Conductive glass for thin-film solar cells and its preparation method and application
Through the liquid two-phase vibration method and chemical vapor deposition nanosilver wire layer technology, combined with nanomaterials, the conductive performance and mechanical strength of conductive glass for thin film solar cells have been improved, and the problem of incompatibility between conductivity and optical transmittance has been solved. It is suitable for in environments with large temperature differences.
Patent Information
- Application Number
- CN202410896389.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Existing conductive glass for thin film solar cells has poor electrical conductivity and insufficient mechanical properties in environments with large temperature differences, making it difficult to balance electrical conductivity and optical transmittance.
The liquid two-phase vibration method is used to form wrinkles on the glass substrate, and the chemical vapor deposition nanosilver wire layer is combined with the silicon nitride and ITO layers to improve the electrical conductivity, and the mechanical properties of the glass substrate are enhanced through nanotitanium dioxide and nanoboron nitride.
Significantly improves the conductivity and mechanical strength of conductive glass, is suitable for use in outdoor environments of -20-30°C, and takes into account high light transmittance and low resistivity.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of conductive glass for thin-film solar cells, in particular to conductive glass for thin-film solar cells and a preparation method and application thereof. Background Art
[0002] As a new and efficient solar energy conversion technology, thin-film solar cells have shown great application potential in the field of solar cells due to their advantages such as light weight, flexibility, and easy integration. Conductive glass is an important component of thin-film solar cells, and its performance directly affects the overall performance of the cell. Therefore, the development of new high-performance conductive glass is of great significance to improving the performance of thin-film solar cells.
[0003] Traditional conductive glass for thin-film solar cells mainly includes a glass substrate and a transparent conductive film disposed on the glass substrate. The transparent conductive film is usually composed of a metal oxide conductive layer, such as ITO (tin-doped indium oxide), FTO (fluorine-doped tin oxide) and AZO (aluminum-doped zinc oxide). These materials have certain conductivity and optical transmittance, but also have many limitations.
[0004] Chinese patent application CN108218246A, published on June 29, 2018, discloses a method for preparing transparent conductive film glass, wherein polyvinyl pyrrolidone powder is dissolved in a complex stannous sulfate solution, and the low surface energy of polyvinyl pyrrolidone can make the metal ions in the transparent homogeneous sol have good stability, thereby improving the light transmittance of the transparent conductive film glass. Although the formula and preparation method of the glass have been adjusted to a certain extent, the conductivity is still not high.
[0005] In the prior art, conductive glass used in thin-film solar cells often has poor conductivity and is difficult to make compatible with optical transmittance. In addition, existing glass substrates have poor mechanical properties in environments with large temperature differences. Summary of the invention
[0006] In view of the above deficiencies in the prior art, the object of the present invention is to provide a conductive glass for thin-film solar cells, which has high strength, good toughness, excellent light transmittance and high conductivity.
[0007] Another object of the present invention is to provide a method for preparing conductive glass for thin-film solar cells, which adopts a liquid two-phase vibration method to form wrinkles at the interface of the two phases. Through the wrinkles, a nano silver wire layer is chemically vapor deposited, which greatly reduces the resistivity of the conductive film glass and greatly improves its performance.
[0008] The third object of the present invention is to provide an application of conductive glass for thin-film solar cells, which is applied to solar panels outdoors at a temperature of -20-30°C.
[0009] The present invention is achieved by adopting the following technical solutions:
[0010] The conductive glass for thin-film solar cells comprises a glass substrate and a conductive film layer. The glass substrate is composed of the following raw materials in parts by weight: SiO2: 54-58 parts; Al2O3: 6-10 parts; CaO: 8-12 parts; MgO: 3-5 parts; glass fiber reinforced plastic: 0.3-1.2 parts; nano titanium dioxide: 1-2 parts; nano boron nitride: 0.5-1 parts; Na2O: 8-12 parts;
[0011] The conductive film layer includes: a base film layer of 60-80nm, a metal mesh layer of 300-450nm, a functional layer of 1000-1200nm, and an anti-reflection layer of 120-150nm; the base film layer is a silicon nitride layer; the metal mesh layer is nano silver wire; the functional layer is an ITO layer; and the anti-reflection layer is a SiO2-TiO2 layer.
[0012] The method for preparing the glass substrate comprises the following steps:
[0013] (1) SiO2, Al2O3, nano titanium dioxide and nano boron nitride are stirred and mixed for 1-1.5 hours according to the weight ratio, and pre-sintered at 485-500°C for 1-1.5 hours to obtain a mixture A;
[0014] (2) Adding CaO, MgO, glass fiber reinforced plastic and Na2O to the mixture A obtained in step (1) according to the weight ratio, stirring for 1-2 hours to obtain a mixture B;
[0015] (3) Melting the mixture B at 1535-1550°C;
[0016] (4) After homogenization, forming, annealing and cooling, a glass substrate is obtained.
[0017] The method for preparing the conductive glass for thin-film solar cells comprises the following steps:
[0018] S1, preparing a silicon nitride mixed solution and an ethyl acetate solution, and then mixing them to obtain a two-phase mixed solution;
[0019] S2, placing the two-phase mixed liquid on a glass substrate and letting it stand for 0.5-1h;
[0020] S3, start the electromagnetic vibrator to vibrate and level the mixed liquid for 0.5-1h;
[0021] S4, heating the glass substrate to increase the temperature, drying the mixed liquid, and forming a closely connected silicon nitride layer and an ethyl acetate layer, wherein the ethyl acetate layer is located above the silicon nitride layer;
[0022] S5, performing plasma etching on the ethyl acetate layer;
[0023] S6, then chemically vapor depositing a nano silver wire layer on the silicon nitride surface;
[0024] S7, magnetron sputtering an ITO layer on the nano silver wire layer;
[0025] S8. Magnetron sputtering an anti-reflection layer on the ITO layer to obtain conductive glass for thin-film solar cells.
[0026] The silicon nitride mixed liquid is a mixed liquid of silicon nitride powder and water, and the solvent of the ethyl acetate solution is acetone.
[0027] The ethyl acetate is tetraglycidyl meta-xylene diamine. When preparing the ethyl acetate solution, a curing agent needs to be added. The curing agent is methyl hexahydrophthalic anhydride. The amount of the curing agent added is 35-40% of the mass of the ethyl acetate.
[0028] In the step S4, when drying the mixed solution, the temperature is first controlled at 76-80°C and maintained for 5-8 minutes; then the temperature is raised to 85-90°C and maintained for 10-15 minutes; and finally the temperature is raised to 105-108°C until a tightly connected silicon nitride layer and ethyl acetate layer are formed.
[0029] In the step S5, the etching gas for plasma etching is SF6, the gas flow rate is 35-60 sccm, the RF power is 250-350 watts, the etching chamber pressure is 5-8 mTorr, and the time is 30-90 seconds.
[0030] The step S51 is further included between the steps S5 and S6: washing the ethyl acetate layer;
[0031] The cleaning comprises the following steps:
[0032] a. The silicon nitride layer of the glass substrate obtained in step S5 is sprayed with a sodium hydroxide solution having a mass fraction of 30%-60%, and the solution temperature is controlled at 50C-70°C;
[0033] b. The silicon nitride layer treated in step a is sprayed with a hydrochloric acid solution having a concentration of 0.05-0.5 mol / L, and the hydrochloric acid residence time is 30-60 seconds;
[0034] c. Rinse the silicon nitride layer repeatedly with deionized water for 2-5 minutes.
[0035] In the step S6, the silver source in the chemical vapor deposition nano silver wire layer is one of disilver cyclopentadiene and monosilver cyclopentadiene.
[0036] The conductive glass for thin-film solar cells is applied to solar panels outdoors at a temperature of -20-30°C.
[0037] Glass fiber reinforced plastics can enhance mechanical properties and improve the strength and toughness of glass substrates. Nano boron nitride helps in the application of glass substrates in high temperature environments. Nano titanium dioxide and nano boron nitride can form a good interface bond between the glass phase and the reinforcing material in the glass substrate, which helps to improve the stability and performance of the overall structure. In addition, nano titanium dioxide and nano boron nitride can affect the thermal expansion coefficient of glass, thereby improving the dimensional stability of the substrate, especially in an environment with temperature changes. Moreover, through pre-sintering, the nanoparticles form a stable phase and structure, while preventing the particles from growing. Through the above adjustments, the mechanical properties of the glass substrate can be significantly improved.
[0038] The wrinkles produced at the interface of silicon nitride and ethyl acetate can increase the surface roughness, thereby providing more attachment points for nanosilver wires, increasing the contact area of nanosilver wires, and helping to improve the overall conductivity. By removing ethyl acetate through etching technology, the surface of silicon nitride can be exposed, providing a pure substrate for the next step of deposition of the nanosilver wire layer. Due to its high conductivity and flexibility, nanosilver wires can form a conductive network that covers the wrinkled silicon nitride surface, effectively improving the conductivity of the overall structure. The ITO layer coated on top of the nanosilver wire layer is a transparent conductive material with high visible light transmittance and low resistivity, which further enhances the conductivity of the conductive film. The high transmittance of the ITO layer helps to maintain the light transmittance of the glass.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] (1) The conductive glass for thin-film solar cells prepared in the present application has high strength and good toughness. It maintains high conductivity while having high light transmittance. In particular, when the visible light transmittance is 88.2% and the haze is 1.1%, the sheet resistance can still reach 5.42Ω / sq, thus solving the problem that the conductive glass for thin-film solar cells has poor conductivity and is difficult to be compatible with the optical transmittance.
[0041] (2) Through the compounding of nano-titanium dioxide and nano-boron nitride, as well as the interaction with other raw materials and the pre-sintering of the raw materials, the mechanical properties of the glass substrate are greatly improved, solving the problem of poor mechanical properties of the glass substrate in an environment with a large temperature difference. It is suitable for use in an environment with a large temperature difference outdoors.
[0042] (3) The liquid two-phase vibration method is used to form wrinkles at the interface between the two phases. A nano-silver wire layer is chemically vapor deposited on the wrinkles, which greatly reduces the resistivity of the conductive film glass and greatly improves its performance.
[0043] (4) It can be applied to solar panels outdoors at temperatures between -20 and 30°C. DETAILED DESCRIPTION
[0044] The present invention is further described below with reference to the embodiments, but they do not limit the implementation of the present invention.
[0045] Example 1
[0046] The glass substrate is composed of the following raw materials in parts by weight: SiO2: 56 parts; Al2O3: 8 parts; CaO: 10 parts; MgO: 4 parts; glass fiber reinforced plastic: 0.8 parts; nano titanium dioxide: 2 parts; nano boron nitride: 0.8 parts; and Na2O: 10 parts.
[0047] A method for preparing a glass substrate comprises the following steps:
[0048] (1) SiO2, Al2O3, nano-titanium dioxide and nano-boron nitride were stirred and mixed for 1.5 hours according to the weight ratio, and pre-sintered at 490°C for 1.5 hours to obtain a mixture A;
[0049] (2) Adding CaO, MgO, glass fiber reinforced plastic and Na2O to the mixture A obtained in step (1) according to the weight ratio, stirring for 2 hours to obtain a mixture B;
[0050] (3) Melting the mixture B at 1540°C;
[0051] (4) After homogenization, forming, annealing and cooling, a glass substrate is obtained.
[0052] The conductive film layer includes: a base film layer of 70nm, a metal mesh layer of 400nm, a functional layer of 1100nm, and an anti-reflection layer of 140nm; the base film layer is a silicon nitride layer; the metal mesh layer is nano silver wire; the functional layer is an ITO layer; and the anti-reflection layer is a SiO2-TiO2 layer.
[0053] A method for preparing conductive glass for thin-film solar cells comprises the following steps:
[0054] S1, preparing a mixed solution of silicon nitride powder and water, and an acetone solution of tetraglycidyl-m-xylene diamine, adding 38% by weight of methyl hexahydrophthalic anhydride to the tetraglycidyl-m-xylene diamine, and then mixing them to obtain a two-phase mixed solution;
[0055] S2, placing the two-phase mixed liquid on a glass substrate and leaving it to stand for 0.8h;
[0056] S3, start the electromagnetic vibrator to vibrate and level the mixed liquid for 0.8h;
[0057] S4, heating the glass substrate, first controlling the temperature at 77° C. and maintaining it for 6 minutes; then heating it to 88° C. and maintaining it for 12 minutes; finally heating it to 106° C. and drying the mixed liquid to form a closely connected silicon nitride layer and an ethyl acetate layer, wherein the ethyl acetate layer is located above the silicon nitride layer;
[0058] S5, performing plasma etching on the ethyl acetate layer, wherein the etching gas for the plasma etching is SF6, the gas flow rate is 45 sccm, the radio frequency power is 300 watts, the etching chamber pressure is 7 mTorr, and the time is 60 seconds;
[0059] S51, cleaning the ethyl acetate layer, comprising the following steps:
[0060] a. The silicon nitride layer of the glass substrate obtained in step S5 is sprayed with a 45% mass fraction of a sodium hydroxide solution, and the solution temperature is controlled at 60 ℃;
[0061] b The silicon nitride layer treated in step a was sprayed with a 0.3 mol / L hydrochloric acid solution, the hydrochloric acid residence time was 50 seconds;
[0062] c. Use deionized water to repeatedly rinse the silicon nitride layer for 3 minutes;
[0063] S6, then chemically vapor depositing a nano silver wire layer on the silicon nitride surface, wherein the silver source in the chemically vapor deposited nano silver wire layer is disilver cyclopentadiene;
[0064] S7, magnetron sputtering an ITO layer on the nano silver wire layer;
[0065] S8. Magnetron sputtering an anti-reflection layer on the ITO layer to obtain conductive glass for thin-film solar cells.
[0066] Example 2
[0067] The glass substrate is composed of the following raw materials in parts by weight: SiO2: 54 parts; Al2O3: 6 parts; CaO: 8 parts; MgO: 3 parts; glass fiber reinforced plastic: 0.3 parts; nano titanium dioxide: 1 part; nano boron nitride: 0.5 parts; and Na2O: 8 parts.
[0068] A method for preparing a glass substrate comprises the following steps:
[0069] (1) SiO2, Al2O3, nano-titanium dioxide and nano-boron nitride were stirred and mixed for 1 hour according to the weight ratio, and pre-sintered at 485°C for 1 hour to obtain a mixture A;
[0070] (2) Adding CaO, MgO, glass fiber reinforced plastic and Na2O to the mixture A obtained in step (1) according to the weight ratio, stirring for 1 hour to obtain a mixture B;
[0071] (3) Melting the mixture B at 1535°C;
[0072] (4) After homogenization, forming, annealing and cooling, a glass substrate is obtained.
[0073] The conductive film layer includes a base film layer of 60nm, a metal mesh layer of 300nm, a functional layer of 1000nm, and an anti-reflection layer of 120nm; the base film layer is a silicon nitride layer; the metal mesh layer is a nano silver wire; the functional layer is an ITO layer; and the anti-reflection layer is a SiO2-TiO2 layer.
[0074] A method for preparing conductive glass for thin-film solar cells comprises the following steps:
[0075] S1, preparing a mixed solution of silicon nitride and water, and an acetone solution of tetraglycidyl-m-xylene diamine, adding 35% by weight of methyl hexahydrophthalic anhydride to the tetraglycidyl-m-xylene diamine, and then mixing them to obtain a two-phase mixed solution;
[0076] S2, placing the two-phase mixed liquid on a glass substrate and letting it stand for 0.5h;
[0077] S3, start the electromagnetic vibrator to vibrate and level the mixed liquid for 0.5h;
[0078] S4, heating the glass substrate, first controlling the temperature at 76° C. and maintaining it for 5 minutes; then heating it to 85° C. and maintaining it for 10 minutes; finally heating it to 105° C. and drying the mixed liquid to form a closely connected silicon nitride layer and an ethyl acetate layer, wherein the ethyl acetate layer is located above the silicon nitride layer;
[0079] S5, performing plasma etching on the ethyl acetate layer, wherein the etching gas for the plasma etching is SF6, the gas flow rate is 35 sccm, the radio frequency power is 250 watts, the etching chamber pressure is 5 mTorr, and the time is 30 seconds;
[0080] S51, cleaning the ethyl acetate layer, comprising the following steps:
[0081] a. The silicon nitride layer of the glass substrate obtained in step S5 is sprayed with a 30% mass fraction of a sodium hydroxide solution, and the solution temperature is controlled at 50 ℃;
[0082] b. The silicon nitride layer treated in step a was sprayed with a 0.05 mol / L hydrochloric acid solution, the hydrochloric acid residence time was 30 seconds;
[0083] c. Use deionized water to repeatedly rinse the silicon nitride layer for 2 minutes;
[0084] S6, then chemically vapor depositing a nano silver wire layer on the silicon nitride surface, wherein the silver source in the chemically vapor deposited nano silver wire layer is monosilver cyclopentadiene;
[0085] S7, magnetron sputtering an ITO layer on the nano silver wire layer;
[0086] S8. Magnetron sputtering an anti-reflection layer on the ITO layer to obtain conductive glass for thin-film solar cells.
[0087] Example 3
[0088] The glass substrate is composed of the following raw materials in parts by weight: SiO2: 58 parts; Al2O3: 10 parts; CaO: 12 parts; MgO: 5 parts; glass fiber reinforced plastic: 1.2 parts; nano titanium dioxide: 2 parts; nano boron nitride: 1 part; and Na2O: 12 parts.
[0089] A method for preparing a glass substrate comprises the following steps:
[0090] (1) SiO2, Al2O3, nano-titanium dioxide and nano-boron nitride were stirred and mixed for 1.5 hours according to the weight ratio, and pre-sintered at 500°C for 1.5 hours to obtain a mixture A;
[0091] (2) Adding CaO, MgO, glass fiber reinforced plastic and Na2O to the mixture A obtained in step (1) according to the weight ratio, stirring for 2 hours to obtain a mixture B;
[0092] (3) Melting the mixture B at 1550°C;
[0093] (4) After homogenization, forming, annealing and cooling, a glass substrate is obtained.
[0094] The conductive film layer includes a base film layer of 80nm, a metal mesh layer of 450nm, a functional layer of 1200nm, and an anti-reflection layer of 150nm; the base film layer is a silicon nitride layer; the metal mesh layer is a nano silver wire; the functional layer is an ITO layer; and the anti-reflection layer is a SiO2-TiO2 layer.
[0095] A method for preparing conductive glass for thin-film solar cells comprises the following steps:
[0096] S1, preparing a mixed solution of silicon nitride and water, and an acetone solution of tetraglycidyl-m-xylene diamine, adding 40% by weight of methylhexahydrophthalic anhydride to the tetraglycidyl-m-xylene diamine, and then mixing them to obtain a two-phase mixed solution;
[0097] S2, placing the two-phase mixed liquid on a glass substrate and letting it stand for 1 hour;
[0098] S3, start the electromagnetic vibrator to vibrate and level the mixed liquid for 1 hour;
[0099] S4, heating the glass substrate, first controlling the temperature at 80° C. and maintaining it for 8 minutes; then heating it to 90° C. and maintaining it for 15 minutes; finally heating it to 108° C. and drying the mixed liquid to form a closely connected silicon nitride layer and an ethyl acetate layer, wherein the ethyl acetate layer is located above the silicon nitride layer;
[0100] S5, performing plasma etching on the ethyl acetate layer, wherein the etching gas for the plasma etching is SF6, the gas flow rate is 60 sccm, the radio frequency power is 350 watts, the etching chamber pressure is 8 mTorr, and the time is 90 seconds;
[0101] S51, cleaning the ethyl acetate layer, comprising the following steps:
[0102] a. The silicon nitride layer of the glass substrate obtained in step S5 is sprayed with a 60% mass fraction of a sodium hydroxide solution, and the solution temperature is controlled at 70 ℃;
[0103] b The silicon nitride layer treated in step a was sprayed with a 0.5 mol / L hydrochloric acid solution, the hydrochloric acid residence time was 60 seconds;
[0104] c. Use deionized water to repeatedly rinse the silicon nitride layer for 5 minutes;
[0105] S6, then chemically vapor depositing a nano silver wire layer on the silicon nitride surface, wherein the silver source in the chemically vapor deposited nano silver wire layer is disilver cyclopentadiene;
[0106] S7, magnetron sputtering an ITO layer on the nano silver wire layer;
[0107] S8. Magnetron sputtering an anti-reflection layer on the ITO layer to obtain conductive glass for thin-film solar cells.
[0108] Example 4
[0109] The glass substrate is composed of the following raw materials in parts by weight: SiO2: 56 parts; Al2O3: 8 parts; CaO: 10 parts; MgO: 4 parts; glass fiber reinforced plastic: 0.8 parts; nano titanium dioxide: 2 parts; nano boron nitride: 0.8 parts; and Na2O: 10 parts.
[0110] A method for preparing a glass substrate comprises the following steps:
[0111] (1) SiO2, Al2O3, nano-titanium dioxide and nano-boron nitride were stirred and mixed for 1.5 hours according to the weight ratio, and pre-sintered at 490°C for 1.5 hours to obtain a mixture A;
[0112] (2) Adding CaO, MgO, glass fiber reinforced plastic and Na2O to the mixture A obtained in step (1) according to the weight ratio, stirring for 2 hours to obtain a mixture B;
[0113] (3) Melting the mixture B at 1540°C;
[0114] (4) After homogenization, forming, annealing and cooling, a glass substrate is obtained.
[0115] The conductive film layer includes a base film layer of 60nm, a metal mesh layer of 300nm, a functional layer of 1000nm, and an anti-reflection layer of 120nm; the base film layer is a silicon nitride layer; the metal mesh layer is a nano silver wire; the functional layer is an ITO layer; and the anti-reflection layer is a SiO2-TiO2 layer.
[0116] A method for preparing conductive glass for thin-film solar cells comprises the following steps:
[0117] S1, preparing a mixed solution of silicon nitride and water, and an acetone solution of tetraglycidyl-m-xylene diamine, adding 40% by weight of methylhexahydrophthalic anhydride to the tetraglycidyl-m-xylene diamine, and then mixing them to obtain a two-phase mixed solution;
[0118] S2, placing the two-phase mixed liquid on a glass substrate and letting it stand for 1 hour;
[0119] S3, start the electromagnetic vibrator to vibrate and level the mixed liquid for 1 hour;
[0120] S4, heating the glass substrate, first controlling the temperature at 77° C. and maintaining it for 6 minutes; then heating it to 88° C. and maintaining it for 15 minutes; finally heating it to 108° C. and drying the mixed liquid to form a closely connected silicon nitride layer and an ethyl acetate layer, wherein the ethyl acetate layer is located above the silicon nitride layer;
[0121] S5, performing plasma etching on the ethyl acetate layer, wherein the etching gas for the plasma etching is SF6, the gas flow rate is 60 sccm, the radio frequency power is 350 watts, the etching chamber pressure is 8 mTorr, and the time is 90 seconds;
[0122] S51, cleaning the ethyl acetate layer, comprising the following steps:
[0123] a. The silicon nitride layer of the glass substrate obtained in step S5 is sprayed with a 60% mass fraction of a sodium hydroxide solution, and the solution temperature is controlled at 70 ℃;
[0124] b The silicon nitride layer treated in step a was sprayed with a 0.5 mol / L hydrochloric acid solution, the hydrochloric acid residence time was 60 seconds;
[0125] c. Use deionized water to repeatedly rinse the silicon nitride layer for 5 minutes;
[0126] S6, then chemically vapor depositing a nano silver wire layer on the silicon nitride surface, wherein the silver source in the chemically vapor deposited nano silver wire layer is disilver cyclopentadiene;
[0127] S7, magnetron sputtering an ITO layer on the nano silver wire layer;
[0128] S8. Magnetron sputtering an anti-reflection layer on the ITO layer to obtain conductive glass for thin-film solar cells.
[0129] Example 5
[0130] The glass substrate is composed of the following raw materials in parts by weight: SiO2: 54 parts; Al2O3: 6 parts; CaO: 8 parts; MgO: 3 parts; glass fiber reinforced plastic: 0.3 parts; nano titanium dioxide: 1 part; nano boron nitride: 0.5 parts; and Na2O: 8 parts.
[0131] A method for preparing a glass substrate comprises the following steps:
[0132] (1) SiO2, Al2O3, nano-titanium dioxide and nano-boron nitride were stirred and mixed for 1.5 hours according to the weight ratio, and pre-sintered at 500°C for 1.5 hours to obtain a mixture A;
[0133] (2) Adding CaO, MgO, glass fiber reinforced plastic and Na2O to the mixture A obtained in step (1) according to the weight ratio, stirring for 2 hours to obtain a mixture B;
[0134] (3) Melting the mixture B at 1550°C;
[0135] (4) After homogenization, forming, annealing and cooling, a glass substrate is obtained.
[0136] The conductive film layer includes a base film layer of 80nm, a metal mesh layer of 450nm, a functional layer of 1200nm, and an anti-reflection layer of 150nm; the base film layer is a silicon nitride layer; the metal mesh layer is a nano silver wire; the functional layer is an ITO layer; and the anti-reflection layer is a SiO2-TiO2 layer.
[0137] A method for preparing conductive glass for thin-film solar cells comprises the following steps:
[0138] S1, preparing a mixed solution of silicon nitride and water, and an acetone solution of tetraglycidyl-m-xylene diamine, adding 38% by weight of methylhexahydrophthalic anhydride to the tetraglycidyl-m-xylene diamine, and then mixing them to obtain a two-phase mixed solution;
[0139] S2, placing the two-phase mixed liquid on a glass substrate and leaving it to stand for 0.8h;
[0140] S3, start the electromagnetic vibrator to vibrate and level the mixed liquid for 0.8h;
[0141] S4, heating the glass substrate, first controlling the temperature at 76° C. and maintaining it for 5 minutes; then heating it to 85° C. and maintaining it for 12 minutes; finally heating it to 106° C. and drying the mixed liquid to form a closely connected silicon nitride layer and an ethyl acetate layer, wherein the ethyl acetate layer is located above the silicon nitride layer;
[0142] S5, performing plasma etching on the ethyl acetate layer, wherein the etching gas for the plasma etching is SF6, the gas flow rate is 45 sccm, the radio frequency power is 300 watts, the etching chamber pressure is 7 mTorr, and the time is 60 seconds;
[0143] S51, cleaning the ethyl acetate layer, comprising the following steps:
[0144] a. The silicon nitride layer of the glass substrate obtained in step S5 is sprayed with a 45% mass fraction of a sodium hydroxide solution, and the solution temperature is controlled at 60 ℃;
[0145] b The silicon nitride layer treated in step a was sprayed with a 0.3 mol / L hydrochloric acid solution, the hydrochloric acid residence time was 50 seconds;
[0146] c. Use deionized water to repeatedly rinse the silicon nitride layer for 3 minutes;
[0147] S6, then chemically vapor depositing a nano silver wire layer on the silicon nitride surface, wherein the silver source in the chemically vapor deposited nano silver wire layer is disilver cyclopentadiene;
[0148] S7, magnetron sputtering an ITO layer on the nano silver wire layer;
[0149] S8. Magnetron sputtering an anti-reflection layer on the ITO layer to obtain conductive glass for thin-film solar cells.
[0150] Comparative Example 1
[0151] The glass substrate is composed of the following raw materials in parts by weight: SiO2: 56 parts; Al2O3: 8 parts; CaO: 10 parts; MgO: 4 parts; and Na2O: 10 parts.
[0152] A method for preparing a glass substrate comprises the following steps:
[0153] (1) SiO2, Al2O3, CaO, MgO and Na2O are stirred for 2 hours according to the weight ratio to obtain a mixture;
[0154] (2) Melting the mixture at 1540°C;
[0155] (3) After homogenization, forming, annealing and cooling, a glass substrate is obtained.
[0156] The conductive film layer includes: a base film layer of 70nm, a metal mesh layer of 400nm, a functional layer of 1100nm, and an anti-reflection layer of 140nm; the base film layer is a silicon nitride layer; the metal mesh layer is nano silver wire; the functional layer is an ITO layer; and the anti-reflection layer is a SiO2-TiO2 layer.
[0157] A method for preparing conductive glass for thin-film solar cells comprises the following steps:
[0158] S1, preparing a mixed solution of silicon nitride and water, and an acetone solution of tetraglycidyl-m-xylene diamine, adding 38% by weight of methylhexahydrophthalic anhydride to the tetraglycidyl-m-xylene diamine, and then mixing them to obtain a two-phase mixed solution;
[0159] S2, placing the two-phase mixed liquid on a glass substrate and leaving it to stand for 0.8h;
[0160] S3, start the electromagnetic vibrator to vibrate and level the mixed liquid for 0.8h;
[0161] S4, heating the glass substrate, first controlling the temperature at 77° C. and maintaining it for 6 minutes; then heating it to 88° C. and maintaining it for 12 minutes; finally heating it to 106° C. and drying the mixed liquid to form a closely connected silicon nitride layer and an ethyl acetate layer, wherein the ethyl acetate layer is located above the silicon nitride layer;
[0162] S5, performing plasma etching on the ethyl acetate layer, wherein the etching gas for the plasma etching is SF6, the gas flow rate is 45 sccm, the radio frequency power is 300 watts, the etching chamber pressure is 7 mTorr, and the time is 60 seconds;
[0163] S51, cleaning the ethyl acetate layer, comprising the following steps:
[0164] a. The silicon nitride layer of the glass substrate obtained in step S5 is sprayed with a 45% mass fraction of a sodium hydroxide solution, and the solution temperature is controlled at 60 ℃;
[0165] b The silicon nitride layer treated in step a was sprayed with a 0.3 mol / L hydrochloric acid solution, the hydrochloric acid residence time was 50 seconds;
[0166] c. Use deionized water to repeatedly rinse the silicon nitride layer for 3 minutes;
[0167] S6, then chemically vapor depositing a nano silver wire layer on the silicon nitride surface, wherein the silver source in the chemically vapor deposited nano silver wire layer is disilver cyclopentadiene;
[0168] S7, magnetron sputtering an ITO layer on the nano silver wire layer;
[0169] S8. Magnetron sputtering an anti-reflection layer on the ITO layer to obtain conductive glass for thin-film solar cells.
[0170] Comparative Example 2
[0171] The glass substrate is composed of the following raw materials in parts by weight: SiO2: 56 parts; Al2O3: 8 parts; CaO: 10 parts; MgO: 4 parts; glass fiber reinforced plastic: 0.8 parts; nano titanium dioxide: 2 parts; nano boron nitride: 0.8 parts; and Na2O: 10 parts.
[0172] A method for preparing a glass substrate comprises the following steps:
[0173] (1) SiO2, Al2O3, nano-titanium dioxide and nano-boron nitride were stirred and mixed for 1.5 hours according to the weight ratio, and pre-sintered at 490°C for 1.5 hours to obtain a mixture A;
[0174] (2) Adding CaO, MgO, glass fiber reinforced plastic and Na2O to the mixture A obtained in step (1) according to the weight ratio, stirring for 2 hours to obtain a mixture B;
[0175] (3) Melting the mixture B at 1540°C;
[0176] (4) After homogenization, forming, annealing and cooling, a glass substrate is obtained.
[0177] The conductive film layer includes: a base film layer of 70nm, a metal mesh layer of 400nm, a functional layer of 1100nm, and an anti-reflection layer of 140nm; the base film layer is a silicon nitride layer; the metal mesh layer is nano silver wire; the functional layer is an ITO layer; and the anti-reflection layer is a SiO2-TiO2 layer.
[0178] A method for preparing conductive glass for thin-film solar cells comprises the following steps:
[0179] S1, coating a silicon nitride layer on a glass substrate;
[0180] S2, printing a metal mesh wire on the silicon nitride layer;
[0181] S4, magnetron sputtering an ITO layer on the metal mesh layer;
[0182] S5. Magnetron sputtering an anti-reflection layer on the ITO layer to obtain conductive glass for thin-film solar cells.
[0183] Comparative Example 3
[0184] The glass substrate is composed of the following raw materials in parts by weight: SiO2: 56 parts; Al2O3: 8 parts; CaO: 10 parts; MgO: 4 parts; glass fiber reinforced plastic: 0.8 parts; nano titanium dioxide: 2 parts; nano boron nitride: 0.8 parts; and Na2O: 10 parts.
[0185] A method for preparing a glass substrate comprises the following steps:
[0186] (1) SiO2, Al2O3, nano-titanium dioxide and nano-boron nitride were stirred and mixed for 1.5 hours according to the weight ratio, and pre-sintered at 490°C for 1.5 hours to obtain a mixture A;
[0187] (2) Adding CaO, MgO, glass fiber reinforced plastic and Na2O to the mixture A obtained in step (1) according to the weight ratio, stirring for 2 hours to obtain a mixture B;
[0188] (3) Melting the mixture B at 1540°C;
[0189] (4) After homogenization, forming, annealing and cooling, a glass substrate is obtained.
[0190] The conductive film layer includes: a base film layer of 70nm, a metal mesh layer of 400nm, a functional layer of 1100nm, and an anti-reflection layer of 140nm; the base film layer is a silicon nitride layer; the metal mesh layer is a copper mesh; the functional layer is an ITO layer; and the anti-reflection layer is a SiO2-TiO2 layer.
[0191] A method for preparing conductive glass for thin-film solar cells comprises the following steps:
[0192] S1, preparing a mixed solution of silicon nitride and water, and an acetone solution of tetraglycidyl-m-xylene diamine, adding 38% by weight of methylhexahydrophthalic anhydride to the tetraglycidyl-m-xylene diamine, and then mixing them to obtain a two-phase mixed solution;
[0193] S2, placing the two-phase mixed liquid on a glass substrate and leaving it to stand for 0.8h;
[0194] S3, start the electromagnetic vibrator to vibrate and level the mixed liquid for 0.8h;
[0195] S4, heating the glass substrate, first controlling the temperature at 77° C. and maintaining it for 6 minutes; then heating it to 88° C. and maintaining it for 12 minutes; finally heating it to 106° C. and drying the mixed liquid to form a closely connected silicon nitride layer and an ethyl acetate layer, wherein the ethyl acetate layer is located above the silicon nitride layer;
[0196] S5, performing plasma etching on the ethyl acetate layer, wherein the etching gas for the plasma etching is SF6, the gas flow rate is 45 sccm, the radio frequency power is 300 watts, the etching chamber pressure is 7 mTorr, and the time is 60 seconds;
[0197] S51, cleaning the ethyl acetate layer, comprising the following steps:
[0198] a. The silicon nitride layer of the glass substrate obtained in step S5 is sprayed with a 45% mass fraction of a sodium hydroxide solution, and the solution temperature is controlled at 60 ℃;
[0199] b The silicon nitride layer treated in step a was sprayed with a 0.3 mol / L hydrochloric acid solution, the hydrochloric acid residence time was 50 seconds;
[0200] c. Use deionized water to repeatedly rinse the silicon nitride layer for 3 minutes;
[0201] S6, then printing a copper mesh layer on the silicon nitride surface;
[0202] S7, magnetron sputtering an ITO layer on the copper mesh layer;
[0203] S8. Magnetron sputtering an anti-reflection layer on the ITO layer to obtain conductive glass for thin-film solar cells.
[0204] The test data of Examples 1-5 and Comparative Examples 1-3 are shown in Table 1.
[0205] Table 1 Test data of Examples 1-5 and Comparative Examples 1-3
[0206]
[0207] Note: Young's modulus reflects the test data of glass substrate.
[0208] By comparing Example 1 with Comparative Example 1, it can be seen that the mechanical strength of the glass substrate of Example 1 is significantly improved when the formula and preparation method of the glass substrate are adjusted; by comparing Comparative Example 2 with Example 1, it can be seen that the preparation method of the metal mesh layer is more critical; by comparing Comparative Example 3 with Example 1, it can be seen that the selection of raw materials for the metal mesh layer is crucial. In summary, the present invention adopts a liquid two-phase vibration method to form wrinkles at the interface of the two phases, and a nano silver wire layer is chemically vapor deposited on the wrinkles, which greatly reduces the resistivity of the conductive film glass and greatly improves its performance.
[0209] The high temperature (80°C, 120 hours) and low temperature (-20°C, 120 hours) thermal stability test results of Example 1 and Comparative Examples 2-3 are shown in Table 2.
[0210] Table 2 Thermal stability test results of Example 1 and Comparative Examples 2-3 at high temperature (80°C, 120 hours) and low temperature (-20°C, 120 hours)
[0211]
[0212] Note: The thermal stability index is (R-R0) / R, where R0 is the initial resistance value and R is the resistance value after the test; Test: GB / T 30984.2-2014 "Solar Glass Part 2: Transparent Conductive Oxide Film Glass".
[0213] It can be seen from the above data that the conductive glass for thin-film solar cells prepared by the present invention can be applied to solar panels outdoors at a temperature of -20-30°C and has good thermal stability.
Claims
1. A conductive glass for thin-film solar cells, characterized in that: It comprises a glass substrate and a conductive film layer, wherein the glass substrate is composed of the following raw materials in parts by weight: SiO2: 54-58 parts; Al2O3: 6-10 parts; CaO: 8-12 parts; MgO: 3-5 parts; glass fiber reinforced plastic: 0.3-1.2 parts; nano titanium dioxide: 1-2 parts; nano boron nitride: 0.5-1 parts; Na2O: 8-12 parts; The conductive film layer includes: a base film layer of 60-80nm, a metal mesh layer of 300-450nm, a functional layer of 1000-1200nm, and an anti-reflection layer of 120-150nm; the base film layer is a silicon nitride layer; the metal mesh layer is a nano silver wire; the functional layer is an ITO layer; and the anti-reflection layer is a SiO2-TiO2 layer; The method for preparing the glass substrate comprises the following steps: (1) SiO2, Al2O3, nano titanium dioxide and nano boron nitride are stirred and mixed for 1-1.5 hours according to the weight ratio, and pre-sintered at 485-500°C for 1-1.5 hours to obtain a mixture A; (2) Adding CaO, MgO, glass fiber reinforced plastic and Na2O to the mixture A obtained in step (1) according to the weight ratio, stirring for 1-2 hours to obtain a mixture B; (3) Melting the mixture B at 1535-1550°C; (4) After homogenization, forming, annealing and cooling, a glass substrate is obtained; The method for preparing the conductive glass for thin-film solar cells comprises the following steps: S1, preparing a silicon nitride mixed solution and an ethyl acetate solution, and then mixing them to obtain a two-phase mixed solution; S2, placing the two-phase mixed liquid on a glass substrate and letting it stand for 0.5-1h; S3, start the electromagnetic vibrator to vibrate and level the mixed liquid for 0.5-1h; S4, heating the glass substrate to increase the temperature, drying the mixed liquid, and forming a closely connected silicon nitride layer and an ethyl acetate layer, wherein the ethyl acetate layer is located above the silicon nitride layer; S5, performing plasma etching on the ethyl acetate layer; S6, then chemically vapor depositing a nano silver wire layer on the silicon nitride surface; S7, magnetron sputtering an ITO layer on the nano silver wire layer; S8, magnetron sputtering an anti-reflection layer on the ITO layer to obtain a conductive glass for thin-film solar cells; In the step S4, when drying the mixed solution, the temperature is first controlled at 76-80°C and maintained for 5-8 minutes; then the temperature is raised to 85-90°C and maintained for 10-15 minutes; and finally the temperature is raised to 105-108°C until a closely connected silicon nitride layer and ethyl acetate layer are formed; In the step S6, the silver source in the chemical vapor deposition nano silver wire layer is one of disilver cyclopentadiene and monosilver cyclopentadiene; The conductive glass for thin-film solar cells is applied to solar panels outdoors at a temperature of -20-30°C.
2. The conductive glass for thin-film solar cells according to claim 1, characterized in that: The silicon nitride mixed liquid is a mixed liquid of silicon nitride powder and water, and the solvent of the ethyl acetate solution is acetone.
3. The conductive glass for thin-film solar cells according to claim 1, characterized in that: The ethyl acetate is tetraglycidyl meta-xylene diamine. When preparing the ethyl acetate solution, a curing agent needs to be added. The curing agent is methyl hexahydrophthalic anhydride. The amount of the curing agent added is 35-40% of the mass of the ethyl acetate.
4. The conductive glass for thin-film solar cells according to claim 1, characterized in that: In the step S5, the etching gas for plasma etching is SF6, the gas flow rate is 35-60 sccm, the RF power is 250-350 watts, the etching chamber pressure is 5-8 mTorr, and the time is 30-90 seconds.
5. The conductive glass for thin-film solar cells according to claim 1, characterized in that: The step S51 is further included between the steps S5 and S6: washing the ethyl acetate layer; The cleaning comprises the following steps: a. The silicon nitride layer of the glass substrate obtained in step S5 is sprayed with a sodium hydroxide solution having a mass fraction of 30%-60%, and the solution temperature is controlled at 50-70 ℃; b. The silicon nitride layer treated in step a is sprayed with a concentration of 0.05-0.5mol / L of hydrochloric acid solution, the hydrochloric acid residence time is 30-60 seconds; c. Rinse the silicon nitride layer repeatedly with deionized water for 2-5 minutes.
Citation Information
Patent Citations
Preparation method of transparent conducting film glass
CN108218246A
Conductive glass for thin film solar battery and preparation method thereof
CN102683436A
Method for preparing AZO film texture structure used for film solar cell
CN103266302A
Low resistance transparent conductive film and preparation method
CN105225728A
Glass substrate of CIGS (copper-indium-gallium-selenide) thin-film solar cell
CN105837032A