositing a second semiconductor layer on the back surface obtained in S105, wherein the second semiconductor layer comprises an intrinsic silicon layer and a second doped silicon layer; S107 , performing a second etching on a portion of the second semiconductor layer on the back side of the silicon substrate to form a first semiconductor opening region spaced apart from the second semiconductor opening region.
8. The method for manufacturing a combined passivation back contact cell according to claim 7, characterized in that: The deposition conditions of the ultra-thin amorphous silicon layer include: a process pressure of 100-500Pa and a power of 5-15kW; and when the ultra-thin amorphous silicon layer is hydrogenated amorphous silicon, silane and hydrogen are introduced, and the flow ratio of silane to hydrogen is 0.1-1:1; the deposition conditions of the anti-reflection layer include: at least silane and ammonia are introduced, the process pressure is 100-500Pa, and the power is 10-30kW; and / or, The method for manufacturing the combined passivation back contact cell also includes the following steps: S108, depositing a conductive film layer on the back surface obtained in S107; S109, performing a third etching on a portion of the conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove; S110 , forming metal electrodes on the outer surfaces of the corresponding conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
9. A combined passivation back contact cell, characterized in that: The battery is manufactured by the method for manufacturing a combined passivation back contact battery as claimed in claim 7 or 8.
10. A photovoltaic module, characterized in that: It comprises a combined passivated back contact cell with a light-receiving surface specifically passivated as claimed in any one of claims 1 to 6, or comprises a combined passivated back contact cell as claimed in claim 9.
Citation Information
Patent Citations
Combined passivation back contact battery and preparation method thereof
CN115207137A
Double-sided tunneling silicon-oxide passivated back-contact solar cell and preparation method thereof
US20240170590A1