A method for preparing an interface coating of an iron negative electrode of an aqueous iron ion battery
By coating the surface of the iron anode of an aqueous iron-ion battery with a porous Nb2O5 protective coating, the problems of iron dendrites and side reactions during battery recycling are solved, the cycle stability and electrochemical performance of the battery are improved, and the battery life is extended.
Patent Information
- Application Number
- CN202410841127.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-27
AI Technical Summary
During the recycling process of aqueous iron-ion batteries, the formation of iron dendrites and side reactions lead to cycle stability and life problems. The iron anode needs to be interface modified to improve performance.
The porous Nb2O5 material is prepared using solvothermal method and heat treatment process, and mixed with polyvinylidene fluoride to form a protective coating, which is coated on the surface of the iron anode to inhibit dendrite growth and improve electrochemistry through high ion conductivity and suitable pore structure. performance.
It significantly improves the cycle stability and electrochemical performance of aqueous iron-ion batteries, extends the service life of the battery, and achieves long-life and stable operation of the iron anode.
Smart Images

Figure CN118398753B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of interface modification of an iron negative electrode of an aqueous iron ion battery, and in particular relates to a method for preparing an interface coating of an iron negative electrode of an aqueous iron ion battery. Background Art
[0002] Among existing energy storage technologies, lithium-ion batteries dominate the portable device market due to their advantages such as high energy density, high output voltage and good cycle performance. However, the volatile organic electrolytes used in lithium-ion batteries can cause fire and explosion, and energy storage systems have long been safety issues. Therefore, people have been exploring non-flammable and energy-dense aqueous rechargeable batteries as an alternative to traditional energy storage devices. Among them, aqueous iron ion rechargeable batteries (AZIRBs) have favorable properties, including high theoretical capacities (820 mAh g - 1 and 5855mAh cm - 3 ), high reserves (crustal abundance of 46,500 ppm), low cost (electrode cost is only about $0.06 / kWh) and significant safety, it has become a highly promising candidate rechargeable battery for the next generation of energy storage applications. However, during the recycling of aqueous iron-ion batteries, the formation of iron dendrites and side reactions in water (such as hydrogen evolution reaction and corrosion reaction) seriously affect the cycle stability and cycle life of AZIRBs, which requires the interface modification of the iron negative electrode of aqueous iron-ion batteries to effectively improve its cycle stability and electrochemical performance. Therefore, the interface modification of the iron electrode of aqueous iron-ion batteries has become a hot topic for researchers. Summary of the invention
[0003] In view of the shortcomings of the current recycling process of the iron negative electrode of an aqueous iron ion battery, the present invention provides a method for preparing an interface coating of the iron negative electrode of an aqueous iron ion battery, which is used to effectively solve the problems of corrosion, dendrite growth and the like of the iron negative electrode during the recycling process of the battery. The method adopts a simple and controllable solvent thermal method and a heat treatment process to prepare a porous Nb2O5 material, and then the porous Nb2O5 material is mixed with polyvinylidene fluoride (PVDF) and coated on the surface of the iron negative electrode to form a protective coating of a specific thickness. The protective coating effectively improves the reversibility and electrochemical properties of the iron negative electrode, thereby realizing the long-life recycling of the aqueous iron ion battery.
[0004] The present invention adopts the following technical solution to solve the above technical problems, a method for preparing an iron negative electrode interface coating of an aqueous iron ion battery, characterized in that the specific steps are:
[0005] Step S1, using NH4F and NbCl5 as reaction raw materials, using anhydrous ethanol as reaction solvent, reacting at 60-80°C to obtain a (NH4)3NbOF6 precursor, and then calcining the (NH4)3NbOF6 precursor at 400-600°C for 2-8h to obtain a porous Nb2O5 iron negative electrode material;
[0006] Step S2, mixing the porous Nb2O5 iron negative electrode material obtained in step S1 and polyvinylidene fluoride, grinding them in a mortar to make them evenly mixed to obtain a coating material, and then coating the obtained coating material on the surface of the iron negative electrode to form a porous Nb2O5 protective coating. The iron negative electrode with the porous Nb2O5 protective coating is used as a negative electrode sheet for assembling an aqueous iron ion battery. The porous Nb2O5 iron negative electrode material in the prepared iron negative electrode protective coating has high ion conductivity, high dielectric constant and suitable pore structure, wherein the high ion conductivity and suitable pore structure are conducive to ion transport, thereby inducing uniform stripping and deposition of iron ions, and the higher dielectric constant can achieve uniform ion flux and inhibit two-dimensional diffusion, thereby achieving uniform arrangement of iron ions and preventing the growth of dendrites, thereby significantly improving the problem of poor cycle stability of aqueous iron ion secondary batteries caused by iron negative electrode corrosion and dendrite growth, so that it can operate stably for a long life.
[0007] Furthermore, the mass ratio of NH4F to NbCl5 in step S1 is 1-5:1.
[0008] Furthermore, in step S2, the mass ratio of the porous Nb2O5 iron negative electrode material to polyvinylidene fluoride is 6~10:1.
[0009] Furthermore, the specific process of step S1 is: NbCl5 and NH4F are dispersed in anhydrous ethanol reaction solvent respectively, stirred and dissolved, the two solutions are stirred and mixed evenly, and then the mixture is allowed to react at 70°C for 12 hours to obtain a mixture, and then the mixture is cooled and placed in anhydrous ethanol reaction solvent for centrifugal washing for multiple times to obtain a precipitated product, and the obtained product is dried at 70°C for 12 hours to obtain a (NH4)3NbOF6 precursor; the (NH4)3NbOF6 precursor is placed in a muffle furnace, and the temperature is increased to 500°C at a heating rate of 2°C / min in an air atmosphere and calcined for 2 hours to obtain a porous Nb2O5 negative electrode material.
[0010] Furthermore, the specific process of step S2 is: the porous Nb2O5 negative electrode material obtained in step S1 and polyvinylidene fluoride are placed in a mortar and ground in a mass ratio of 8:1, and NMP is continuously added during the process to make them mix evenly, and then the porous Nb2O5 iron negative electrode coating material is obtained after standing at room temperature for 2 hours to remove the volatile solvent therein, and the obtained porous Nb2O5 iron negative electrode coating material is applied to the surface of the iron negative electrode to form a porous Nb2O5 protective coating.
[0011] Furthermore, the aqueous iron ion secondary battery assembled in step S2 is an asymmetric button battery or a symmetric button battery, which uses FeSO4 solution as the electrolyte, a metal copper, metal iron or iron negative electrode with a porous Nb2O5 protective coating as the positive electrode, and a glass fiber diaphragm as the diaphragm.
[0012] Furthermore, the metallic iron is a single substance of iron sheet or foamed iron, and the metallic copper is a single substance of copper sheet or foamed copper.
[0013] Compared with the prior art, the present invention has the following advantages and beneficial effects: the preparation process of the present invention is simple and efficient, the preparation conditions are easy to control, and it is suitable for large-scale production; the high ion conductivity and suitable pore structure of the iron negative electrode interface coating prepared by the present invention are conducive to ion transmission, thereby inducing uniform stripping and deposition of iron ions; at the same time, the higher dielectric constant can achieve uniform ion flux and inhibit two-dimensional diffusion, thereby achieving uniform arrangement of iron ions and preventing dendrite growth, thereby effectively improving the reversibility and electrochemical performance of the iron negative electrode, realizing the long-life cycle use of aqueous iron ion secondary batteries, and having practical prospects and commercial value. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is the XRD diffraction pattern of the porous Nb2O5 iron negative electrode material prepared in Example 1 of the present invention.
[0015] Figure 2 This is a scanning electron microscope image of the porous Nb2O5 iron negative electrode material prepared in Example 1 of the present invention.
[0016] Figure 3 The symmetrical cell assembled with the Nb2O5@Fe electrode prepared in Example 2 and the symmetrical cell assembled with the pure iron electrode prepared in Comparative Example 1 was tested at a current density of 1 mA cm -2 , with a surface capacity of 1 mA h cm -2 The following cycle performance comparison chart.
[0017] Figure 4 The Fe / / Nb2O5@Cu asymmetric battery prepared in Example 2 of the present invention and the Fe / / Cu asymmetric battery prepared in Comparative Example 2 have a current density of 1 mA cm -2 , with a surface capacity of 1 mAh cm -2 The following cycle performance comparison chart. DETAILED DESCRIPTION
[0018] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Example 1
[0019] Preparation of porous Nb2O5 iron anode material
[0020] (1) Preparation of (NH4)3NbOF6 precursor: 0.6g NH4F was placed in a beaker containing 50mL of anhydrous ethanol, and 0.35g NbCl5 was placed in a centrifuge tube containing 50mL of anhydrous ethanol, and stirred to dissolve. The two solutions were stirred and mixed evenly, and then allowed to react at 70°C for 12h. The precipitate was obtained by centrifugation three times with anhydrous ethanol. The precipitate was dried at 70°C for 12h to obtain (NH4)3NbOF6 precursor.
[0021] (2) Preparation of porous Nb2O5 iron negative electrode material: The dried (NH4)3NbOF6 precursor material was placed in a muffle furnace, heated to 500°C at a heating rate of 2°C / min in an air atmosphere and calcined for 2 h to obtain a porous Nb2O5 iron negative electrode material.
[0022] Figure 1 Figure 2 is the X-ray diffraction (XRD) phase analysis result of the obtained product. It can be seen from the figure that the diffraction peak of the obtained sample is consistent with the peak of the standard card, indicating that the sample prepared by this method is Nb2O5 material. Figure 2 This is the microscopic morphology of the product. It can be seen from the figure that the surface of the sample is porous spherical. Example 2
[0023] Application of porous Nb2O5 material modified iron anode in iron ion batteries
[0024] (1) Preparation of porous Nb2O5 material-modified iron negative electrode: The porous Nb2O5 iron negative electrode material prepared in Example 1 and PVDF were mixed in a mass ratio of 8:1, ground and mixed evenly in a mortar, and NMP was continuously added during the process to accelerate the mixing of the materials, and finally a uniform coating material was obtained. The coating material was then applied on an iron sheet to obtain an iron negative electrode modified with a porous Nb2O5 material.
[0025] (2) Symmetrical battery assembly: The prepared Nb2O5 porous material modified iron electrode is used as both the positive and negative electrodes of the button battery. First, take a positive electrode sheet, put it into the positive electrode shell with the coated side facing up, then put it into the glass fiber separator, and drip 120μL of 1mol / L ferrous sulfate electrolyte. Then take a negative electrode sheet, put it on the separator with the coated side facing down, and then put the gasket and shrapnel in turn. Finally, buckle the negative electrode shell and seal the battery with a button battery sealing machine. Then, a symmetrical button battery containing an iron negative electrode modified with Nb2O5 porous material is obtained, which is marked as Nb2O5@Fe / / Fe symmetrical button battery.
[0026] Asymmetric battery assembly: The copper sheet modified with the prepared Nb2O5 porous material is used as the positive electrode of the button battery, and the iron negative electrode is used as the negative electrode of the button battery. First, take a positive electrode sheet and put it into the positive electrode shell with the coated side facing up, then put in a glass fiber separator, drip 120μL of 1mol / L ferrous sulfate electrolyte, then take a negative electrode sheet, and then put in the gasket and shrapnel in turn, and finally buckle the negative electrode shell, and use the button battery sealing machine to seal the battery, and then obtain an asymmetric button battery modified with Nb2O5 porous material, marked as Fe / / Nb2O5@Cu asymmetric button battery.
[0027] Comparative Example 1
[0028] Aqueous iron ion symmetric button cell with pure iron sheet electrode
[0029] The positive and negative electrodes are made of pure iron sheets, and the assembly method is the same as above, marked as Fe / / Fe symmetrical button battery.
[0030] Comparative Example 2
[0031] Aqueous iron ion asymmetric button battery with pure copper sheet electrode
[0032] The positive electrode is made of pure copper and the negative electrode is made of pure iron. The assembly method is the same as above and it is marked as Cu / / Fe asymmetric button battery.
[0033] The battery tests of the present invention are all carried out on the Xinwei testing system.
[0034] Symmetrical battery constant current charge and discharge test (cycle life): at a current density of 1 mA cm -2 , with a surface capacity of 1 mAh cm -2 Under the condition of constant current charge and discharge test, the aqueous iron ion symmetrical button battery is tested. The test results are as follows Figure 3 As shown. The Fe / / Fe symmetric button cell experienced a short circuit after about 160 hours of cycling, indicating that a serious side reaction occurred during the cycling process, resulting in uneven stripping and deposition of iron ions, which caused the iron dendrites to grow rapidly and pierce the diaphragm, causing the battery to short-circuit within a short period of time. The Nb2O5@Fe / / Fe symmetric button cell was able to cycle stably for 540 hours, indicating that the iron negative electrode modified with Nb2O5 porous material can inhibit the occurrence of side reactions during battery cycling, ensure uniform deposition and stripping of iron ions, and improve the battery's cycling stability.
[0035] Asymmetric battery constant current charge and discharge test (Coulomb efficiency) at a current density of 1 mA cm -2 , with a surface capacity of 1 mAh cm -2 Under the condition of constant current charge and discharge test, the aqueous iron ion asymmetric button battery was tested. The results are as follows Figure 4As shown in the charge and discharge cycle curve, the coulombic efficiency of the Cu / / Fe asymmetric button cell begins to drop sharply after 100 cycles and short circuits occur after 100 cycles, while the Fe / / Nb2O5@Cu asymmetric button cell can stably cycle for more than 200 cycles with a more stable coulombic efficiency, which indicates that the iron negative electrode modified with Nb2O5 porous material is conducive to the uniform stripping and deposition of iron ions, thereby improving the cycle stability of aqueous iron ion batteries.
[0036] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. A method for preparing an interface coating of an iron negative electrode of an aqueous iron ion battery, characterized in that The specific steps are: Step S1, using NH4F and NbCl5 as reaction raw materials, using anhydrous ethanol as reaction solvent, reacting at 60-80°C to obtain a (NH4)3NbOF6 precursor, and then calcining the (NH4)3NbOF6 precursor at 400-600°C for 2-8h to obtain a porous Nb2O5 iron negative electrode material, wherein the mass ratio of NH4F to NbCl5 is 1-5:1; Step S2, mixing the porous Nb2O5 iron negative electrode material obtained in step S1 with polyvinylidene fluoride, wherein the mass ratio of the porous Nb2O5 iron negative electrode material to polyvinylidene fluoride is 6~10:1, grinding them in a mortar to make them mix evenly to obtain a coating material, and then applying the obtained coating material on the surface of the iron negative electrode to form a porous Nb2O5 protective coating. The iron negative electrode with the porous Nb2O5 protective coating is used as a negative electrode sheet for assembling an aqueous iron ion battery.
2. The method for preparing the iron negative electrode interface coating of the aqueous iron ion battery according to claim 1, characterized in that The specific process of step S1 is: NbCl5 and NH4F are dispersed in anhydrous ethanol reaction solvent respectively and stirred to dissolve, the two solutions are stirred and mixed evenly, and then the mixture is allowed to stand at 70°C for 12 hours to obtain a mixture, and then the mixture is cooled and placed in anhydrous ethanol reaction solvent for centrifugal washing for multiple times to obtain a precipitated product, and the obtained product is dried at 70°C for 12 hours to obtain a (NH4)3NbOF6 precursor; the (NH4)3NbOF6 precursor is placed in a muffle furnace, and the temperature is increased to 500°C at a heating rate of 2°C / min in an air atmosphere and calcined for 2 hours to obtain a porous Nb2O5 negative electrode material.
3. The method for preparing the iron negative electrode interface coating of the aqueous iron ion battery according to claim 1, characterized in that The specific process of step S2 is: the porous Nb2O5 negative electrode material obtained in step S1 and polyvinylidene fluoride are placed in a mortar and ground in a mass ratio of 8:1, and NMP is continuously added during the process to make them mix evenly, and then the porous Nb2O5 iron negative electrode coating material is obtained after standing at room temperature for 2 hours to remove the volatile solvent therein, and the obtained porous Nb2O5 iron negative electrode coating material is applied to the surface of the iron negative electrode to form a porous Nb2O5 protective coating.
4. The method for preparing the iron negative electrode interface coating of an aqueous iron ion battery according to claim 1, characterized in that: The aqueous iron ion secondary battery assembled in step S2 is an asymmetric button battery or a symmetric button battery, which uses FeSO4 solution as the electrolyte, a metal copper, metal iron or iron negative electrode with a porous Nb2O5 protective coating as the positive electrode, and a glass fiber diaphragm as the diaphragm.
5. The method for preparing the iron negative electrode interface coating of the aqueous iron ion battery according to claim 4, characterized in that: The metal iron is a single substance of iron sheet or foamed iron, and the metal copper is a single substance of copper sheet or foamed copper.
Citation Information
Cited By
Preparation method of iron negative electrode double-layer interface coating of water-based iron metal battery
CN120854465A