Method for determining liquid injection amount of cylindrical battery and liquid injection method of cylindrical battery
By calculating the pores and layer gaps of the positive electrode sheet, negative electrode sheet, and separator of the cylindrical battery, combined with the electrolyte consumption rate, the liquid injection amount is accurately calculated, which solves the problem of inaccurate liquid injection and improves the electrochemical performance and life of the battery.
Patent Information
- Application Number
- CN202410822572.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-25
AI Technical Summary
When calculating the liquid injection amount of a cylindrical battery, the existing technology ignores the core layer gap and the liquid injection amount of the Overhang, resulting in inaccurate liquid injection, prolonging the liquid injection time, and affecting the electrochemical performance.
By calculating the pores of the positive electrode sheet, the pores of the negative electrode sheet, the separator pores, the interlayer gaps and the consumption rate of the electrolyte during the formation process, we can accurately calculate the primary liquid injection volume and the secondary liquid injection volume, and utilize the mechanism of electrolyte consumption through the formation and later use of the battery. The model uses the same mechanism of electrolyte consumption during the process to achieve precise control of the amount of liquid injected.
It greatly reduces the extended liquid injection time caused by excessive or insufficient primary liquid injection volume, ensures sufficient electrode liquid volume, achieves precise control of the secondary liquid injection volume, and improves battery life and electrochemical performance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, and in particular to a method for determining a liquid injection amount of a cylindrical battery and a liquid injection method for a cylindrical battery. Background Art
[0002] With the development of technology, cylindrical batteries have the advantages of high production efficiency and high safety. Currently, large cylindrical batteries are increasingly favored by consumers in the energy storage market. However, due to the high volume space utilization rate of cylindrical batteries, some difficulties have been brought to the battery manufacturing end. Among them, when injecting liquid into the battery, the cylindrical battery has less space gaps, which makes it difficult to inject liquid into the battery, thus greatly prolonging the injection time of the battery. Therefore, the cylindrical battery injects the electrolyte in batches, forming the secondary injection technology used by most battery factories now.
[0003] For the current secondary injection technology, most battery designers usually do not have a reasonable method to design the primary injection amount and the secondary injection amount. In particular, in the calculation of the primary injection amount, the required injection amount in the "layer gap" and "overhang" of the core is usually ignored, resulting in inaccurate primary injection amount. In the calculation of the secondary injection amount, the secondary injection amount is usually determined based on experience or experimental results, resulting in inaccurate secondary injection amount.
[0004] Therefore, there is an urgent need to provide a method that can accurately calculate the primary injection volume and the secondary injection volume, so as to ensure the electrochemical performance of the cylindrical battery.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a method for determining the liquid injection amount of a cylindrical battery and a liquid injection method for a cylindrical battery, aiming to accurately calculate the primary liquid injection amount and the secondary liquid injection amount to improve the electrochemical performance of the battery.
[0007] The present invention is achieved in that:
[0008] In a first aspect, the present invention provides a method for determining the liquid injection amount of a cylindrical battery, comprising:
[0009] The amount of electrolyte injected once is calculated based on the pores of the positive electrode sheet, the pores of the negative electrode sheet, the pores of the diaphragm, the interlayer gaps, the gaps in the area where the negative electrode exceeds the positive electrode, and the consumption rate of the electrolyte during the formation process;
[0010] The secondary injection volume is calculated based on the consumption rate of the electrolyte during the formation process and the battery life requirements;
[0011] Among them, the calculation formula for one injection volume M1 is as follows:
[0012] M1=((V c +Va +V s +V τ +V o )×ρ)×k1+υ×(1-η)×C1;
[0013] Where V c Indicates the pores of the positive electrode sheet, in cm³;
[0014] V a Indicates the pores of the negative electrode sheet, in cm³;
[0015] V s Indicates the diaphragm pore size in cm³;
[0016] V τ Indicates the interlayer gap, in cm³;
[0017] V o Indicates the space between the negative electrode and the positive electrode, in cm³;
[0018] ρ represents the density of the electrolyte, in g / cm³;
[0019] k1 represents the coefficient, with a value of 1.00-1.05;
[0020] υ represents the consumption rate of electrolyte during the formation process, in g / mAh;
[0021] η represents the first coulombic efficiency;
[0022] C1 represents the first charge capacity of the formation, in mAh;
[0023] Secondary injection volume M2 = υ × k2 × (1-Sb) × C0;
[0024] Wherein, υ represents the consumption rate of electrolyte during the formation process, and the unit is g / mAh;
[0025] k2 is a constant with a value of 1-1.5;
[0026] Sb is the battery life requirement, ranging from 50% to 100%;
[0027] C0 is the rated capacity of the battery cell, in mAh.
[0028] In an alternative embodiment, V c =σc×Lc×Wc×Hc; wherein, σc represents the porosity of the positive electrode sheet, Lc represents the length of the positive electrode sheet, Wc represents the width of the positive electrode sheet dressing, and Hc represents the thickness of the positive electrode sheet after being immersed in the electrolyte for 24h-72h.
[0029] In an optional embodiment, Va=σa×La×Wa×Ha; wherein, σa represents the porosity of the negative electrode sheet, La represents the length of the negative electrode sheet, Wa represents the width of the negative electrode sheet dressing, and Ha represents the thickness of the negative electrode sheet after being immersed in the electrolyte for 24h-72h.
[0030] In an optional embodiment, Vs=σs×(Ls1+Ls2)×Ws×Hs; wherein σs represents the porosity of the diaphragm, Ls1 represents the length of the inner ring diaphragm, Ls2 represents the length of the outer ring diaphragm, Ws represents the width of the diaphragm, and Hs represents the thickness of the diaphragm.
[0031] In an optional embodiment, Vτ=La×Wa×Hτ; wherein La represents the length of the negative electrode sheet, Wa represents the width of the negative electrode sheet, and Hτ represents the interlayer gap.
[0032] In an optional embodiment, the interlayer gap Hτ is calculated as follows:
[0033] Hτ=(Dd) / (2×n)-(Ha+Hc+2×Hs); where n represents the number of windings of the negative electrode sheet, D is the core diameter, d is the winding needle diameter, Ha represents the thickness of the negative electrode sheet, Hc represents the thickness of the positive electrode sheet, and Hs represents the thickness of the separator.
[0034] In an optional embodiment, Vo=(Wa-Wc)×Lc×(Hτ+Hc); wherein Wa represents the width of the negative electrode sheet dressing, Wc represents the width of the positive electrode sheet dressing, Lc represents the length of the positive electrode sheet, Hτ represents the layer gap, and Hc represents the thickness of the positive electrode sheet;
[0035] The value range of Wa-Wc is 0.5mm-5mm.
[0036] In an optional embodiment, the consumption rate of the electrolyte during the formation process is υ=(m1-m2) / (C1-C2), and the first coulombic efficiency η=C2 / C1;
[0037] Among them, m1 is the mass of the electrolyte before formation, m2 is the mass of the electrolyte after formation, C1 is the first charge capacity after formation, and C2 is the first discharge capacity after formation;
[0038] Take the electrolyte before and after formation of the same design battery cell, and measure the mass fraction of the film-forming additive before and after formation. The mass fraction of the film-forming additive before formation is marked as P1, and the mass fraction of the film-forming additive after formation is marked as P2. m2 is calculated according to the following formula:
[0039] m2=(P2 / P1)×m1.
[0040] In a second aspect, the present invention provides a method for injecting liquid into a cylindrical battery, comprising: determining a primary injection volume and a secondary injection volume according to the determination method of any one of the aforementioned embodiments.
[0041] In an optional embodiment, the injection method includes: injecting a cylindrical battery cell once with a primary injection volume, then forming, aging, and discharging, and then injecting a second time with a secondary injection volume.
[0042] The present invention has the following beneficial effects: the amount of liquid injection is calculated based on the pores of the positive electrode sheet, the pores of the negative electrode sheet, the pores of the diaphragm, the interlayer gaps, the gaps of the negative electrode beyond the positive electrode area (overhang gaps) and the consumption rate of the electrolyte during the formation process. On the one hand, the injection time extension caused by excessive amount of liquid injection can be greatly reduced, and on the other hand, the problem of insufficient amount of electrode liquid required for formation due to insufficient amount of liquid injection can be avoided. The amount of liquid injection is calculated based on the consumption rate of electrolyte during the formation process and the battery life requirements. The model that the mechanism of electrolyte consumption during formation and the mechanism of electrolyte consumption during the later use of the battery are the same can achieve accurate control of the amount of liquid injection and control of the battery life. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0044] An embodiment of the present invention provides a method for determining the liquid filling amount of a cylindrical battery, comprising the following steps:
[0045] S1. Pre-calculation test
[0046] Calculate the positive electrode pore V c 、Negative electrode sheet pore V a 、Diaphragm pore V s , interlayer gap V τ 、The negative electrode exceeds the positive electrode area gap V o And the consumption rate of electrolyte during the formation process υ, the specific calculation steps are as follows:
[0047] (1) Calculate the positive electrode pore V c
[0048] Pore V of positive electrode c =σc×Lc×Wc×Hc; where σc represents the porosity of the positive electrode sheet, Lc represents the length of the positive electrode sheet, Wc represents the width of the positive electrode sheet dressing, and Hc represents the thickness of the positive electrode sheet after being immersed in the electrolyte for 24h-72h. The units of length, width and thickness are cm.
[0049] That is to say, when calculating the positive electrode pore V cBefore that, the length Lc and width Wc of the positive electrode sheet are measured first; the positive electrode sheet about 48 hours after rolling is placed in the electrolyte for sealing and soaking for 24 hours to 72 hours, and the thickness Hc of the positive electrode sheet after soaking is measured. According to the thickness Hc of the positive electrode sheet and the true density of each material in the electrode sheet formula, the porosity σc of the positive electrode sheet is calculated by conventional calculation methods.
[0050] (2) Calculate the pore size V of the negative electrode sheet a
[0051] Negative electrode sheet pore Va=σa×La×Wa×Ha; where σa represents the porosity of the negative electrode sheet. La represents the length of the negative electrode sheet, Wa represents the width of the negative electrode sheet dressing, and Ha represents the thickness of the negative electrode sheet after being immersed in the electrolyte for 24h-72h. The units of length, width, and thickness are cm.
[0052] That is to say, before calculating the negative electrode sheet pore Va, first measure the negative electrode sheet length La and negative electrode sheet width Wa; place the negative electrode sheet sealed and soaked in the electrolyte for 24h-72h after rolling for about 48h, and measure the thickness Ha of the negative electrode sheet after soaking. According to the thickness Ha of the negative electrode sheet and the true density of each material in the electrode sheet formula, the porosity σa of the negative electrode sheet is calculated by conventional calculation methods.
[0053] (3) Calculation of diaphragm pore V s
[0054] Diaphragm pore Vs = σs × (Ls1 + Ls2) × Ws × Hs; where σs represents the porosity of the diaphragm. Ls1 represents the length of the inner diaphragm, Ls2 represents the length of the outer diaphragm, Ws represents the width of the diaphragm, and Hs represents the thickness of the diaphragm. The units of length, width, and thickness are cm.
[0055] It should be noted that the product of the length (including the inner circle and the outer circle), width and thickness of the diaphragm is the volume of the diaphragm, and the volume of the diaphragm multiplied by the porosity of the diaphragm is the pores of the diaphragm.
[0056] (4) Calculate the interlayer gap V τ
[0057] Interlayer gap Vτ=La×Wa×Hτ; where La represents the length of the negative electrode sheet, Wa represents the width of the negative electrode sheet, and Hτ represents the interlayer gap, in cm. Since the width of the negative electrode sheet is greater than that of the positive electrode sheet, the interlayer gap is calculated based on the size of the negative electrode sheet.
[0058] The calculation formula of the interlayer gap Hτ is as follows:
[0059] Hτ=(Dd) / (2×n)-(Ha+Hc+2×Hs); where n represents the number of turns of the negative electrode sheet, D is the core diameter, d is the needle diameter, Ha represents the thickness of the negative electrode sheet, Hc represents the thickness of the positive electrode sheet, Hs represents the thickness of the separator, and the units of D, Ha, Hc, and Hs are consistent, all in cm.
[0060] It should be noted that the positive electrode sheet, the negative electrode sheet and the two separators form a unit. The sum of their thicknesses is the thickness of a unit. The size of a single turn is obtained by dividing the core diameter D by the number of turns n of the negative electrode sheet. The interlayer gap is obtained by subtracting the thickness of a unit from the size of a single turn.
[0061] (5) Calculate the gap V between the negative electrode and the positive electrode o
[0062] The gap in the area where the negative electrode exceeds the positive electrode (Overhang gap) Vo = (Wa-Wc) × Lc × (Hτ+Hc); where Wa represents the width of the negative electrode sheet dressing, Wc represents the width of the positive electrode sheet dressing, Lc represents the length of the positive electrode sheet, Hτ represents the layer gap, and Hc represents the thickness of the positive electrode sheet. The units of Wa, Wc, Lc, Hτ, and Hc are the same.
[0063] The value range of Wa-Wc is 0.5mm-5mm, that is, the width difference between the positive electrode sheet and the negative electrode sheet is 0.5mm-5mm, such as 0.5mm, 1.0mm, 2.0mm, 3.0mm, 4.0mm, 5.0mm, etc.
[0064] (6) Calculate the consumption rate of electrolyte during the formation process υ and the first coulombic efficiency η
[0065] The consumption rate of electrolyte during the formation process υ = (m1-m2) / (C1-C2), the first coulomb efficiency η = C2 / C1; where m1 is the mass of the electrolyte before formation, m2 is the mass of the electrolyte after formation, and the units of m1 and m2 are g; C1 is the first charging capacity after formation, C2 is the first discharge capacity after formation, and the units of C1 and C2 are mAh; the consumption rate of electrolyte during the formation process υ is g / mAh.
[0066] Since it is inconvenient to weigh the mass m2 of the electrolyte after formation, it can be calculated based on the mass fraction of the film-forming additive before and after formation. Specifically: take the electrolyte of the same design battery before and after formation, and measure the mass fraction of the film-forming additive before and after formation. The mass fraction of the film-forming additive before formation is marked as P1, and the mass fraction of the film-forming additive after formation is marked as P2. m2 is calculated according to the following formula:
[0067] m2=(P2 / P1)×m1.
[0068] Specifically, the film-forming additives are additives in conventional technologies, such as VC, FEC, DTD, MMDS, and the like.
[0069] S2. Calculate the injection volume
[0070] The amount of liquid injected at one time is calculated according to the pores of the positive electrode sheet, the pores of the negative electrode sheet, the pores of the diaphragm, the gaps between the layers, the gaps in the area where the negative electrode exceeds the positive electrode, and the consumption rate of the electrolyte during the formation process. The present invention takes into account the gaps between the layers and the gaps in the overhang, etc., and can accurately calculate the amount of liquid injected at one time. On the one hand, it can greatly reduce the extension of the injection time caused by excessive injection amount at one time, and on the other hand, it can avoid the problem of insufficient amount of electrode liquid required for formation due to insufficient injection amount at one time.
[0071] Furthermore, the calculation formula for the injection volume M1 is as follows:
[0072] M1=((V c +V a +V s +V τ +V o )×ρ)×k1+υ×(1-η)×C1;
[0073] Where V c Indicates the pores of the positive electrode sheet, in cm³;
[0074] V a Indicates the pores of the negative electrode sheet, in cm³;
[0075] V s Indicates the diaphragm pore size in cm³;
[0076] V τ Indicates the interlayer gap, in cm³;
[0077] V o Indicates the space between the negative electrode and the positive electrode, in cm³;
[0078] ρ represents the density of the electrolyte, in g / cm³;
[0079] k1 represents the coefficient, and its value ranges from 1.00 to 1.05, such as 1.00, 1.01, 1.02, 1.03, 1.04, 1.05, etc.;
[0080] υ represents the consumption rate of electrolyte during the formation process, in g / mAh;
[0081] η represents the first coulombic efficiency;
[0082] C1 represents the initial charge capacity after formation, in mAh.
[0083] According to the calculation results of S1, the positive electrode pore V c 、Negative electrode sheet pore V a 、Diaphragm pore V s , interlayer gap V τ 、The negative electrode exceeds the positive electrode area gap V o , the consumption rate of electrolyte during the formation process υ, the first coulomb efficiency η and other parameters are substituted into the calculation formula, and an appropriate k1 value is taken for calculation.
[0084] S3. Calculate the secondary injection volume
[0085] The secondary injection volume is calculated based on the electrolyte consumption rate during the formation process and the SOH requirement of the battery life. The electrolyte consumption rate during formation is introduced into the calculation of the secondary injection volume. The model uses the same mechanism of electrolyte consumption during formation and the electrolyte consumption mechanism during the later use of the battery to achieve precise control of the secondary injection volume and control of the battery life.
[0086] Furthermore, the secondary injection volume M2 = υ × k2 × (1-Sb) × C0;
[0087] Wherein, υ represents the consumption rate of electrolyte during the formation process, in g / mAh, which is calculated from S1;
[0088] k2 is a constant with a value of 1-1.5;
[0089] Sb is the battery life requirement, and its value ranges from 50% to 100%, which can be determined based on design requirements.
[0090] C0 is the rated capacity of the battery cell, in mAh.
[0091] The present invention provides a method for injecting liquid into a cylindrical battery, comprising: determining a primary injection volume and a secondary injection volume according to a method provided in an embodiment of the present invention, so as to achieve two precise injections and help to improve the life of the battery.
[0092] In some embodiments, the injection method includes: injecting a cylindrical battery cell with a primary injection amount, then forming, aging, and discharging, and then injecting a secondary injection amount. The battery after formation and aging is charged to 100% SOC, then discharged to 100% DOD, and the amount of electrolyte is injected into the battery according to the calculation result of the secondary injection amount, and the sealing nail is welded.
[0093] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0094] Example 1
[0095] This embodiment provides a method for determining the liquid filling amount of a cylindrical battery, comprising the following steps:
[0096] (1) The parameters of the electrode sheet, electrolyte, diaphragm, etc. used in this embodiment are as follows:
[0097] The electrolyte composition is as follows: (13% LiPF 6 , 30%EC, 20%EMC, 50%DMC, 2%VC, 1.5%DTD, 3%FEC), the film-forming additives are (VC, DTD, FEC), and the mass fraction of the film-forming additives is 6.5%.
[0098] Positive electrode sheet: The commercially available 46140 type positive electrode sheet, the active material is LFP, the current collector is an aluminum foil with a thickness of 13μm, the length of the positive electrode sheet Lc is 4236mm, the width of the positive electrode sheet Wc is 62mm, and the porosity σc of the positive electrode sheet is (32.27%). The positive electrode sheet was rolled for 48 hours and then placed in the electrolyte for sealing and soaking for 50 hours. The thickness of the electrode sheet after soaking was measured to be 171μm.
[0099] Negative electrode sheet: The commercially available 4680 model negative electrode sheet, the active material is graphite, the current collector is a copper foil with a thickness of 6μm, the length La of the negative electrode sheet is 4395mm, the width Wa of the negative electrode sheet is 66mm, and the porosity σa of the negative electrode sheet is 39.66%. The negative electrode sheet was rolled for 48 hours and then placed in the electrolyte for sealing and soaking for 50 hours. The thickness Ha of the electrode sheet after soaking was measured to be 141μm.
[0100] Diaphragm: The diaphragm thickness Hs is 14μm, the material is PP diaphragm, and the porosity σs of the diaphragm is 42%.
[0101] The positive electrode sheet, negative electrode sheet and separator are wound into a cylindrical battery. The number of windings of the negative electrode sheet is 54, the winding core diameter D is 43.3 cm, and the winding needle diameter d is 6 mm. The inner circle separator length Ls1 is 4679 mm, the outer circle separator length Ls2 is 4738 mm, and the separator width Ws is 70 mm.
[0102] The cylindrical battery was formed, and the mass m1 of the electrolyte before formation was tested to be 55g, the first charge capacity C1 after formation was 15620mAh, and the first discharge capacity C2 after formation was 14270mAh. The electrolyte of the same design battery before and after formation was taken, and the mass fraction of the film-forming additive before and after formation was measured. The mass fraction P1 of the film-forming additive before formation was 6.5%, and the mass fraction P2 of the film-forming additive after formation was 6.0%. The mass m2 of the electrolyte after formation was calculated according to the following formula:
[0103] m2=P2 / P1×m1=(6.0 / 6.5)×55=50.76923077.
[0104] (2) Calculate the positive electrode pore V c 、Negative electrode sheet pore V a 、Diaphragm pore Vs , interlayer gap V τ 、The negative electrode exceeds the positive electrode area gap V o And the consumption rate of electrolyte during the formation process υ, the specific calculation steps are as follows:
[0105] Pore V of positive electrode c =σc×Lc×Wc×Hc=32.27%×423.6×6.2×0.0171=14.49248023cm³;
[0106] Negative electrode pore Va = σa × La × Wa × Ha = 39.66% × 439.5 × 6.6 × 0.0141 = 16.22088844 cm³; diaphragm pore Vs =
[0107] σs×(Ls1+Ls2)×Ws×Hs=42%×(467.9+473.8)×7×0.0014=3.8760372cm³;
[0108] Interlayer gap Hτ = (Dd) / (2×n)-(Ha+Hc+2×Hs)=(4.33-0.6) / (2×54)-(0.0141+0.0171+2×0.0014)=5.37037037μm;
[0109] Interlayer gap Vτ=La×Wa×Hτ=439.5×6.6×5.37037037×10 -4 =1.557783333cm³;
[0110] The gap between the negative electrode and the positive electrode (overhang gap) Vo = (Wa-Wc) × Lc × (Hτ + Hc) = (6.6-6.2) × 423.6 × (5.37037037 + 171) × 10 -4 =2.988419556cm³;
[0111] The consumption rate of electrolyte during the formation process is υ = (m1-m2) / (C1-C2) = (55-50.76923077) / (15620-14270) = 0.0031 g / mAh;
[0112] The first coulombic efficiency η=C2 / C1=14270 / 15620=91.4%.
[0113] (3) Calculate the injection volume M1
[0114] The calculation formula of one injection volume M1 is as follows:
[0115] M1=((V c +V a +Vs +V τ +V o )×ρ)×k1+υ×(1-η)×C1, where ρ is 1.21 g / cm 3 , k1 value is 1.02, and the battery cell model is 4680.
[0116] M1=(14.49248023+16.22088844+3.8760372+1.557783333+2.988419556)×1.21×1.02+0.0031×(1-91.4%)×14270=52.53194g
[0117] (4) Calculate the secondary injection volume M2
[0118] Secondary injection volume M2 = υ × k2 × (1-Sb) × C0 = 0.0031 × 1.2 × (1-80%) × 14000 = 10.52991 g. Among them, k2 is 1.2, Sb is 80%, and C0 is 14000 mAh.
[0119] Example 2
[0120] This embodiment provides a method for determining the liquid filling amount of a cylindrical battery, comprising the following steps:
[0121] (1) The parameters of the electrode sheet, electrolyte, diaphragm, etc. used in this embodiment are as follows:
[0122] The electrolyte composition is as follows: (13% LiPF 6 , 30%EC, 20%EMC, 50%DMC, 2%VC, 1.5%DTD, 3%FEC), the film-forming additives are (VC, DTD, FEC), and the mass fraction of the film-forming additives is 6.5%.
[0123] Positive electrode sheet: The commercially available 46140 type positive electrode sheet, the active material is LFP, the current collector is an aluminum foil with a thickness of 13μm, the length of the positive electrode sheet Lc is 4236mm, the width of the positive electrode sheet Wc is 62mm, and the porosity σc of the positive electrode sheet is (32.27%). The positive electrode sheet was rolled for 48 hours and then placed in the electrolyte for sealing and soaking for 50 hours. The thickness of the electrode sheet after soaking was measured to be 171μm.
[0124] Negative electrode sheet: The commercially available 4680 model negative electrode sheet, the active material is graphite, the current collector is a copper foil with a thickness of 6μm, the length La of the negative electrode sheet is 4395mm, the width Wa of the negative electrode sheet is 66mm, and the porosity σa of the negative electrode sheet is 39.66%. The negative electrode sheet was rolled for 48 hours and then placed in the electrolyte for sealing and soaking for 50 hours. The thickness Ha of the electrode sheet after soaking was measured to be 141μm.
[0125] Diaphragm: The diaphragm thickness Hs is 14μm, the material is PP diaphragm, and the porosity σs of the diaphragm is 42%.
[0126] The positive electrode sheet, negative electrode sheet and separator are wound into a cylindrical battery. The number of windings of the negative electrode sheet is 54, the winding core diameter D is 43.3 cm, and the winding needle diameter d is 6 mm. The inner circle separator length Ls1 is 4679 mm, the outer circle separator length Ls2 is 4738 mm, and the separator width Ws is 70 mm.
[0127] The cylindrical battery was formed, and the mass m1 of the electrolyte before formation was tested to be 55g, the first charge capacity C1 after formation was 15620mAh, and the first discharge capacity C2 after formation was 14270mAh. The electrolyte of the same design battery before and after formation was taken, and the mass fraction of the film-forming additive before and after formation was measured. The mass fraction P1 of the film-forming additive before formation was 6.5%, and the mass fraction P2 of the film-forming additive after formation was 6.0%. The mass m2 of the electrolyte after formation was calculated according to the following formula:
[0128] m2=P2 / P1×m1=50.76923077.
[0129] (2) Calculate the positive electrode pore V c 、Negative electrode sheet pore V a 、Diaphragm pore V s , interlayer gap V τ 、The negative electrode exceeds the positive electrode area gap V o And the consumption rate of electrolyte during the formation process υ, the specific calculation steps are as follows:
[0130] Pore V of positive electrode c =σc×Lc×Wc×Hc=14.49248023cm³;
[0131] Negative electrode pore Va = σa × La × Wa × Ha = 16.22088844 cm³; diaphragm pore Vs =
[0132] σs×(Ls1+Ls2)×Ws×Hs=3.8760372cm³;
[0133] Interlayer gap Hτ = (Dd) / n-(Ha + Hc + 2 × Hs) = = 5.37037037 μm;
[0134] Interlayer gap Vτ=La×Wa×Hτ=1.557783333cm³;
[0135] The gap between the negative electrode and the positive electrode (overhang gap) Vo = (Wa-Wc) × Lc × (Hτ + Hc) = 2.988419556 cm³;
[0136] The consumption rate of electrolyte during the formation process is υ = (m1-m2) / (C1-C2) = 0.0031g / mAh;
[0137] The first coulombic efficiency η=C2 / C1=14270 / 15620=91.4%.
[0138] (3) Calculate the injection volume M1
[0139] The calculation formula of one injection volume M1 is as follows:
[0140] M1=((V c +V a +V s +V τ +V o )×ρ)×k1+υ×(1-η)×C1=51.58486g, where ρ is 1.21g / cm 3 , k1 value is 1, battery cell model is 4680.
[0141] (4) Calculate the secondary injection volume M2
[0142] Secondary injection volume M2 = υ × k2 × (1-Sb) × C0 = 10.52991 g. Among them, k2 is 1.2, Sb is 80%, and C0 is 14000 mAh.
[0143] Example 3
[0144] The only difference from Embodiment 1 is that k1=1, k2=1.
[0145] After calculation: M1=51.58486g, M2=8.774929.
[0146] Example 4
[0147] The only difference from Example 1 is that k1=1.05 and k2=1.
[0148] After calculation: M1=53.95256g, M2=8.774929.
[0149] Example 5
[0150] The only difference from Example 1 is that k1=1.05 and k2=1.5.
[0151] After calculation: M1=53.95256g, M2=13.16239.
[0152] Comparative Example 1
[0153] This comparative example provides a method for determining the liquid injection amount of a cylindrical battery, comprising the following steps:
[0154] (1) By calculating the rebound thickness of the pole piece after rolling (the pole piece is not immersed in electrolyte during this process), Hc=170μm, Ha=139.5μm, Vc, Va, Vs are calculated to calculate the injection volume once, Vc=14.40772889cm 3 ,Va=16.0483258cm 3 , Vs is consistent with that in Example 1, and other parameters such as Lc, Wc, La, Wa, etc. refer to those in Example 1.
[0155] (2) Calculation of injection volume: M1 = (V c +V a +V s )×ρ)×k1=((14.40772889+16.0483258+3.8760372)×1.21)×1.05=43.61892g;where ρ is 1.21g / cm 3 , k1 value is 1.05, and the battery cell model is 4680.
[0156] Secondary injection volume calculation: M2=M1×k3, k3 value is 0.05-0.15
[0157] When k3=0.1, M2=43.61892×0.1=4.361892
[0158] Comparative Example 2
[0159] This comparative example provides a method for determining the liquid injection amount of a cylindrical battery, comprising the following steps:
[0160] Calculated by injection coefficient, injection coefficient = C0 / (M1+M2);
[0161] k4=M1 / (M1+M2)=0.8-0.9;
[0162] The battery model in this comparative example is 4680, and the electrolyte density is 1.21g / cm 3 , k1=1.05, k4=0.85, C0=14000mAh, injection coefficient 4Ah / g;
[0163] M1+M2=4×14=56g
[0164] M1=47.6g, M2=8.40g
[0165] Test Example 1
[0166] The first injection volume M1 and the second injection volume M2 calculated according to Example 1 were used for injection, and then the electrochemical performance of the battery was tested. The results are shown in Table 1.
[0167] Injection method: inject the electrolyte into the cylindrical battery cell with a primary injection amount, then form, age and discharge, and then inject the electrolyte into the battery with a secondary injection amount for sealing nail welding.
[0168] Table 1 Performance test results of the battery after formation
[0169]
[0170] It can be seen from Table 1 that the method provided in the embodiment of the present invention is used to determine the primary injection amount and the secondary injection amount, which is beneficial to further improve the cycle stability of the battery compared with the method of the comparative example.
[0171] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for determining the liquid filling amount of a cylindrical battery, characterized in that: include: The amount of electrolyte injected once is calculated based on the pores of the positive electrode sheet, the pores of the negative electrode sheet, the pores of the diaphragm, the interlayer gaps, the gaps in the area where the negative electrode exceeds the positive electrode, and the consumption rate of the electrolyte during the formation process; The secondary injection volume is calculated based on the consumption rate of the electrolyte during the formation process and the battery life requirements; Among them, the calculation formula for one injection volume M1 is as follows: M1=((V c +V a +V s +V τ +V o )×ρ)×k1+υ×(1-η)×C1; Where V c Indicates the pores of the positive electrode sheet, in cm³; V a Indicates the pores of the negative electrode sheet, in cm³; V s Indicates the diaphragm pore size in cm³; V τ Indicates the interlayer gap, in cm³; V o Indicates the space between the negative electrode and the positive electrode, in cm³; ρ represents the density of the electrolyte, in g / cm³; k1 represents the coefficient, with a value of 1.00-1.05; υ represents the consumption rate of electrolyte during the formation process, in g / mAh; η represents the first coulombic efficiency; C1 represents the first charge capacity of the formation, in mAh; Secondary injection volume M2 = υ × k2 × (1-Sb) × C0; Wherein, υ represents the consumption rate of electrolyte during the formation process, and the unit is g / mAh; k2 is a constant with a value of 1-1.5; Sb is the battery life requirement, ranging from 50% to 100%; C0 is the rated capacity of the battery cell, in mAh.
2. The determination method according to claim 1, characterized in that: V c =σc×Lc×Wc×Hc; wherein, σc represents the porosity of the positive electrode sheet, Lc represents the length of the positive electrode sheet, Wc represents the width of the positive electrode sheet dressing, and Hc represents the thickness of the positive electrode sheet after being immersed in the electrolyte for 24h-72h.
3. The determination method according to claim 1, characterized in that: Va=σa×La×Wa×Ha; where σa represents the porosity of the negative electrode sheet, La represents the length of the negative electrode sheet, Wa represents the width of the negative electrode sheet dressing, and Ha represents the thickness of the negative electrode sheet after being immersed in the electrolyte for 24h-72h.
4. The determination method according to claim 1, characterized in that: Vs=σs×(Ls1+Ls2)×Ws×Hs; wherein, σs represents the porosity of the diaphragm, Ls1 represents the length of the inner diaphragm, Ls2 represents the length of the outer diaphragm, Ws represents the width of the diaphragm, and Hs represents the thickness of the diaphragm.
5. The determination method according to claim 1, characterized in that: Vτ=La×Wa×Hτ; where La represents the length of the negative electrode sheet, Wa represents the width of the negative electrode sheet, and Hτ represents the layer gap.
6. The determination method according to claim 5, characterized in that: The calculation formula of interlayer gap Hτ is as follows: Hτ=(Dd) / (2×n)-(Ha+Hc+2×Hs); where n represents the number of windings of the negative electrode sheet, D is the core diameter, d is the winding needle diameter, Ha represents the thickness of the negative electrode sheet, Hc represents the thickness of the positive electrode sheet, and Hs represents the thickness of the separator.
7. The determination method according to claim 1, characterized in that: Vo=(Wa-Wc)×Lc×(Hτ+Hc);Wa represents the width of the negative electrode sheet dressing, Wc represents the width of the positive electrode sheet dressing, Lc represents the length of the positive electrode sheet, Hτ represents the layer gap, and Hc represents the thickness of the positive electrode sheet; The value range of Wa-Wc is 0.5mm-5mm.
8. The determination method according to claim 1, characterized in that: The consumption rate of electrolyte during the formation process is υ=(m1-m2) / (C1-C2), and the first coulomb efficiency is η=C2 / C1; Among them, m1 is the mass of the electrolyte before formation, m2 is the mass of the electrolyte after formation, C1 is the first charge capacity after formation, and C2 is the first discharge capacity after formation; Take the electrolyte before and after formation of the same design battery cell, and measure the mass fraction of the film-forming additive before and after formation. The mass fraction of the film-forming additive before formation is marked as P1, and the mass fraction of the film-forming additive after formation is marked as P2. m2 is calculated according to the following formula: m2=(P2 / P1)×m1.
9. A method for injecting liquid into a cylindrical battery, characterized in that: include: The primary injection volume and the secondary injection volume are determined according to the determination method described in any one of claims 1 to 8.
10. The liquid injection method according to claim 9, characterized in that: The injection method comprises: injecting a cylindrical battery cell once with a primary injection volume, then forming, aging, discharging, and then injecting a second time with a secondary injection volume.
Citation Information
Patent Citations
Method for determining liquid injection amount of battery
CN116093558A
Method for determining liquid injection amount of battery and lithium ion battery
CN116937088A
Cited By
A cylindrical lithium-ion battery and a method of assembling the same
CN122800701A