Amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber and preparation method thereof
By controlling polymerization conditions and using composite initiators, a polyisoprene-polyethylene glycol block copolymer liquid rubber with amphiphilicity and high controllability is prepared, solving the amphiphilic and controllable problems in the existing technology. Solve the problem of insufficient performance and realize the preparation of high-performance materials suitable for many fields.
Patent Information
- Application Number
- CN202410881342.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-03
AI Technical Summary
It is difficult to prepare an olefin-alkylene oxide block copolymer with amphiphilicity and high controllability using existing technology, and rare earth catalysts are expensive and difficult to achieve industrial production.
By controlling polymerization conditions such as temperature, time and initiator concentration, a composite initiator composed of alkyl lithium and alkali metal alkoxide is used to form a polyisoprene-polyethylene glycol block copolymer liquid rubber to achieve control of the segment molecular weight. And structure control, with dual properties of hydrophilic and lipophilic.
The prepared amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber has excellent physical and chemical properties and is suitable for solid electrolytes, polymer drug carriers, surfactants, phase transfer catalysts and other fields, and Can be further functionalized to meet different needs.
Smart Images

Figure CN118406224B_ABST
Abstract
Description
Technical Field
[0001] The invention specifically relates to the field of polymer material synthesis, and is an amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber and a preparation method thereof. Background Art
[0002] The block copolymers synthesized from dienes and alkylene oxides have unique internal molecular structures, containing both hydrophilic and lipophilic segments, and thus exhibit extraordinary properties in multiple physical and chemical properties. These properties include unique micellar behavior, obvious microphase separation properties, stable rheology, and adjustable viscoelasticity. These special properties make it widely used in many fields, such as being used as a fixed electrolyte in battery manufacturing, as a polymer drug carrier for drug delivery, as a surfactant to improve the interfacial properties of substances, and as a phase transfer catalyst to promote chemical reactions.
[0003] What is more worth mentioning is that the main chain of this block copolymer contains abundant double bond structures, which makes it possible to further functionalize it. For example, through hydrogenation reaction, these double bonds can be converted into saturated alkane segments, thereby changing its physical properties. In addition, other chemical modification methods, such as addition and substitution reactions, can also be used to prepare functional resins with special properties to meet the needs of different fields.
[0004] When synthesizing this block copolymer, commonly used methods include anionic polymerization and chemical coupling. Anionic polymerization has the advantages of fast reaction speed and controllable product molecular weight, which is suitable for large-scale production. Chemical coupling can adjust the structure and properties of the copolymer by precisely controlling the position and number of cross-linking points, thereby achieving precise regulation of its function.
[0005] Invention patent CN107556416B discloses a liquid polyisoprene rubber and a preparation method thereof, which can better control the progress of the polymerization reaction, thereby obtaining a liquid polyisoprene rubber with a narrow molecular weight distribution and highly controllable molecular weight at a higher monomer conversion rate, and can be carried out at a high monomer concentration, and has good industrial application value. However, the liquid isoprene prepared by the patent does not involve the introduction of polar chain ends, and therefore cannot exhibit amphiphilicity.
[0006] Zhang Yifeng et al. (Science Bulletin, 1995, 40(9), 795-798) reported the block copolymerization of isoprene and epichlorohydrin catalyzed by rare earth coordination. However, the rare earth catalyst used in the reaction requires special treatment and is expensive, making it difficult to achieve industrial production. Summary of the invention
[0007] The purpose of the present invention is to provide an amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber and a preparation method thereof in view of the deficiencies of the prior art, and to achieve regulation of the molecular weight and structure of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber chain segments by controlling polymerization conditions (such as temperature, time and initiator concentration). The amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber of the present invention has a number average molecular weight of 1000 to 20000, and not only has excellent physical and chemical properties, but also has good processability and crosslinkability, and is expected to be applied to the fields of solid electrolytes, polymer drug carriers, surfactants and phase transfer catalysts.
[0008] In a first aspect, the present invention provides an amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber having a molecular structure shown in Formula I:
[0009] Formula I
[0010] In Formula I, in the molecular structure, x and y represent the number of repeating units A and B, x+y=m; m is an integer from 10 to 300; the ratio of x / m is 10% to 90%; n represents the number of repeating units C, which is an integer from 1 to 400; the two types of repeating units A and B are randomly distributed, and the repeating unit C is block distributed. The random distribution and block distribution are terms well known to researchers in the professional and technical field, and will not be repeated here.
[0011] In addition, the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber provided by the present invention can be further chemically modified and functionalized due to the double bond structure on its main chain to prepare a functional resin with special properties. The chemical modification method includes but is not limited to hydrogenation, grafting, and cross-linking chemical reactions.
[0012] The hydrogenation refers to adding hydrogen atoms to double bonds under the action of a specific catalyst (such as Pd / C) to reduce the unsaturation on the molecular chain, causing the reaction shown in Formula II to convert all or part of the double bonds in the molecular chain into single bonds;
[0013]
[0014] The grafting refers to connecting the functional group to the double bond through an addition reaction, thereby giving the liquid rubber certain functionality, which includes but is not limited to pH responsiveness, photosensitivity, thermosensitivity, etc.
[0015] The cross-linking refers to the use of the polymerizable properties of double bonds to react with cross-linking agents such as sulfur, sulfide, peroxide, etc., so that cross-linking points are formed between molecular chains, thereby changing from a liquid state to a solid or semi-solid state. This cross-linking reaction can be carried out by thermal initiation, light initiation, or radiation initiation, and the appropriate cross-linking method and cross-linking agent can be selected according to specific application requirements and process conditions.
[0016] The modifiability and functionalization characteristics of amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber give it broad application prospects in the preparation of high-performance composite materials, functional coatings, biomedical materials, etc. For example, in the biomedical field, it can be chemically modified and functionalized to make it biocompatible and bioactive, and then used to prepare drug carriers, biosensors, etc.; in the coating field, it can be adjusted by adjusting its molecular structure and functional groups to prepare coatings with excellent weather resistance, chemical corrosion resistance and self-cleaning functions.
[0017] The amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber of the present invention has both hydrophilic and lipophilic properties and exhibits unique micelle behavior, microphase separation, rheological properties, viscoelasticity and other properties.
[0018] In a second aspect, the present invention provides a method for preparing an amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber, which is carried out as follows: isoprene monomer is mixed with a polar solvent to form a polymerization monomer solution, a composite initiator comprising alkyl lithium and alkali metal alkoxide is configured in the polar solvent to form a composite initiator solution, the composite initiator solution is added to the polymerization monomer solution, mixed to form a reaction solution, the reaction solution is polymerized at a predetermined temperature for a predetermined time to obtain a polyisoprene solution; ethylene oxide monomer is added to the polyisoprene solution, polymerized at another predetermined temperature for a predetermined time, and the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber is obtained through post-treatment.
[0019] The specific steps include:
[0020] Step 1. Prepare a composite initiator comprising alkyl lithium and alkali metal alkoxide in a polar solvent to form a composite initiator solution. In this step, the selection of the polar solvent should take into account its solubility in the initiator and the monomer to ensure the smooth progress of the polymerization reaction.
[0021] The polar solvent is selected from one or more of tetrahydrofuran, ether, dimethylformamide and dioxane;
[0022] The alkyl lithium is selected from one or more of methyl lithium, ethyl lithium, propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, pentyl lithium, n-hexyl lithium, cyclohexyl lithium, tert-octyl lithium, n-dodecyl lithium, n-eicosyl lithium, phenyl lithium, methyl phenyl lithium, butyl phenyl lithium, naphthyl lithium and butyl cyclohexyl lithium;
[0023] The alkali metal alkoxide is selected from one or more of the sodium salt or potassium salt of methanol, ethanol, propanol, isopropanol, tert-butanol, pentanol, hexanol, n-octanol, ethylene glycol, propylene glycol, hexylene glycol, glycerol, 1,2,4-butanetriol, 1,2,5-pentanetriol, tetramethylene glycol and pentaerythritol;
[0024] Step 2. Mixing isoprene monomer with a polar solvent to form a polymerization monomer solution. The amount of isoprene monomer used can be adjusted according to the desired properties of the copolymer.
[0025] In the polymerization monomer solution, the concentration of isoprene is preferably 5 g to 15 g isoprene / 100 ml of polar solvent.
[0026] Step 3. Add the composite initiator solution prepared in step 1 to the polymerization monomer solution in step 2, mix thoroughly to form a reaction solution, and polymerize at a predetermined temperature for a predetermined time to obtain a polyisoprene solution.
[0027] In this step, the molecular weight and structure of the polyisoprene chain segment can be regulated by controlling the polymerization conditions (such as temperature, time and initiator concentration).
[0028] The predetermined temperature in step 3 is -40°C to 80°C, preferably -20°C to 60°C;
[0029] The predetermined time in step 3 is 0.5 h to 6 h, preferably 1 h to 5 h.
[0030] For example, the amount of composite initiator added: for every 5g to 15g of isoprene monomer or 5g to 15g of ethylene oxide monomer, add 2x10 alkyl lithium -3 moL to 4x10 -3 moL and alkali metal alkoxide 0.10g to 0.15g.
[0031] Step 4. Add ethylene oxide monomer into the polyisoprene solution obtained in step 3, polymerize at another predetermined temperature for a predetermined time, and obtain an amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber through post-treatment. In this step, the addition of ethylene oxide monomer allows the ethylene glycol segment to be introduced into the polyisoprene segment to form a block copolymer.
[0032] In step 4, the relative ratio of the weight of the ethylene oxide monomer introduced to the volume of the polar solvent is in the range of 5 g to 15 g / 100 ml;
[0033] The other predetermined temperature in step 4 is -40°C to 80°C, preferably -20°C to 75°C;
[0034] The another predetermined time in step 4 is 1 hour to 8 hours, preferably 3 hours to 6 hours.
[0035] In the above steps 1, 2, 3, and 4, unless otherwise specified, all glassware used were treated with standard Schlenk technology to remove impurities such as water and oxygen that are harmful to the reaction, and all operations used standard anhydrous and oxygen-free operation techniques.
[0036] In step 4, post-treatment refers to conventional treatment techniques well known to those skilled in the art, specifically including but not limited to the combined application of quenching, concentration, extraction, separation and other operation methods. Since it belongs to conventional technical means, its specific steps and operation details will not be described in detail here.
[0037] The beneficial effects of the present invention are:
[0038] The molecular structure of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber prepared by the present invention is shown in Formula I, wherein the two types of repeating units A and B are randomly distributed, and the repeating unit C is distributed in blocks. The rubber has both hydrophilic and lipophilic properties, and exhibits unique micellar behavior, microphase separation, rheological properties, viscoelastic properties and the like.
[0039] The present invention uses a composite initiator composed of alkyl lithium and alkali metal alkoxide, firstly uses alkyl lithium as an initiator and alkali metal alkoxide as a molecular weight regulator, polymerizes isoprene monomer in a polar solvent to form a polyisoprene segment. Subsequently, ethylene oxide monomer is added to the polymerization system, and the alkali metal alkoxide in the system is used to initiate the polymerization of ethylene oxide monomer, and the ethylene glycol segment is introduced into the polyisoprene segment to form a polyisoprene-polyethylene glycol block copolymer. In this process, by accurately controlling the degree of polymerization of each block component, the fine regulation of the copolymer structure and performance is achieved, and an amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber with a number average molecular weight of 1000 to 20000 is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 TEM image of amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber.
[0041] Figure 1 Shooting parameters: microscope model: JEM-1011; accelerating voltage: 100 kV; magnification: 50000; camera length: 0 mm; shooting specification: 500 nm. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0043] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods. Unless otherwise specified, the percentages in the present invention are all mass percentages.
[0044] The present invention is described in detail below in conjunction with specific embodiments. Example 1
[0045] Preparation steps
[0046] Step 1. Add 1 ml of tetrahydrofuran solution of n-butyl lithium (2.0 mol / L) and 0.10 g of potassium tert-butoxide to 100 mL of tetrahydrofuran and stir well to form a composite initiator solution.
[0047] Step 2. 10 g of isoprene monomer was mixed with tetrahydrofuran to form a polymerization monomer solution.
[0048] Step 3. Add the composite initiator solution to the polymerization monomer solution, mix thoroughly to form a reaction solution, place the reaction solution in a 25° C. water bath, and react for 2 hours to obtain a polyisoprene solution.
[0049] Step 4. Add 10 g of ethylene oxide monomer to the polyisoprene solution, maintain the temperature at 25°C, and continue the reaction for 3 hours. After the reaction is completed, the reaction solution is subjected to post-treatment operations such as quenching, concentration, extraction, and liquid separation to obtain 19.8 g of amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber. The number average molecular weight of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber obtained by gel permeation chromatography (GPC) is 11,200.
[0050] Example 2-5: The amount of isoprene monomer in step 2 of Example 1 was changed to 5 g, 8 g, 12 g, and 15 g, respectively. The other steps were the same as in Example 1. The number average molecular weight of the obtained amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber is shown in Table 1.
[0051] As shown in Table 1, the number average molecular weight of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber can be adjusted by controlling the amount of isoprene monomer used. Example 6
[0052] Preparation steps
[0053] Step 1. Add 2 ml of tetrahydrofuran solution of n-dodecyl lithium (2.0 mol / L) and 0.15 g of sodium isopropoxide to 100 mL of ether to form a composite initiator solution.
[0054] Step 2. 10 g of isoprene monomer was mixed with diethyl ether to form a polymerization monomer solution.
[0055] Step 3. Add the composite initiator solution to the polymerization monomer solution, mix thoroughly to form a reaction solution, heat the reaction solution to 35° C., stir and react for 3 hours to obtain a polyisoprene solution.
[0056] Step 4. Add 10 g of ethylene oxide monomer to the polyisoprene solution, control the temperature at 75°C, and continue the reaction for 4 hours. After the reaction is completed, perform conventional post-treatment to obtain an amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber. The number average molecular weight of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber obtained by GPC measurement is 5700.
[0057] Examples 7-10: The amount of ethylene oxide monomer in step 4 in Example 6 was changed to 5 g, 8 g, 12 g, and 15 g, respectively. The other steps were the same as in Example 6. The number average molecular weight of the obtained amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber is shown in Table 2.
[0058] It can be seen from Table 2 that the number average molecular weight of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber can be adjusted by controlling the amount of ethylene oxide monomer. Embodiment 11
[0059] Preparation steps
[0060] Step 1. Mix 1 ml of tert-butyl lithium tetrahydrofuran solution (2.0 mol / L) and 0.15 g of potassium ethylene glycol in 10 ml of dioxane to form a composite initiator solution.
[0061] Step 2. 15 g of isoprene monomer was mixed with dioxane to form a polymerization monomer solution.
[0062] Step 3. Add the composite initiator solution to the polymerization monomer solution, mix thoroughly to form a reaction solution, stir the reaction solution at 0° C. for 3 hours to obtain a polyisoprene solution.
[0063] Step 4. Then, 10 g of ethylene oxide monomer was introduced into the polyisoprene solution, the reaction temperature was controlled to 0°C, and the reaction was continued under stirring for 6 hours. After the reaction was completed, the amphiphilic mixed olefin-polyethylene glycol block copolymer liquid rubber was obtained according to conventional post-treatment steps. The number average molecular weight of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber was about 15,700.
[0064] In the amphiphilic mixed olefin-polyethylene glycol block copolymer liquid rubber obtained in Example 11, the A segment accounts for 24%, the B segment accounts for 31%, and the C segment accounts for 45%.
[0065] Example 12-15: Changing the reaction temperature in step 3 of Example 11, the reaction temperatures are respectively
[0066] -20°C, 20°C, 40°C, 60°C, and other steps were the same as in Example 11. The proportions of A, B, and C segments in the obtained amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber are shown in Table 3.
[0067] It can be seen from Table 3 that by controlling the polymerization reaction temperature of step 3, the proportion of each segment component of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber can be adjusted. Example 16
[0068] Preparation steps
[0069] Step 1. Add 1.5 ml of tetrahydrofuran solution of n-hexyl lithium (2.0 mol / L) and 0.10 g of potassium 1,2,4-butanetriol to 100 mL of tetrahydrofuran and stir well to form a composite initiator solution.
[0070] Step 2. 12 g of isoprene monomer was mixed with tetrahydrofuran to form a polymerization monomer solution.
[0071] Step 3. Add the composite initiator solution to the polymerization monomer solution, mix thoroughly to form a reaction solution, place the reaction system in an ice water bath at 0°C, start the agitator to carry out the polymerization reaction, and continue the reaction for 5 hours to obtain a polyisoprene solution.
[0072] Step 4. 10 g of ethylene oxide monomer was gradually introduced into the polyisoprene solution, the reaction temperature was controlled at 40°C, and the stirring reaction was maintained for 3 hours. After the reaction was completed, the product was subjected to conventional post-treatments such as quenching, concentration, extraction, and liquid separation to obtain an amphiphilic mixed olefin-polyethylene glycol block copolymer liquid rubber. The number average molecular weight of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber tested by GPC reached 7200.
[0073] In the amphiphilic mixed olefin-polyethylene glycol block copolymer liquid rubber obtained in Example 16, the A segment accounts for 36%, the B segment accounts for 14%, and the C segment accounts for 50%.
[0074] Example 17-20: Changing the reaction temperature in step 4 of Example 16, the reaction temperatures are respectively
[0075] -20°C, 20°C, 60°C, 80°C, the other steps are the same as in Example 16, and the proportions of A, B, and C segments in the obtained amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber are shown in Table 3.
[0076] It can be seen from Table 3 that by controlling the polymerization reaction temperature of step 4, the proportion of each segment component of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber can be adjusted. Embodiment 21
[0077] Take 5 g of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber obtained in Example 1, add it to a high-pressure reactor, add 100 ml of n-hexane and stir to dissolve, then add 0.1 g of Pd / C, replace with nitrogen three times, tighten the lid of the reactor, pass H2, hydrogen pressure 20 atm, react at 70 ° C for 6 h, stop the reaction, release the pressure after cooling to room temperature, pour out the polymer solution, add 200 ml of tetrahydrofuran, filter after fully dissolving, and rotary evaporate the aluminum to complete dryness to obtain 5.1 g of hydrogenation reaction product. Embodiment 22
[0078] Take 0.1g of the amphiphilic polyisoprene-polyethylene glycol liquid rubber obtained in Example 1, add it dropwise with a syringe (continue to drop after the previous drop is completely emulsified) to 100mL of ultrapure water under vigorous stirring at 1100rpm, and stir at 40℃ for 2h; ultrasonicate for 30min after the stirring is completed, and ultrasonicate for 1.5h at room temperature to obtain an amphiphilic polyisoprene-polyethylene glycol liquid rubber micelle solution. Irradiate the solution with a laser pen, and there is an obvious light path. This shows that the solution has obvious Tyndall phenomenon. The solution is dropped on a copper mesh, and after drying, a transmission electron microscope sample is prepared (see Figure 1 ), micelles with diameters of 150-250 nm were observed.
[0079] It can be seen from Example 22 that the amphiphilic polyisoprene-polyethylene glycol liquid rubber exhibits unique micellar behavior. Comparative Example 1
[0080] Step 1. Add 1 ml of tetrahydrofuran solution of n-butyl lithium (2.0 mol / L) to 100 ml of tetrahydrofuran and stir well to form an initiator solution.
[0081] Step 2. Add 10 g of isoprene monomer to the above initiator solution and mix thoroughly to form a reaction solution.
[0082] Step 3. The reaction solution was placed in a 25°C water bath and reacted for 2 hours to obtain a polyisoprene solution.
[0083] Step 4. Add 10 g of ethylene oxide monomer to the polyisoprene solution, maintain the temperature at 25°C, and continue the reaction for 3 hours. After the reaction is completed, the reaction solution is subjected to post-treatment operations such as quenching, concentration, extraction, and separation to obtain 9.9 g of isoprene liquid rubber. The number average molecular weight of the copolymer liquid rubber obtained by gel permeation chromatography (GPC) is 4980. Nuclear magnetic resonance testing shows that the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber of the molecular structure shown in Examples 1 to 20 is not obtained. Comparative Example 2
[0084] Step 1. Add 0.1 g of potassium tert-butoxide to 100 mL of tetrahydrofuran and stir well to form an initiator solution.
[0085] Step 2. Add 10 g of isoprene monomer to the above initiator solution and mix thoroughly to form a reaction solution.
[0086] Step 3. The reaction solution was placed in a 25°C water bath and reacted for 2 hours. The reaction solution was subjected to post-treatment operations such as quenching, concentration, extraction, and separation. No polyisoprene was obtained, indicating that isoprene was not initiated and the reaction could not proceed.
[0087] It can be seen from Comparative Examples 1 and 2 that the composite initiator of the present invention plays a vital role in the copolymerization of isoprene monomer and ethylene oxide, and both alkyl lithium and alkali metal alkoxide are indispensable in the composite initiator.
[0088] The amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber provided by the present invention not only has excellent physical and chemical properties, but also has a simple and controllable preparation method, which injects new vitality into the development of the field of polymer materials. By regulating the amount of monomers and composite initiators added, as well as the polymerization temperature and time, the structure and performance of the copolymer can be precisely regulated, thereby meeting the needs for high-performance and multifunctional polymer materials in the fields of fixed electrolytes, polymer drug carriers, surfactants, and phase transfer catalysts.
[0089] The above embodiments are only used for illustrative purposes and do not constitute a limitation on the scope of protection of the present invention. In practical applications, the types of raw materials, proportions, reaction conditions, etc. can be appropriately adjusted according to specific needs and conditions to prepare copolymer liquid rubbers with different properties and application fields. Therefore, for those skilled in the art, without departing from the concept of the present invention, equivalent replacements or modifications made to the contents recorded in the embodiments should all be included in the scope of protection of the present invention.
[0090] Table 1
[0091]
[0092] Table 2
[0093]
[0094] Table 3
[0095]
Claims
1. A method for preparing an amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber, characterized in that: The method comprises mixing an isoprene monomer with a polar solvent to form a polymerization monomer solution, configuring a composite initiator comprising an alkyl lithium and an alkali metal alkoxide in the polar solvent to form a composite initiator solution, adding the composite initiator solution to the polymerization monomer solution, mixing to form a reaction solution, and polymerizing the reaction solution at a predetermined temperature for a predetermined time to obtain a polyisoprene solution; The ethylene oxide monomer is added to the polyisoprene solution, polymerized at another predetermined temperature for a predetermined time, and then post-treated to obtain an amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber having a molecular structure shown in Formula I: Formula I In formula I, x and y represent the number of repeating units A and B, x+y=m; m is an integer from 10 to 300; the ratio of x / m is 10% to 90%; n represents the number of repeating units C, which is an integer from 1 to 400; the repeating units A and B are randomly distributed, and the repeating unit C is distributed in blocks; Wherein, the alkyl lithium is selected from one or more of methyl lithium, ethyl lithium, propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, pentyl lithium, n-hexyl lithium, cyclohexyl lithium, tert-octyl lithium, n-dodecyl lithium, n-eicosyl lithium, phenyl lithium, methyl phenyl lithium, butyl phenyl lithium, naphthyl lithium and butyl cyclohexyl lithium; The alkali metal alkoxide is selected from one or more of the sodium salt or potassium salt of methanol, ethanol, propanol, isopropanol, tert-butanol, pentanol, hexanol, n-octanol, ethylene glycol, propylene glycol, hexylene glycol, glycerol, 1,2,4-butanetriol, 1,2,5-pentanetriol, tetramethylene glycol and pentaerythritol; The amount of composite initiator added: for every 5g to 15g of isoprene monomer or every 5g to 15g of ethylene oxide monomer, add 2x10 -3 moL to 4x10 -3 moL and alkali metal alkoxide 0.10g to 0.15g; The number average molecular weight of the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber is 1,000 to 20,000.
2. The method for preparing the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber according to claim 1, characterized in that: The polar solvent is selected from one or more of tetrahydrofuran, ether, dimethylformamide and dioxane.
3. The method for preparing the amphiphilic polyisoprene-polyethylene glycol block copolymer liquid rubber according to claim 1 or 2, characterized in that: The polymerization temperature of the isoprene monomer is -20°C to 60°C, and the polymerization time is 1h to 5h; or / and, the polymerization temperature of the ethylene oxide monomer and polyisoprene is -20°C to 75°C, and the polymerization time is 3h to 6h.