A kind of oxygen-free curing anti-fingerprint resin and preparation method thereof

Through the use of oxygen-free curing anti-fingerprint resin, combined with specific processes and photoinitiators, the problem of skin-like coatings easily retaining fingerprints is solved, achieving both skin-like and anti-fingerprinting, and improving the anti-fouling and adhesion of the coating.

CN118406429BActive Publication Date: 2024-10-08CHANGZHOU JIASHIJIA DECORATIVE NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410636781.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2024-10-08
Estimated Expiration
2044-05-22

AI Technical Summary

Technical Problem

Existing skin-feel coatings are prone to leave fingerprint marks and affect visual perception, making it difficult to achieve both skin-feel and anti-fingerprint effects.

Method used

Using an oxygen-free curing anti-fingerprint resin, polyurethane acrylate, acrylate copolymer, ethoxylated trimethylolpropane triacrylate and other components are combined with a photoinitiator and specific process to form a hydrophobic and high-performance anti-fingerprint resin. The highly cross-linked coating promotes the formation of surface wrinkles and achieves skin feel and anti-fingerprint effects.

Benefits of technology

It achieves a delicate skin-feel effect on the surface of the decorative panel, while improving the anti-fingerprint performance of the coating, enhancing the anti-fouling and easy-to-clean capabilities, and improving the hardness and adhesion of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118406429B_ABST
    Figure CN118406429B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of skin-feel resins, specifically a kind of anaerobic curing anti-fingerprint resin and preparation method thereof, including 11-17 parts of polyurethane acrylate, 2-3 parts of acrylate copolymer, 18-20 parts of ethoxylated trimethylolpropane triacrylate, 7-8 parts of cyclotrimethylolpropane formal acrylate, 8-10 parts of ditrimethylolpropane tetraacrylate, 2-5 parts of tripropylene glycol diacrylate, 20-25 parts of 1,6-ethylene glycol diacrylate, 5-10 parts of hydroxyethyl methacrylate, 5-10 parts of trimethylolpropane triacrylate and 0-4.5 parts of photoinitiator. The present invention cooperates with anaerobic curing anti-fingerprint resin components through process and anaerobic excimer lamp irradiation, so that the surface of anaerobic curing anti-fingerprint resin forms wrinkles, and the skin-feel effect of decorative paper / board surface is realized; the preparation process and components of the control component are improved to improve the anti-fingerprint effect of its surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oxygen-free curing skin-feel resins, in particular to an oxygen-free curing anti-fingerprint resin and a preparation method thereof. Background Art

[0002] Decorative panels used in homes have good physical and chemical properties and colors, but as people's requirements for quality of life continue to increase, consumers expect decorative panels to produce a delicate skin-feeling effect when touched, creating a warmer and more comfortable effect. As a result, skin-feeling has become an important direction for the development of decorative panels. The key to the generation of skin-feeling lies in the construction of the surface structure, which is formed by structures such as wrinkles and ripples. Although some existing skin-feel coatings provide people with skin-feeling sensations, they are also prone to leaving fingerprints on their surfaces, affecting visual perception. Therefore, we propose an oxygen-free curing anti-fingerprint resin and a preparation method thereof. Summary of the invention

[0003] The object of the present invention is to provide an oxygen-free curing anti-fingerprint resin and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0004] In order to solve the above technical problems, the present invention provides the following technical solution: an oxygen-free curing anti-fingerprint resin, comprising the following components by mass: 11 to 17 parts of polyurethane acrylate, 2 to 3 parts of acrylate copolymer, 18 to 20 parts of ethoxylated trimethylolpropane triacrylate, 7 to 8 parts of cyclotrimethylolpropane formal acrylate, 8 to 10 parts of ditrimethylolpropane tetraacrylate, 2 to 5 parts of tripropylene glycol diacrylate, 20 to 25 parts of 1,6-ethylene glycol diacrylate, 5 to 10 parts of hydroxyethyl methacrylate, 5 to 10 parts of trimethylolpropane triacrylate and 0 to 4.5 parts of photoinitiator.

[0005] Furthermore, the photoinitiator includes: 1 to 2 parts of methyl benzoylformate (photoinitiator MBF), 0.3 to 0.5 parts of phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide (photoinitiator XBPO) and 1 to 2 parts of 1-hydroxycyclohexyl phenyl acetone (photoinitiator 184).

[0006] A method for preparing an oxygen-free curing anti-fingerprint resin comprises the following processes:

[0007] Take polyurethane acrylate, acrylate copolymer, ethoxylated trimethylolpropane triacrylate, cyclotrimethylolpropane formal acrylate, ditrimethylolpropane tetraacrylate, tripropylene glycol diacrylate, 1,6-ethylene glycol diacrylate, hydroxyethyl methacrylate, trimethylolpropane triacrylate and ethyl acetate, stir and mix at a speed of 400-750 r / min; adjust the speed to 700-1200 r / min, continue stirring for 30-45 minutes, and obtain an oxygen-free curing anti-fingerprint resin.

[0008] Furthermore, the polyurethane acrylate is prepared by the following process:

[0009] Mix isophorone diisocyanate and ethyl acetate, raise the temperature to 40-50°C, add castor oil and catalyst, and keep the temperature to react for 115-125 minutes;

[0010] Raise the temperature to 50-60°C, add hydroxy polydimethylsiloxane and catalyst dropwise, add them over 30 minutes, raise the temperature to 60-70°C, and stir the reaction for 115-125 minutes;

[0011] The temperature was raised to 70-80°C, and hexahydro-1,3,5-tri(hydroxyethyl)-s-triazine, hydroxyl-containing acrylate, catalyst and 4-methoxyphenol were added dropwise within 2 hours, and the mixture was kept warm to react until the -NCO group content was ≤0.1%. Triethylamine was added for neutralization reaction for 20-30 minutes to obtain polyurethane acrylate.

[0012] Furthermore, the polyurethane acrylate includes the following components by mass: 24.7-25.0 parts of isophorone diisocyanate, 54.8-55.0 parts of castor oil, 5-8 parts of hydroxy polydimethylsiloxane, 8-10 parts of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine, and 5-7 parts of hydroxyl-containing acrylate.

[0013] Furthermore, the hydroxyl-containing acrylate is a mixture of one or more of pentaerythritol triacrylate, hydroxyethyl acrylate, triethylene glycol diacrylate, and trimethylolpropane triacrylate.

[0014] Furthermore, the catalyst is dibutyltin dilaurate, and the amount used each time is 0.1wt% of the mass of the aforementioned added components (same addition process);

[0015] 4-methoxyphenol is 0.1wt% of the total mass of the hydroxyl-containing acrylate;

[0016] The mass ratio of isophorone diisocyanate to ethyl acetate is 45:100.

[0017] Furthermore, the castor oil is fluorinated and modified by the following process:

[0018] Castor oil, glacial acetic acid, cationic resin and toluene are mixed and stirred, placed at 55-60° C., hydrogen peroxide is added dropwise, and the mixture is reacted for 7-8 hours; the mixture is washed with a sodium carbonate aqueous solution, filtered, and toluene is removed by rotary evaporation, and dried at 70-80° C. for 100-150 minutes to obtain epoxidized castor oil;

[0019] Mix bisphenol AF, anhydrous potassium carbonate and N,N'-dimethylformamide, add 2-chloro-5-nitrotrifluorotoluene, stir and heat to 115-122°C, react for 12-15 hours; filter, distill under reduced pressure, recrystallize using ethylene glycol methyl ether, filter, and dry to obtain a dinitro compound;

[0020] Mix a dinitro compound, carbon black, ferric chloride and ethylene glycol methyl ether, heat to 108-112° C., drop hydrazine hydrate, and react for 12-13 hours; filter, add hydrochloric acid to the filtrate, adjust the pH of the system to 10±0.2 with ammonia water, filter, wash the precipitate, recrystallize with anhydrous ethanol, and vacuum dry to obtain a fluorine-containing diamine;

[0021] Take epoxidized castor oil, fluorinated diamine and ether, mix them at 0-6°C, heat to 27-34°C, stir and reflux for 60-120 minutes; distill under reduced pressure, wash and dry to obtain fluorinated castor oil.

[0022] Furthermore, in the preparation of epoxidized castor oil, the mass ratio of castor oil, glacial acetic acid, cationic resin, and hydrogen peroxide is 10:(1.82-1.86):(2.70-2.75):(1.84-1.88);

[0023] The ratio of castor oil to toluene is 2 g / mL;

[0024] Hydrogen peroxide was added in the form of a 30 wt % hydrogen peroxide aqueous solution.

[0025] Furthermore, in the preparation of the dinitro compound, the molar ratio of bisphenol AF, 2-chloro-5-nitrotrifluorotoluene, and anhydrous potassium carbonate is 1:(2.0-2.1):1;

[0026] The ratio of bisphenol AF to N,N'-dimethylformamide is 80 g / 100 mL.

[0027] Furthermore, in the preparation of the fluorinated diamine, the ratio of the dinitro compound, hydrazine hydrate, carbon black, and ferric chloride is 10:(0.49-0.55):(0.07-0.09):(2.83-2.88);

[0028] The ratio of dinitro compound and ethylene glycol methyl ether is 7.5 g / 10 mL;

[0029] Hydrazine hydrate is added in the form of an 85 wt % hydrazine hydrate aqueous solution;

[0030] The hydrochloric acid concentration was 25 wt%.

[0031] Furthermore, in the preparation of the fluorinated diamine, the mass ratio of epoxidized castor oil to the fluorinated diamine is 10:(20.6-21.0);

[0032] The ratio of epoxidized castor oil to ether is 10 g / 100 mL.

[0033] Furthermore, the oxygen-free curing anti-fingerprint resin also includes 5 to 10 parts of fluorine-containing acrylate, and the specific preparation process is as follows:

[0034] Take a mixture of fluorinated diamine and anhydrous ethanol, stir and add tripropylene glycol diacrylate under the protection of nitrogen atmosphere, and react at a temperature of 32-37° C. for 12 hours to obtain fluorinated acrylate.

[0035] Further, the mass ratio of fluorinated diamine to tripropylene glycol diacrylate is 10:(9.20-9.65);

[0036] The ratio of fluorinated diamine to anhydrous ethanol is 50 g / 100 mL.

[0037] In the above technical scheme, dibutyltin dilaurate is used as a catalyst, castor oil is used as a polyol, and it is reacted with isophorone diisocyanate to prepare a polyurethane prepolymer, and hydroxy polydimethylsiloxane is added for silicone modification, which can reduce the surface energy of the prepared polyurethane acrylate, improve the hydrophobicity of the coating (anti-fingerprint layer), and improve its anti-fouling and easy-to-clean capabilities; at the same time, due to the difference in surface energy between the polydimethylsiloxane chain segment and the acrylate copolymer and the acrylic acid monomer, a more obvious phase separation occurs between the polyurethane acrylate and other resins (acrylate copolymer, acrylic acid monomer), and the longer the polydimethylsiloxane chain segment, the more serious the phase separation phenomenon, which intensifies the unbalanced stress generated during the curing process of the coating (anaerobic curing anti-fingerprint resin) and promotes the generation of wrinkles on the coating surface. Then, hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine and hydroxyl-containing acrylate are added as end-capping agents to improve the antibacterial ability of the coating to a certain extent, and double bonds are introduced into the molecular structure of polyurethane acrylate, so that it can participate in polymerization with other components under the action of photoinitiators, increase the cross-linking degree of the coating system, and improve its comprehensive properties such as hardness, strength, and adhesion. Higher hardness can make the coating have long-lasting and stable antifouling properties.

[0038] In the above technical scheme, the unsaturated double bonds in castor oil are first epoxidized by glacial acetic acid to obtain epoxidized castor oil. The two phenolic hydroxyl groups in bisphenol AF react with the chlorine group in 2-chloro-5-nitrotrifluorotoluene to obtain an etherified product with a dinitro end, which is recorded as a dinitro compound; then the nitro group is converted into an amino group to form a fluorinated diamine. The obtained fluorinated diamine is reacted with epoxidized castor oil to graft the trifluorotoluene phenoxyhexafluoropropane structure on the castor oil molecular chain, which can effectively improve the hydrophobicity, stability and corrosion resistance of the prepared polyurethane acrylate, so that the prepared coating has higher hardness, water resistance, antifouling and easy cleaning, heat resistance and corrosion resistance. At the same time, the grafting of fluorinated diamine increases the crosslinking degree of polyurethane acrylate, and the comprehensive properties of the prepared coating such as strength and adhesion can be improved.

[0039] The introduction of trifluorotoluene phenoxyhexafluoropropane on the side chain of castor oil molecules can further reduce the surface energy of polyurethane acrylate, promote its phase separation with acrylate copolymer and acrylate monomer, enhance the contrast, intensify the unbalanced stress during the curing process, and further promote the formation of wrinkles on the coating surface.

[0040] In the above technical scheme, a fluorinated acrylate is added to the acrylic monomer system. The fluorinated acrylate is obtained by reacting the aforementioned fluorinated diamine with tripropylene glycol diacrylate, and is formed by addition between an amino group and an unsaturated double bond. The fluorinated acrylate contains double bonds and can participate in polymerization during the curing process. While improving the surface properties of the coating such as hydrophobicity, anti-fouling, and anti-fingerprint, it is also compatible with polyurethane acrylate, which helps polyurethane acrylate participate in the double bond polymerization between acrylate copolymers and acrylate monomers, thereby enhancing the adhesion and strength of the prepared coating and improving its hydrophobicity, anti-fouling, and anti-fingerprint capabilities.

[0041] The invention discloses an application of an oxygen-free curing anti-fingerprint resin, and adopts the oxygen-free curing anti-fingerprint resin to prepare anti-fingerprint decorative paper.

[0042] Furthermore, the anti-fingerprint decorative paper comprises the following layer structures from top to bottom: an anti-fingerprint layer, a first filling layer, paper, a second filling layer and an adhesive layer;

[0043] The anti-fingerprint layer is obtained by coating and curing an oxygen-free curing anti-fingerprint resin; the first filling layer is amino-acrylic resin; the second filling layer is amino resin; and the bonding layer is polyurethane acrylate.

[0044] Furthermore, in the preparation of the anti-fingerprint layer, the coating amount of the oxygen-free curing anti-fingerprint resin is 25 to 30 g / m 2 .

[0045] Furthermore, in the preparation of the anti-fingerprint layer, the curing process conditions are: first pre-bake at 40-50°C for 20-30 minutes; then pre-cure with a nitrogen-protected excimer lamp; and finally UV curing or electron beam curing;

[0046] If UV curing is selected, a photoinitiator needs to be added during the preparation stage of the anti-fingerprint resin.

[0047] Furthermore, in the pre-curing process, the curing energy of the nitrogen-protected excimer lamp (wavelength 172nm) pre-curing is 10-15mJ / cm 2 .

[0048] Furthermore, UV curing uses a mercury lamp for 3 to 5 seconds with an irradiation intensity of 250 to 350 mJ / cm 2 ;

[0049] The radiation dose for electron beam curing is 16 to 80 keV.

[0050] Furthermore, the anti-fingerprint decorative paper can be used to make an anti-fingerprint decorative board.

[0051] The anti-fingerprint decorative plate comprises the following structures from top to bottom: anti-fingerprint decorative paper, substrate and balancing layer;

[0052] The substrate is particle board, solid wood board, acrylic board or other board materials;

[0053] The balancing layer is melamine impregnated paper, anti-fingerprint decorative paper, PET facing or other film materials.

[0054] In the above technical scheme, polyurethane acrylate, acrylate copolymer and acrylate monomer are used as resin components, and a photoinitiator is added to form an oxygen-free curable anti-fingerprint resin. Under the irradiation of an anaerobic excimer lamp, the resin components are polymerized, and a shrinkage gradient is formed in the thickness direction due to the different shrinkage ratios of polyurethane acrylate, acrylate copolymer and acrylate monomer, so that a compression / tensile stress difference is formed between the surface and the interior of the coating (anti-fingerprint layer), thereby causing shrinkage wrinkles on the surface, and showing a delicate and smooth feeling, achieving the skin-feeling effect of the coating. Then, UV irradiation is carried out under a mercury lamp to cure the coating as a whole to obtain an anti-fingerprint layer, which helps to achieve its surface anti-fingerprint effect.

[0055] In the initial stage of curing, the acrylate monomer is prepolymerized to form a relatively hard thin layer on the surface of the coating; as the curing process proceeds, incompatibility exists between the composite system of polyurethane acrylate and acrylate copolymer, resulting in phase separation; due to its low surface tension characteristics, the polyurethane acrylate migrates to the surface to a certain extent, and through the difference in surface tension, it causes the coating to shrink unevenly, generates internal stress during curing and shrinkage, forms unbalanced stress, and brings about mechanical instability. The acrylate monomer deforms to balance the aforementioned internal stress, and the hard thin layer on the surface is compressed by the compressive stress generated by the prepolymer that continues to cure after UV irradiation, thereby forming a wrinkled texture on the surface of the coating (anti-fingerprint layer), showing certain skin-feel properties.

[0056] Compared with the prior art, the present invention has the following beneficial effects:

[0057] The present invention describes an anaerobic curing anti-fingerprint resin, which forms wrinkles on the surface of the anaerobic curing anti-fingerprint resin through appropriate processes and anaerobic excimer lamp irradiation, thereby achieving a skin-feel effect on the surface of the decorative panel; and improves the surface anti-fingerprint effect through the preparation process of the components and the control of the components. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0059] Figure 1 It is the anti-fingerprint layer prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0060] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0061] In the following specific implementations,

[0062] Polyurethane acrylate: U-CURE 9531, from Kunshan Custer Polymer Materials Co., Ltd.;

[0063] Acrylate copolymer: acrylic acid-acrylate copolymer (25133-97-5), sourced from Hubei Jusheng Technology Co., Ltd.;

[0064] Castor oil (CO): from Shanghai Myril Biochemical Technology Co., Ltd.;

[0065] Cationic resin: SK110, from Mitsubishi Chemical Corporation;

[0066] Carbon black: Wokai activated carbon powder, analytical grade, from Sinopharm Chemical Reagent Co., Ltd.;

[0067] Hydroxypolydimethylsiloxane: dihydroxy-terminated polydimethylsiloxane, MCR-C62Mn=5000, from Shanghai Myrel Biochemical Technology Co., Ltd.

[0068] The "parts" mentioned below are all parts by mass; the specific implementation methods below are all small-scale experimental trials.

[0069] Embodiment 1: A method for preparing an oxygen-free curing anti-fingerprint resin, comprising the following process:

[0070] S1. Fluorination modification of castor oil:

[0071] Take 10g of castor oil, 1.82g of glacial acetic acid, 2.70g of cationic resin and 5mL of toluene, stir and mix, place at 55°C, add 1.84g of hydrogen peroxide (added in the form of 30wt% hydrogen peroxide aqueous solution), react for 7h; wash with sodium carbonate aqueous solution, filter, remove toluene by rotary evaporation, and dry at 70°C for 150min to obtain epoxidized castor oil;

[0072] 8 g of bisphenol AF, anhydrous potassium carbonate and 10 mL of N,N'-dimethylformamide were mixed, 2-chloro-5-nitrotrifluorotoluene was added, the mixture was stirred and heated to 115°C, and the reaction was continued for 12 hours; the mixture was filtered, distilled under reduced pressure, recrystallized using ethylene glycol methyl ether, filtered, and dried to obtain a dinitro compound; the molar ratio of bisphenol AF, 2-chloro-5-nitrotrifluorotoluene and anhydrous potassium carbonate was 1:2.0:1;

[0073] 7.5 g of a dinitro compound, carbon black, ferric chloride and 10 mL of ethylene glycol methyl ether were mixed, the temperature was raised to 108° C., hydrazine hydrate (added in the form of an 85 wt % hydrazine hydrate aqueous solution) was added dropwise, and the mixture was reacted for 12 h; the mixture was filtered, 25 wt % hydrochloric acid was added to the filtrate, the pH value of the system was adjusted to 10 with aqueous ammonia, the mixture was filtered, the precipitate was washed, recrystallized with anhydrous ethanol, and vacuum dried to obtain a fluorinated diamine; the ratio of the dinitro compound, hydrazine hydrate, carbon black and ferric chloride was 10:0.49:0.07:2.83;

[0074] Take 10g of epoxidized castor oil, fluorinated diamine and 100mL of ether, mix them at 0°C, heat to 27°C, stir and reflux for 60min; distill under reduced pressure, wash and dry to obtain fluorinated castor oil; the mass ratio of epoxidized castor oil to fluorinated diamine is 10:20.6;

[0075] S2. Preparation of polyurethane acrylate:

[0076] 22.5 g of isophorone diisocyanate and 50 g of ethyl acetate were mixed, the temperature was raised to 40° C., fluorinated castor oil and catalyst dibutyltin dilaurate (0.1 wt% of the mass of fluorinated castor oil) were added, and the reaction was kept warm for 125 min;

[0077] The temperature was raised to 50°C, and hydroxypolydimethylsiloxane and catalyst dibutyltin dilaurate (0.1wt% of the mass of hydroxypolydimethylsiloxane) were added dropwise over 30 minutes, and the temperature was raised to 60°C, and the reaction was stirred for 125 minutes;

[0078] The temperature was raised to 70° C., hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine, hydroxyl-containing acrylate, catalyst dibutyltin dilaurate (0.1wt% of the total mass of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine and hydroxyl-containing acrylate) and 4-methoxyphenol (0.1wt% of the mass of hydroxyl-containing acrylate) were added dropwise, and the addition was completed within 2 hours. The mixture was kept warm and reacted until the -NCO group content was ≤0.1%. Triethylamine was added for neutralization reaction for 20 minutes to obtain polyurethane acrylate. The polyurethane acrylate included the following components by mass: 24.7 parts of isophorone diisocyanate, 54.8 parts of fluorinated castor oil, 10 parts of hydroxyl polydimethylsiloxane, 8 parts of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine, and 5 parts of hydroxyl-containing acrylate. The hydroxyl-containing acrylate was a mixture of pentaerythritol triacrylate, hydroxyethyl acrylate, and triethylene glycol diacrylate in a mass ratio of 1:3:2.

[0079] S3. Preparation of fluorinated acrylate:

[0080] Take 10g of fluorinated diamine and 20mL of anhydrous ethanol, mix them, stir under nitrogen atmosphere, add 9.20g of tripropylene glycol diacrylate, and react at 32°C for 12h to obtain fluorinated acrylate;

[0081] S4. Preparation of oxygen-free curing anti-fingerprint resin:

[0082] Take polyurethane acrylate, acrylate copolymer, ethoxylated trimethylolpropane triacrylate, cyclotrimethylolpropane formal acrylate, ditrimethylolpropane tetraacrylate, tripropylene glycol diacrylate, 1,6-ethylene glycol diacrylate, hydroxyethyl methacrylate, trimethylolpropane triacrylate, fluorine-containing acrylate, photoinitiator and ethyl acetate, stir and mix at a speed of 400 r / min; adjust the speed to 700 r / min, continue stirring for 45 minutes, and obtain an oxygen-free curing anti-fingerprint resin; the oxygen-free curing anti-fingerprint resin includes the following mass components: 17 The invention discloses a novel novel nanostructured carbon foam prepared from the present invention comprises the following components: polyurethane acrylate, 3 parts of acrylate copolymer, 18 parts of ethoxylated trimethylolpropane triacrylate, 7 parts of cyclotrimethylolpropane formal acrylate, 8 parts of ditrimethylolpropane tetraacrylate, 2 parts of tripropylene glycol diacrylate, 20 parts of 1,6-ethylene glycol diacrylate, 5 parts of hydroxyethyl methacrylate, 5 parts of trimethylolpropane triacrylate, 5 parts of fluorine-containing acrylate and 2.3 parts of photoinitiator; the photoinitiator is 1 part of methyl benzoylformate, 0.3 parts of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide and 1 part of 1-hydroxycyclohexyl phenyl acetone.

[0083] Embodiment 2: A method for preparing an oxygen-free curing anti-fingerprint resin, comprising the following process:

[0084] S1. Fluorination modification of castor oil:

[0085] Take 10g castor oil, 1.84g glacial acetic acid, 2.72g cationic resin and 5mL toluene, stir and mix, place at 58°C, add 1.86g hydrogen peroxide (added in the form of 30wt% hydrogen peroxide aqueous solution), react for 7.5h; wash with sodium carbonate aqueous solution, filter, remove toluene by rotary evaporation, and dry at 75°C for 120min to obtain epoxidized castor oil;

[0086] 8 g of bisphenol AF, anhydrous potassium carbonate and 10 mL of N,N'-dimethylformamide were mixed, 2-chloro-5-nitrotrifluorotoluene was added, the mixture was stirred and heated to 120°C, and the reaction was carried out for 13 hours; the mixture was filtered, distilled under reduced pressure, recrystallized using ethylene glycol methyl ether, filtered, and dried to obtain a dinitro compound; the molar ratio of bisphenol AF, 2-chloro-5-nitrotrifluorotoluene and anhydrous potassium carbonate was 1:2.05:1;

[0087] 7.5 g of a dinitro compound, carbon black, ferric chloride and 10 mL of ethylene glycol methyl ether were mixed, the temperature was raised to 108° C., hydrazine hydrate (added in the form of an 85 wt % hydrazine hydrate aqueous solution) was added dropwise, and the reaction was continued for 12.5 h; the mixture was filtered, 25 wt % hydrochloric acid was added to the filtrate, the pH value of the system was adjusted to 10 with aqueous ammonia, the mixture was filtered, the precipitate was washed, recrystallized with anhydrous ethanol, and vacuum dried to obtain a fluorinated diamine; the ratio of the dinitro compound, hydrazine hydrate, carbon black and ferric chloride was 10:0.52:0.08:2.85;

[0088] Take 10g of epoxidized castor oil, fluorinated diamine and 100mL of ether, mix them at 3°C, heat to 30°C, stir and reflux for 90min; distill under reduced pressure, wash and dry to obtain fluorinated castor oil; the mass ratio of epoxidized castor oil to fluorinated diamine is 10:20.8;

[0089] S2. Preparation of polyurethane acrylate:

[0090] 22.5 g of isophorone diisocyanate and 50 g of ethyl acetate were mixed, the temperature was raised to 45° C., fluorinated castor oil and catalyst dibutyltin dilaurate (0.1 wt% of the mass of fluorinated castor oil) were added, and the mixture was kept warm for 120 min.

[0091] The temperature was raised to 55°C, and hydroxypolydimethylsiloxane and catalyst dibutyltin dilaurate (0.1wt% of the mass of hydroxypolydimethylsiloxane) were added dropwise over 30 minutes, and the temperature was raised to 65°C, and the reaction was stirred for 120 minutes;

[0092] The temperature was raised to 75° C., hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine, hydroxyl-containing acrylate, catalyst dibutyltin dilaurate (0.1wt% of the total mass of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine and hydroxyl-containing acrylate) and 4-methoxyphenol (0.1wt% of the mass of hydroxyl-containing acrylate) were added dropwise, and the addition was completed within 2 hours. The mixture was kept warm and reacted until the -NCO group content was ≤0.1%. Triethylamine was added for neutralization reaction for 25 minutes to obtain polyurethane acrylate. The polyurethane acrylate included the following components by mass: 24.8 parts of isophorone diisocyanate, 54.9 parts of fluorinated castor oil, 6.5 parts of hydroxyl polydimethylsiloxane, 9 parts of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine, and 6 parts of hydroxyl-containing acrylate. The hydroxyl-containing acrylate was a mixture of pentaerythritol triacrylate, hydroxyethyl acrylate, and triethylene glycol diacrylate in a mass ratio of 1:3:2.

[0093] S3. Preparation of fluorinated acrylate:

[0094] Take 10g of fluorinated diamine and 20mL of anhydrous ethanol, mix them, stir under nitrogen atmosphere, add 9.42g of tripropylene glycol diacrylate, and react at 35°C for 12h to obtain fluorinated acrylate;

[0095] S4. Preparation of oxygen-free curing anti-fingerprint resin:

[0096] Take polyurethane acrylate, acrylate copolymer, ethoxylated trimethylolpropane triacrylate, cyclotrimethylolpropane formal acrylate, ditrimethylolpropane tetraacrylate, tripropylene glycol diacrylate, 1,6-ethylene glycol diacrylate, hydroxyethyl methacrylate, trimethylolpropane triacrylate, fluorine-containing acrylate, photoinitiator and ethyl acetate, stir and mix at a speed of 600 r / min; adjust the speed to 850 r / min, continue stirring for 38 minutes, and obtain an anaerobic curing anti-fingerprint resin; the anaerobic curing anti-fingerprint resin includes the following mass components: 14 parts of polyurethane acrylate, 2.5 parts of acrylate copolymer, 19 parts of ethoxylated trimethylolpropane triacrylate, 7.5 parts of cyclotrimethylolpropane formal acrylate, 9 parts of ditrimethylolpropane tetraacrylate, 3.5 parts of tripropylene glycol diacrylate, 22.5 parts of 1,6-ethylene glycol diacrylate, 7.5 parts of hydroxyethyl methacrylate, 7.5 parts of trimethylolpropane triacrylate, 7.5 parts of fluorine-containing acrylate and 3.4 parts of photoinitiator; the photoinitiator is 1.5 parts of methyl benzoylformate, 0.4 parts of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide and 1.5 parts of 1-hydroxycyclohexyl phenyl acetone.

[0097] Embodiment 3: A method for preparing an oxygen-free curing anti-fingerprint resin, comprising the following process:

[0098] S1. Fluorination modification of castor oil:

[0099] Take 10g castor oil, 1.86g glacial acetic acid, 2.75g cationic resin and 5mL toluene, stir and mix, place at 60°C, add 1.88g hydrogen peroxide (added in the form of 30wt% hydrogen peroxide aqueous solution), react for 8h; wash with sodium carbonate aqueous solution, filter, remove toluene by rotary evaporation, and dry at 80°C for 100min to obtain epoxidized castor oil;

[0100] 8 g of bisphenol AF, anhydrous potassium carbonate and 10 mL of N,N'-dimethylformamide were mixed, 2-chloro-5-nitrotrifluorotoluene was added, the mixture was stirred and heated to 122°C, and the reaction was carried out for 12 hours; the mixture was filtered, distilled under reduced pressure, recrystallized using ethylene glycol methyl ether, filtered, and dried to obtain a dinitro compound; the molar ratio of bisphenol AF, 2-chloro-5-nitrotrifluorotoluene and anhydrous potassium carbonate was 1:2.1:1;

[0101] 7.5 g of a dinitro compound, carbon black, ferric chloride and 10 mL of ethylene glycol methyl ether were mixed, the temperature was raised to 112° C., hydrazine hydrate (added in the form of an 85 wt % hydrazine hydrate aqueous solution) was added dropwise, and the reaction was continued for 12 h; the mixture was filtered, 25 wt % hydrochloric acid was added to the filtrate, the pH value of the system was adjusted to 10 with aqueous ammonia, the mixture was filtered, the precipitate was washed, recrystallized with anhydrous ethanol, and vacuum dried to obtain a fluorinated diamine; the ratio of the dinitro compound, hydrazine hydrate, carbon black and ferric chloride was 10:0.55:0.09:2.88;

[0102] Take 10g of epoxidized castor oil, fluorinated diamine and 100mL of ether, mix them at 6°C, heat to 34°C, stir and reflux for 60min; distill under reduced pressure, wash and dry to obtain fluorinated castor oil; the mass ratio of epoxidized castor oil to fluorinated diamine is 10:21.0;

[0103] S2. Preparation of polyurethane acrylate:

[0104] 22.5 g of isophorone diisocyanate and 50 g of ethyl acetate were mixed, the temperature was raised to 50° C., fluorinated castor oil and catalyst dibutyltin dilaurate (0.1 wt% of the mass of fluorinated castor oil) were added, and the reaction was kept warm for 115 min;

[0105] The temperature was raised to 60°C, and hydroxypolydimethylsiloxane and catalyst dibutyltin dilaurate (0.1wt% of the mass of hydroxypolydimethylsiloxane) were added dropwise over 30 minutes, and the temperature was raised to 70°C, and the reaction was stirred for 115 minutes;

[0106] The temperature was raised to 80° C., hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine, hydroxyl-containing acrylate, catalyst dibutyltin dilaurate (0.1wt% of the total mass of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine and hydroxyl-containing acrylate) and 4-methoxyphenol (0.1wt% of the mass of hydroxyl-containing acrylate) were added dropwise, and the addition was completed within 2 hours. The mixture was kept warm and reacted until the -NCO group content was ≤0.1%. Triethylamine was added for neutralization reaction for 30 minutes to obtain polyurethane acrylate. The polyurethane acrylate included the following components by mass: 25.0 parts of isophorone diisocyanate, 55.0 parts of fluorinated castor oil, 8 parts of hydroxyl polydimethylsiloxane, 10 parts of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine, and 7 parts of hydroxyl-containing acrylate. The hydroxyl-containing acrylate was a mixture of pentaerythritol triacrylate, hydroxyethyl acrylate, and triethylene glycol diacrylate in a mass ratio of 1:3:2.

[0107] S3. Preparation of fluorinated acrylate:

[0108] Take 10g of fluorinated diamine and 20mL of anhydrous ethanol, mix them, stir under nitrogen atmosphere, add 9.65g of tripropylene glycol diacrylate, and react at 37°C for 12h to obtain fluorinated acrylate;

[0109] S4. Preparation of oxygen-free curing anti-fingerprint resin:

[0110] Take polyurethane acrylate, acrylate copolymer, ethoxylated trimethylolpropane triacrylate, cyclotrimethylolpropane formal acrylate, ditrimethylolpropane tetraacrylate, tripropylene glycol diacrylate, 1,6-ethylene glycol diacrylate, hydroxyethyl methacrylate, trimethylolpropane triacrylate, fluorine-containing acrylate, photoinitiator and ethyl acetate, stir and mix at a speed of 750 r / min; adjust the speed to 1200 r / min, continue stirring for 30 minutes, and obtain an anaerobic curing anti-fingerprint resin; the anaerobic curing anti-fingerprint resin includes the following mass components: 11 parts Polyurethane acrylate, 2 parts of acrylate copolymer, 20 parts of ethoxylated trimethylolpropane triacrylate, 8 parts of cyclotrimethylolpropane formal acrylate, 10 parts of ditrimethylolpropane tetraacrylate, 5 parts of tripropylene glycol diacrylate, 25 parts of 1,6-ethylene glycol diacrylate, 10 parts of hydroxyethyl methacrylate, 10 parts of trimethylolpropane triacrylate, 10 parts of fluorine-containing acrylate and 4.5 parts of photoinitiator; the photoinitiator is 2 parts of methyl benzoylformate, 0.5 parts of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide and 2 parts of 1-hydroxycyclohexyl phenyl acetone.

[0111] Embodiment 4: A method for preparing an oxygen-free curing anti-fingerprint resin, comprising the following process:

[0112] S1-S3 are the same as in Example 3;

[0113] S4. Preparation of oxygen-free curing anti-fingerprint resin:

[0114] Take polyurethane acrylate, acrylate copolymer, ethoxylated trimethylolpropane triacrylate, cyclotrimethylolpropane formal acrylate, ditrimethylolpropane tetraacrylate, tripropylene glycol diacrylate, 1,6-ethylene glycol diacrylate, hydroxyethyl methacrylate, trimethylolpropane triacrylate, fluorine-containing acrylate and ethyl acetate, stir and mix at a speed of 750 r / min; adjust the speed to 1200 r / min, continue stirring for 30 minutes, and obtain an anaerobic curing anti-fingerprint resin; the anaerobic curing anti-fingerprint resin includes the following mass components: 11 parts of polyurethane acrylate, 2 parts of acrylate copolymer, 20 parts of ethoxylated trimethylolpropane triacrylate, 8 parts of cyclotrimethylolpropane formal acrylate, 10 parts of ditrimethylolpropane tetraacrylate, 5 parts of tripropylene glycol diacrylate, 25 parts of 1,6-ethylene glycol diacrylate, 10 parts of hydroxyethyl methacrylate, 10 parts of trimethylolpropane triacrylate, and 10 parts of fluorine-containing acrylate.

[0115] Comparative Example 1: A method for preparing an oxygen-free curing anti-fingerprint resin, comprising the following process:

[0116] S1-S2 are the same as in Example 1;

[0117] S3. Preparation of oxygen-free curing anti-fingerprint resin:

[0118] Take polyurethane acrylate, acrylate copolymer, ethoxylated trimethylolpropane triacrylate, cyclotrimethylolpropane formal acrylate, ditrimethylolpropane tetraacrylate, tripropylene glycol diacrylate, 1,6-ethylene glycol diacrylate, hydroxyethyl methacrylate, trimethylolpropane triacrylate, tridecafluorooctyl methacrylate, photoinitiator and ethyl acetate, stir and mix at a speed of 400 r / min; adjust the speed to 700 r / min, continue stirring for 45 minutes, and obtain an oxygen-free curing anti-fingerprint resin; the oxygen-free curing anti-fingerprint resin includes the following mass components: 17 The invention discloses a novel novel nanostructured carbon foam prepared from the invention comprises the following: parts of polyurethane acrylate, 3 parts of acrylate copolymer, 18 parts of ethoxylated trimethylolpropane triacrylate, 7 parts of cyclotrimethylolpropane formal acrylate, 8 parts of ditrimethylolpropane tetraacrylate, 2 parts of tripropylene glycol diacrylate, 20 parts of 1,6-ethylene glycol diacrylate, 5 parts of hydroxyethyl methacrylate, 5 parts of trimethylolpropane triacrylate, 5 parts of tridecafluorooctyl methacrylate and 2.3 parts of photoinitiator; the photoinitiator is 1 part of methyl benzoylformate, 0.3 parts of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide and 1 part of 1-hydroxycyclohexyl phenyl acetone.

[0119] Comparative Example 2: A method for preparing an oxygen-free curing anti-fingerprint resin, comprising the following process:

[0120] S1. Preparation of polyurethane acrylate:

[0121] 22.5 g of isophorone diisocyanate and 50 g of ethyl acetate were mixed, the temperature was raised to 40° C., castor oil and catalyst dibutyltin dilaurate (0.1 wt% of the mass of castor oil) were added, and the reaction was kept warm for 125 min;

[0122] The temperature was raised to 50°C, and hydroxypolydimethylsiloxane and catalyst dibutyltin dilaurate (0.1wt% of the mass of hydroxypolydimethylsiloxane) were added dropwise over 30 minutes, and the temperature was raised to 60°C, and the reaction was stirred for 125 minutes;

[0123] The temperature was raised to 70° C., hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine, hydroxyl-containing acrylate, catalyst dibutyltin dilaurate (0.1wt% of the total mass of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine and hydroxyl-containing acrylate) and 4-methoxyphenol (0.1wt% of the mass of hydroxyl-containing acrylate) were added dropwise, and the addition was completed within 2 hours. The mixture was kept warm and reacted until the -NCO group content was ≤0.1%. Triethylamine was added for neutralization reaction for 20 minutes to obtain polyurethane acrylate. The polyurethane acrylate included the following components by mass: 24.7 parts of isophorone diisocyanate, 54.8 parts of castor oil, 10 parts of hydroxyl polydimethylsiloxane, 8 parts of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine, and 5 parts of hydroxyl-containing acrylate. The hydroxyl-containing acrylate was a mixture of pentaerythritol triacrylate, hydroxyethyl acrylate, and triethylene glycol diacrylate in a mass ratio of 1:3:2.

[0124] S2. Preparation of oxygen-free curing anti-fingerprint resin:

[0125] Take polyurethane acrylate, acrylate copolymer, ethoxylated trimethylolpropane triacrylate, cyclotrimethylolpropane formal acrylate, ditrimethylolpropane tetraacrylate, tripropylene glycol diacrylate, 1,6-ethylene glycol diacrylate, hydroxyethyl methacrylate, trimethylolpropane triacrylate, tridecafluorooctyl methacrylate, photoinitiator and ethyl acetate, stir and mix at a speed of 400 r / min; adjust the speed to 700 r / min, continue stirring for 45 minutes, and obtain an oxygen-free curing anti-fingerprint resin; the oxygen-free curing anti-fingerprint resin includes the following mass components: 17 The invention discloses a novel novel nanostructured carbon foam prepared from the invention comprises the following: parts of polyurethane acrylate, 3 parts of acrylate copolymer, 18 parts of ethoxylated trimethylolpropane triacrylate, 7 parts of cyclotrimethylolpropane formal acrylate, 8 parts of ditrimethylolpropane tetraacrylate, 2 parts of tripropylene glycol diacrylate, 20 parts of 1,6-ethylene glycol diacrylate, 5 parts of hydroxyethyl methacrylate, 5 parts of trimethylolpropane triacrylate, 5 parts of tridecafluorooctyl methacrylate and 2.3 parts of photoinitiator; the photoinitiator is 1 part of methyl benzoylformate, 0.3 parts of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide and 1 part of 1-hydroxycyclohexyl phenyl acetone.

[0126] Comparative Example 3: A method for preparing an oxygen-free curing anti-fingerprint resin, comprising the following process:

[0127] Take polyurethane acrylate (U-CURE 9531), acrylate copolymer (25133-97-5), ethoxylated trimethylolpropane triacrylate, cyclotrimethylolpropane formal acrylate, ditrimethylolpropane tetraacrylate, tripropylene glycol diacrylate, 1,6-ethylene glycol diacrylate, hydroxyethyl methacrylate, trimethylolpropane triacrylate, tridecafluorooctyl methacrylate, photoinitiator and ethyl acetate, stir and mix at a speed of 400 r / min; adjust the speed to 700 r / min, continue stirring for 45 minutes, and obtain an anaerobic curing anti-fingerprint resin; the anaerobic curing anti-fingerprint resin includes the following mass Components: 17 parts of polyurethane acrylate, 3 parts of acrylate copolymer, 18 parts of ethoxylated trimethylolpropane triacrylate, 7 parts of cyclotrimethylolpropane formal acrylate, 8 parts of ditrimethylolpropane tetraacrylate, 2 parts of tripropylene glycol diacrylate, 20 parts of 1,6-ethylene glycol diacrylate, 5 parts of hydroxyethyl methacrylate, 5 parts of trimethylolpropane triacrylate, 5 parts of tridecafluorooctyl methacrylate and 2.3 parts of photoinitiator; the photoinitiator is 1 part of methyl benzoylformate, 0.3 parts of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide and 1 part of 1-hydroxycyclohexyl phenyl acetone.

[0128] Experiment: Take the oxygen-free curing anti-fingerprint resin obtained in Examples 1-3 and Comparative Examples 1-3 and apply it on the surface of the base paper at a coating amount of 25 g / m 2 , pre-bake at 45℃ for 25min; pre-cure with nitrogen protected excimer lamp (wavelength 172nm), curing energy 12mJ / cm 2 ; Mercury lamp curing for 4s, irradiation intensity 300mJ / cm 2 , forming an anti-fingerprint layer to prepare a sample;

[0129] The oxygen-free curing anti-fingerprint resin obtained in Example 4 was coated on the surface of the base paper at a coating amount of 25 g / m 2 , pre-bake at 45℃ for 25min; pre-cure with nitrogen protected excimer lamp (wavelength 172nm), curing energy 12mJ / cm 2 ; Electron beam curing, radiation dose of 30keV, to form an anti-fingerprint layer, to prepare a sample; the performance thereof was tested and the test results were recorded respectively:

[0130] Using CB / T 17657 as reference standard, test the adhesion and tensile strength of the specimens;

[0131] An optical contact angle meter was used to measure the contact angle (CA) of the sample, and the test liquid was 1.5 μL deionized water;

[0132] Anti-fingerprint performance test: Let the washed and dried finger stand naturally for 10 minutes, press hard on the sample surface for 5 seconds, remove it, observe the disappearance of the fingerprint and record the disappearance time, repeat 6 times for each group of samples;

[0133]

[0134]

[0135] According to the data in the above table, we can clearly draw the following conclusions:

[0136] The oxygen-free curable anti-fingerprint resin obtained in Example 1-4 is compared with the oxygen-free curable anti-fingerprint resin obtained in Comparative Example 1-3. The test results show that:

[0137] Compared with the comparative example, the anti-fingerprint layer obtained after curing the oxygen-free curable anti-fingerprint resin obtained in Examples 1-4 has a higher contact angle, tensile strength data, and more excellent fingerprint disappearance time and adhesion. This fully demonstrates that the present invention achieves the improvement of the strength, adhesion, hydrophobic antifouling and anti-fingerprint performance of the anti-fingerprint layer.

[0138] Compared with Example 1, the fluorinated acrylate in the oxygen-free curing anti-fingerprint resin of Comparative Example 1 is replaced by 13-fluorooctyl methacrylate; in the preparation of polyurethane acrylate in Comparative Example 2, fluorinated castor oil is replaced by castor oil, and the fluorinated acrylate in the oxygen-free curing anti-fingerprint resin is replaced by 13-fluorooctyl methacrylate; polyurethane acrylate in Comparative Example 3 is a commercially available product, and the fluorinated acrylate in the oxygen-free curing anti-fingerprint resin is replaced by 13-fluorooctyl methacrylate. The oxygen-free curing anti-fingerprint resins obtained in Comparative Examples 1-3 have reduced contact angles and tensile strength data for the anti-fingerprint layer produced, and the fingerprint disappearance time and adhesion data are deteriorated. It can be seen that the setting of the oxygen-free curing anti-fingerprint resin component and its process in the present invention can promote the improvement of the strength, adhesion, hydrophobic antifouling and anti-fingerprint properties of the produced anti-fingerprint layer.

[0139] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0140] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An oxygen-free curing anti-fingerprint resin, characterized in that: The invention comprises the following components by weight: 11 to 17 parts of polyurethane acrylate, 2 to 3 parts of acrylate copolymer, 18 to 20 parts of ethoxylated trimethylolpropane triacrylate, 7 to 8 parts of cyclotrimethylolpropane methylal acrylate, 8 to 10 parts of ditrimethylolpropane tetraacrylate, 2 to 5 parts of tripropylene glycol diacrylate, 20 to 25 parts of 1,6-ethylene glycol diacrylate, 5 to 10 parts of hydroxyethyl methacrylate, 5 to 10 parts of trimethylolpropane triacrylate and 0 to 4.5 parts of photoinitiator; The polyurethane acrylate is prepared by the following process: Mix isophorone diisocyanate and ethyl acetate, raise the temperature to 40-50°C, add castor oil and catalyst, and keep the temperature to react for 115-125 minutes; Raise the temperature to 50-60°C, add hydroxy polydimethylsiloxane and catalyst dropwise, add them over 30 minutes, raise the temperature to 60-70°C, and stir the reaction for 115-125 minutes; Raise the temperature to 70-80°C, add hexahydro-1,3,5-tri(hydroxyethyl)-s-triazine, hydroxyl-containing acrylate, catalyst and 4-methoxyphenol dropwise within 2 hours, and keep warm to react until the -NCO group content is ≤0.1%; add triethylamine for neutralization for 20-30 minutes to obtain polyurethane acrylate; The castor oil is fluorinated and modified by the following process: Castor oil, glacial acetic acid, cationic resin and toluene are mixed and stirred, placed at 55-60°C, hydrogen peroxide is added dropwise, and reacted for 7-8h to obtain epoxidized castor oil; Mix bisphenol AF, anhydrous potassium carbonate and N,N'-dimethylformamide, add 2-chloro-5-nitrotrifluorotoluene, stir and heat to 115-122°C, react for 12-15h to obtain a dinitro compound; Mix a dinitro compound, carbon black, ferric chloride and ethylene glycol methyl ether, raise the temperature to 108-112° C., drop hydrazine hydrate, and react for 12-13 hours to obtain a fluorine-containing diamine; Take epoxidized castor oil, fluorinated diamine and ether, mix them at 0-6°C, heat to 27-34°C, stir and reflux for 60-120 minutes to obtain fluorinated castor oil; The oxygen-free curing anti-fingerprint resin also includes 5 to 10 parts of fluorine-containing acrylate, and the specific preparation process is as follows: Take a mixture of fluorinated diamine and anhydrous ethanol, stir and add tripropylene glycol diacrylate under the protection of nitrogen atmosphere, and react at a temperature of 32-37° C. for 12 hours to obtain fluorinated acrylate.

2. The oxygen-free curing anti-fingerprint resin according to claim 1, characterized in that: The photoinitiator comprises the following components by weight: 1 to 2 parts of methyl benzoylformate, 0.3 to 0.5 parts of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and 1 to 2 parts of 1-hydroxycyclohexylphenylacetone.

3. The oxygen-free curing anti-fingerprint resin according to claim 1, characterized in that: The polyurethane acrylate comprises the following components by mass: 24.7-25.0 parts of isophorone diisocyanate, 54.8-55.0 parts of fluorine-containing castor oil, 5-8 parts of hydroxy polydimethylsiloxane, 8-10 parts of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine, and 5-7 parts of hydroxy-containing acrylate.

4. The oxygen-free curing anti-fingerprint resin according to claim 1, characterized in that: The mass ratio of the fluorine-containing diamine to tripropylene glycol diacrylate is 10:(9.20-9.65).

5. The method for preparing an oxygen-free curing anti-fingerprint resin according to claim 1, characterized in that: Including the following processes: Take polyurethane acrylate, acrylate copolymer, ethoxylated trimethylolpropane triacrylate, cyclotrimethylolpropane formal acrylate, ditrimethylolpropane tetraacrylate, tripropylene glycol diacrylate, 1,6-ethylene glycol diacrylate, hydroxyethyl methacrylate, trimethylolpropane triacrylate, fluorine-containing acrylate and ethyl acetate, stir and mix at a speed of 400-750 r / min; adjust the speed to 700-1200 r / min, continue stirring for 30-45 minutes, and obtain an oxygen-free curing anti-fingerprint resin.

6. Use of an oxygen-free curing anti-fingerprint resin according to any one of claims 1 to 4 or an oxygen-free curing anti-fingerprint resin prepared by the preparation method according to claim 5, characterized in that: Anti-fingerprint decorative paper is prepared by using oxygen-free curing anti-fingerprint resin; The anti-fingerprint decorative paper comprises the following layer structures from top to bottom: an anti-fingerprint layer, a first filling layer, paper, a second filling layer and a bonding layer, wherein the anti-fingerprint layer is obtained by coating and curing an oxygen-free curing anti-fingerprint resin; The anti-fingerprint decorative paper is used for making an anti-fingerprint decorative board.

7. The use of an oxygen-free curing anti-fingerprint resin according to claim 6, characterized in that: The curing process conditions after the anti-fingerprint layer is coated are: first pre-bake at 40-50°C for 20-30 minutes; then use nitrogen protection excimer lamp; and finally UV curing or electron beam curing; When UV curing is selected, a photoinitiator is added to the anti-fingerprint resin.