Infrared nonlinear optical crystal and its preparation method and application
Through the design and preparation of chiral hybrid antimony (Ⅲ) halide infrared nonlinear optical crystals, the problems of pollution and insufficient performance of existing materials have been solved, and high-performance, low-cost, and environmentally friendly nonlinear optical materials have been achieved. SHG response and application prospects.
Patent Information
- Application Number
- CN202410891095.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing nonlinear optical crystal materials have pollution effects in their applications, and it is difficult to design high-performance non-centrosymmetric materials, which cannot effectively meet the needs of green environmental protection and high performance.
Chiral hybrid antimony (Ⅲ) halide infrared nonlinear optical crystal is used, and R-(+)-α-methylbenzylamine or S-(-)-α-methylbenzylamine is introduced as the organic amine ligand. The inorganic framework is induced to produce an intrinsic non-centrosymmetric structure to form C32H48Br10N4Sb2 crystal, and the nanosheets are prepared using a monoclinic crystal structure and a specific preparation method.
It achieves efficient second-order nonlinear optical phenomena, significantly improves the SHG response signal, is low-cost, environmentally friendly, and is suitable for fields such as laser frequency doubling and polarized light detection.
Smart Images

Figure CN118422348B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical crystal materials, and in particular relates to infrared nonlinear optical crystals and a preparation method and application thereof. Background Art
[0002] Nonlinear optical crystals are crystals that show secondary or higher nonlinear optical effects for strong laser electric fields. Nonlinear optical effects originate from the interaction between light and medium. When strong field laser propagates in the medium, nonlinear optical effects will occur, such as linear photoelectric effect, optical rectification effect, sum frequency, difference frequency, high harmonics, etc. Among them, second harmonic generation (SHG) refers to the process in which two photons with a frequency of ω annihilate and generate a new photon with a frequency of 2ω. It can be used to double the laser frequency, expand the tunable range of the laser, modulate the intensity and phase of the laser, realize holographic storage of laser signals, eliminate self-pumping phase conjugation of wavefront domain change, etc. Nonlinear optical crystals play an increasingly important role in laser frequency conversion, microscopic imaging, micro-nano processing, and terahertz waves (THz).
[0003] In recent years, organic-inorganic hybrid metal halides have been widely used in photovoltaic devices, light-emitting diodes, photodetectors, lasers, and nonlinear optics due to their excellent optoelectronic properties. Second harmonic generation (SHG) is the most widely used second-order nonlinear optical phenomenon, which requires the material to have strict non-centrosymmetry, so its material design and preparation is a challenge. Chiral materials have intrinsic non-centrosymmetry. By introducing chiral structures into hybrid metal halides, SHG response has been achieved in metal halide materials such as lead (II), tin (II), and cadmium (II). However, lead-based, tin-based, and cadmium-based materials have inevitable pollution effects, which violates the current green environmental protection orientation. Therefore, developing more green matrices, solving pollution problems, and designing more high-performance hybrid halide materials for nonlinear optics have become one of the major challenges currently faced. Summary of the invention
[0004] The purpose of the present invention is to provide an infrared nonlinear optical crystal and a preparation method and application thereof to address the deficiencies in the prior art. The crystal has an intrinsic non-centrosymmetric structure, can exhibit obvious second-order nonlinear optical phenomena, and produce a higher SHG response.
[0005] To achieve the above object, the present invention adopts the following technical solution:
[0006] The first object of the present invention is to provide an infrared nonlinear optical crystal, wherein the molecular formula of the infrared nonlinear crystal is C 32 H 48 Br 10N4Sb2, whose unit cell parameters are a=28.5206(15) Å, b=13.6307(6) Å, c=12.3307(6) Å, α=90°, β=97.116(2)°, γ=90°, and the crystal structure of the infrared nonlinear optical crystal material belongs to the monoclinic system, and the space group is P twenty one.
[0007] Furthermore, the inorganic skeleton of the infrared nonlinear crystal is composed of isolated [Sb2Br 10 ] 4- Octahedral dimer composition, Sb 3+ is the octahedral center, two [SbBr6] 3- The octahedra are connected by sharing a single edge, and there are 21 helical axes in the structure. The organic amine ligand components surround the inorganic framework through hydrogen bonding and Coulomb interaction.
[0008] Furthermore, the organic amine ligand is R-(+)-α-methylbenzylamine or S-(-)-α-methylbenzylamine.
[0009] The chiral hybrid antimony (III) halide nonlinear crystal provided by the present invention has a chemical formula of (R-MBA)4Sb2Br 10 and (S-MBA)4Sb2Br 10 , wherein R-MBA is R-(+)-α-methylbenzylamine, S-MBA is S-(-)-α-methylbenzylamine, and the structures are respectively Formula 1 and Formula 2:
[0010] Formula 1; Formula 2.
[0011] According to the present invention, the infrared nonlinear optical crystal has excellent infrared second-order nonlinear optical properties and also has fluorescence characteristics.
[0012] The second object of the present invention is to provide a method for preparing the above infrared nonlinear optical crystal, comprising the following steps:
[0013] S1. Dissolve antimony trioxide in a hydrobromic acid solution, add R-(+)-α-methylbenzylamine or S-(-)-α-methylbenzylamine, and then heat and stir to completely dissolve it to obtain a light yellow clear solution, and then cool it to room temperature and slowly evaporate it to obtain a bulk single crystal;
[0014] S2, washing the single crystal sample multiple times with a specific solvent, and then drying it under natural conditions for later use; then dissolving and dispersing it in a good solvent to obtain a light yellow clear solution;
[0015] S3, adding a certain amount of anti-solvent to the light yellow solution obtained in step S2 until fine crystal nuclei appear, thereby obtaining a precursor solution; taking a certain amount of the precursor solution and drop-casting it onto a pretreated silicon wafer substrate, slowly evaporating it at a certain temperature, and finally obtaining chiral organic-inorganic hybrid antimony (III) halide nanosheets, i.e., infrared nonlinear optical crystals, on the substrate.
[0016] Furthermore, in step S1, the mass molar ratio of R-(+)-α-methylbenzylamine to antimony trioxide is 2:1-8:1, or the mass molar ratio of S-(-)-α-methylbenzylamine to antimony trioxide is 2:1-8:1.
[0017] Furthermore, the required heating and stirring temperature is 110-120°C, the stirring time is 25-30 min, and the required evaporation time is 3-7 days.
[0018] Furthermore, in step S2, the washing solvent is n-hexane or cyclohexane, and the good solvent is acetonitrile.
[0019] Furthermore, in step S3, the anti-solvent is toluene.
[0020] Furthermore, in step S3, the pretreatment method of the silicon wafer is: immersing the C-side sapphire substrate in corresponding washing liquids in the order of acetone, ethanol, and water, and ultrasonicating for 20 to 25 minutes respectively; the evaporation temperature is set to 40 to 50°C.
[0021] The third object of the present invention is to provide a use of the above-mentioned infrared nonlinear optical crystal, wherein the infrared nonlinear optical crystal is used to prepare infrared band laser frequency conversion crystal devices and remote sensor devices.
[0022] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0023] (1) The present invention provides a compound having a molecular formula of C 32 H 48 Br 10 The new structure of N4Sb2 is a crystalline compound, belonging to the monoclinic system, with a space group of P21, the unit cell parameters are a=28.5206(15) Å, b=13.6307(6) Å, c=12.3307(6)Å, α=90°, β=97.116(2)°, γ=90°. The chiral amine induces an intrinsic central asymmetric structure, which results in good nonlinear optical performance and high SHG response. Under the excitation of a near-infrared 1064 nm laser (NPILASERS, 1064 nm, <15 ps, 50 MHz, Rainbow 1064OEM), the material shows a high SHG signal at 532 nm. Compared with commercial Y-cut quartz, the SHG response signal of the crystal is 300 times that of quartz, showing a high second-order nonlinear optical coefficient. It is expected to be applied to nonlinear optical devices, laser frequency doubling, polarized light detection, etc., and also provides a new idea for the design of nonlinear optical materials.
[0024] (2) The raw material cost of the present invention is low, the process operation is simple, and it meets environmental protection requirements. In addition, the material has promising application prospects in optical communications and sensors.
[0025] (3) The inventive concept provided by the present invention is that by introducing chiral amines, the inorganic skeleton can be induced to produce chiral transformation, thereby obtaining the intrinsic non-centrosymmetric structure required by SHG. This method provides a good idea for designing nonlinear optical materials. At the same time, organic-inorganic hybrid metal halides have the characteristics of rich and adjustable structures, adjustable electronic structures, and excellent photoelectric properties. In addition, they have low-cost solution processability and are easy to use in large-scale production, so they have broad application prospects in various fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a crystal structure diagram of the chiral organic-inorganic hybrid antimony (III) halide nanosheet prepared in Example 1 of the present invention;
[0027] Figure 2 This is a crystal structure diagram of the chiral organic-inorganic hybrid antimony (III) halide nanosheet prepared in Example 2 of the present invention;
[0028] Figure 3 This is a common optical photograph of the chiral organic-inorganic hybrid antimony (III) halide nanosheet of Example 1;
[0029] Figure 4 The powder XRD patterns of the chiral organic-inorganic hybrid antimony (III) halide powder and single crystal simulation prepared by the present invention;
[0030] Figure 5 The XRD patterns of chiral organic-inorganic hybrid antimony (III) halide powders prepared at different feed molar ratios are shown;
[0031] Figure 6 This is a scanning electron microscope image of the chiral organic-inorganic hybrid antimony (III) halide nanosheet prepared in Example 1;
[0032] Figure 7 This is a comparison chart of SHG signal intensities of the chiral organic-inorganic hybrid antimony (III) halide nanosheets prepared in Example 1 and commercial Y-cut quartz;
[0033] Figure 8 SHG intensity of the chiral organic-inorganic hybrid antimony (III) halide nanosheets prepared in Example 1 at different powers;
[0034] Fig. 9 This is a linear fitting diagram of the SHG intensity of the chiral organic-inorganic hybrid antimony (III) halide nanosheets prepared in Example 1 at different powers as a function of power;
[0035] Fig.10 This is the SHG polarization diagram of the chiral organic-inorganic hybrid antimony (III) halide nanosheet prepared in Example 1. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical scheme and advantages of the present invention clearer, the specific embodiments of the present invention are further described in detail below in conjunction with specific examples and drawings. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially.
[0037] Example 1
[0038] This embodiment provides an infrared nonlinear optical crystal (chiral organic-inorganic hybrid antimony (III) halide nanosheet (R-MBA) 4Sb2Br 10 ) preparation method:
[0039] (1) Dissolve 0.25 mmol of antimony trioxide in 6 mL of 48% hydrobromic acid aqueous solution, add 2 mmol of R-(+)-α-methylbenzylamine, then heat and stir to 120°C. After fully reacting for 30 min, let stand and slowly cool to room temperature. Wait for 3 to 7 days to obtain light yellow block single crystals.
[0040] (2) Take out the light yellow block single crystal obtained in step 1, wash it three times with n-hexane, and dry it under natural conditions for later use;
[0041] (3) Weigh 6 mg of the single crystal obtained in step 2 above, dissolve it in 1 mL of acetonitrile solution, and stir thoroughly to obtain a light yellow clear solution;
[0042] (4) Take 7 mL of toluene and drip it into the light yellow clear solution in step 3 until fine crystal nuclei are produced to obtain a precursor solution. Using the anti-solvent evaporation drop casting method, take 20 µL of the precursor solution and drop cast it on a culture dish covered with a silicon wafer substrate. The solvent is slowly evaporated at 40°C to obtain chiral organic-inorganic hybrid antimony (III) halide nanosheets. The steps for cleaning the silicon wafer substrate are as follows: ultrasonically use acetone, ethanol, and deionized water for 20 minutes in sequence to clean the impurities on the substrate surface.
[0043] The single crystal diffraction data prepared above were collected by a German Bruker D8 Venture single crystal diffractometer. 10 The unit cell parameters obtained by data analysis are: a=28.5206(15) Å, b=13.6307(6) Å, c=12.3307(6) Å, α=90°, β=97.116(2)°, γ=90°, belonging to P 21 space groups.
[0044] like Figure 1 As shown, (R-MBA)4Sb2Br prepared in Example 1 10 Schematic diagram of the crystal structure of a single crystal. As can be seen from the figure, the inorganic skeleton of the crystal consists of isolated [Sb2Br 10 ] 4- Octahedral dimer composition, Sb 3+ is the octahedral center, two [SbBr6] 3- The octahedra are connected by sharing a single edge, and there are 21 helical axes in the structure. The organic amine ligand components surround the inorganic framework through hydrogen bonding and Coulomb interaction.
[0045] like Figure 3 As shown, the infrared nonlinear optical crystal (R-MBA) 4Sb2Br prepared in Example 1 10 Optical photo of nanosheets. As can be seen from the figure, the obtained (R-MBA)4Sb2Br 10 The nanosheets have a regular morphology, and their length and width are at the micrometer level.
[0046] like Figure 4 As shown, the preparation of (R-MBA)4Sb2Br in Examples 1 and 2 10 Powder XRD patterns of powder and single crystal simulation. Figure 4 It can be seen from the XRD diagram that the results obtained by testing the actual powder sample are consistent with the simulated powder XRD diagram, proving that the powder has a high phase purity.
[0047] like Figure 6, which is a scanning electron microscope image of the chiral organic-inorganic hybrid antimony (III) halide nanosheet prepared in Example 1. As can be seen from the figure, the prepared chiral organic-inorganic hybrid antimony (III) halide nanosheet has regular edges, further illustrating the uniformity of the obtained sample.
[0048] like Figure 7 The figure shows the comparison of SHG signal intensity between the chiral organic-inorganic hybrid antimony (III) halide nanosheets prepared in Example 1 and commercial Y-cut quartz under the same test conditions. Using a confocal microscope system, an ultrafast fiber laser (NPI LASERS, 1064 nm, <15 ps, 50 MHz, Rainbow 1064OEM) was used as the light source to irradiate the chiral organic-inorganic hybrid antimony (III) halide nanosheets with a silicon wafer as the substrate, with an output power of 127.4 mW. Under the same test conditions, the SHG response signal of the chiral organic-inorganic hybrid antimony (III) halide nanosheets is about 300 times that of the commercial Y-cut quartz, showing good SHG performance.
[0049] like Figure 8 and Fig. 9 As shown, the SHG intensity of the chiral organic-inorganic hybrid antimony (III) halide nanosheets prepared in Example 1 at different powers and the linear fitting diagram of SHG intensity with power change are shown. As can be seen from the figure, as the power increases, the generated SHG intensity gradually increases. At the same time, the fitting results prove that the SHG intensity and power show a quadratic correlation property, which further proves the second-order nonlinear optical response characteristics of the chiral organic-inorganic hybrid antimony (III) halide nanosheets.
[0050] Example 2
[0051] This embodiment provides an infrared nonlinear optical crystal (chiral organic-inorganic hybrid antimony (III) halide nanosheet (R-MBA) 4Sb2Br 10 ) preparation method:
[0052] (1) Dissolve 0.25 mmol of antimony trioxide in 6 mL of 48% hydrobromic acid aqueous solution, add 2 mmol of R-(+)-α-methylbenzylamine, then heat and stir to 120°C. After fully reacting for 30 min, let stand and slowly cool to room temperature. Wait for 3 to 7 days to obtain light yellow block single crystals.
[0053] (2) Take out the light yellow block single crystal obtained in step 1, wash it three times with n-hexane, and dry it under natural conditions for later use;
[0054] (3) Weigh 6 mg of the single crystal obtained in step 2 above, dissolve it in 1 mL of acetonitrile solution, and stir thoroughly to obtain a light yellow clear solution;
[0055] (4) Take 8 mL of toluene and drip it into the light yellow clear solution in step 3 until fine crystal nuclei are produced to obtain a precursor solution. Using the antisolvent evaporation drop casting method, take 20 µL of the precursor solution and drop cast it on a culture dish covered with a silicon wafer substrate. The solvent is slowly evaporated at 50 °C to obtain chiral organic-inorganic hybrid antimony (III) halide nanosheets.
[0056] like Fig.10 The figure shows the SHG polarization diagram of the chiral organic-inorganic hybrid antimony (III) halide nanosheet prepared in Example 2. It can be seen that the chiral hybrid antimony (III) halide nanosheet prepared in Example 2 has obvious anisotropy, and the polarization rate is 97.4%.
[0057] Example 3
[0058] This embodiment provides an infrared nonlinear optical crystal (chiral organic-inorganic hybrid antimony (III) halide nanosheet (S-MBA) 4Sb2Br 10 ) preparation method:
[0059] (1) Dissolve 0.25 mmol of antimony trioxide in 6 mL of 48% hydrobromic acid aqueous solution, add 2 mmol of S-(-)-α-methylbenzylamine, then heat and stir to 120°C, react for 30 min, then stand and slowly cool to room temperature. Wait for 3 to 7 days to obtain light yellow block single crystals.
[0060] (2) Take out the light yellow block single crystal obtained in step 1, wash it three times with n-hexane, and dry it under natural conditions for later use;
[0061] (3) Weigh 6 mg of the single crystal obtained in step 2 above, dissolve it in 1 mL of acetonitrile solution, and stir thoroughly to obtain a light yellow clear solution;
[0062] (4) Pipette 7 mL of toluene and add the light yellow clear solution in step 3 until fine crystal nuclei appear to obtain a precursor solution. Figure 1 As shown, 20 µL of the precursor solution was drop-cast on a culture dish covered with a silicon wafer substrate, and the solvent was slowly evaporated at 40 °C to obtain chiral organic-inorganic hybrid antimony (III) halide nanosheets.
[0063] like Figure 2 As shown, (S-MBA)4Sb2Br prepared in Example 3 10 Schematic diagram of the crystal structure of a single crystal. As can be seen from the figure, the inorganic skeleton of the crystal consists of isolated [Sb2Br 10 ] 4- Octahedral dimer composition, Sb 3+ is the octahedral center, two [SbBr6]3- Connected by a shared edge, with a 21-helical axis in the structure, the organic amine ligand components wrap around the inorganic framework through hydrogen bonding interactions and Coulomb interactions.
[0064] Example 4
[0065] This embodiment provides infrared nonlinear optical crystals prepared with different feed ratios.
[0066] The specific preparation steps are basically the same as those in Example 1, except that:
[0067] Experimental group 1: the mass molar ratio of R-(+)-α-methylbenzylamine and antimony trioxide was 2:1;
[0068] Experimental group 2: the mass molar ratio of R-(+)-α-methylbenzylamine and antimony trioxide was 4:1;
[0069] Experimental group 3: the mass molar ratio of R-(+)-α-methylbenzylamine and antimony trioxide was 6:1;
[0070] Test group 4: same as Example 1;
[0071] Experimental group 5: the mass molar ratio of S-(+)-α-methylbenzylamine and antimony trioxide was 2:1;
[0072] Experimental group 6: the mass molar ratio of S-(+)-α-methylbenzylamine and antimony trioxide was 4:1;
[0073] Experimental group 7: the mass molar ratio of S-(+)-α-methylbenzylamine to antimony trioxide was 6:1;
[0074] Test group 8: Same as Example 3.
[0075] like Figure 5 As shown, the powder XRD patterns of the infrared nonlinear optical crystals prepared in test groups 1-8 are shown. As can be seen from the figure, the infrared nonlinear optical crystals prepared in test groups 1-8 have the same characteristic diffraction peaks and crystal planes. The inventors found in the research process that when the mass molar ratio of organic ligand to antimony trioxide is higher than 8:1 or lower than 2:1, the generated crystals are more inorganic crystals and cannot achieve infrared nonlinear optical characteristics.
[0076] In the absence of conflict, the above embodiments and features in the embodiments may be combined with each other.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An infrared nonlinear optical crystal, characterized in that: The molecular formula of the infrared nonlinear crystal is C 32 H 48 Br 10 N4Sb2, whose unit cell parameters are a=28.5206(15) Å, b=13.6307(6) Å, c=12.3307(6) Å, α=90°, β=97.116(2)°, γ=90°, and the crystal structure of the infrared nonlinear optical crystal material belongs to the monoclinic system, and the space group is P twenty one; The method for preparing the infrared nonlinear optical crystal comprises the following steps: S1. Dissolve antimony trioxide in a hydrobromic acid solution, add R-(+)-α-methylbenzylamine or S-(-)-α-methylbenzylamine, and then heat and stir to completely dissolve it to obtain a light yellow clear solution, and then cool it to room temperature and slowly evaporate it to obtain a bulk single crystal; S2, washing the single crystal sample multiple times with a specific solvent, and then drying it under natural conditions for later use; then dissolving and dispersing it in a good solvent to obtain a light yellow clear solution; The washing solvent is n-hexane or cyclohexane, and the good solvent is acetonitrile; S3, adding a certain amount of anti-solvent toluene to the light yellow solution obtained in step S2 until fine crystal nuclei appear, thereby obtaining a precursor solution; taking a certain amount of the precursor solution and drop-casting it onto a pretreated silicon wafer substrate, slowly evaporating it at a certain temperature, and finally obtaining a chiral organic-inorganic hybrid antimony (III) halide nanosheet on the substrate, that is, an infrared nonlinear optical crystal.
2. The infrared nonlinear optical crystal according to claim 1, characterized in that: The inorganic framework of the infrared nonlinear crystal is composed of isolated [Sb2Br 10 ] octahedral dimer composition, Sb 3+ It is the octahedral center, two [SbBr6] octahedra are connected by sharing an edge, and there are 21 helical axes in the structure. The organic amine ligand component surrounds the inorganic framework through hydrogen bond interactions and Coulomb interactions.
3. The infrared nonlinear optical crystal according to claim 2, characterized in that: The organic amine ligand is R-(+)-α-methylbenzylamine or S-(-)-α-methylbenzylamine.
4. The infrared nonlinear optical crystal according to claim 3, characterized in that: In step S1, the mass molar ratio of R-(+)-α-methylbenzylamine to antimony trioxide is 2:1-8:1, or the mass molar ratio of S-(-)-α-methylbenzylamine to antimony trioxide is 2:1-8:
1.
5. The infrared nonlinear optical crystal according to claim 4, characterized in that: The required heating and stirring temperature is 110~120℃, the stirring time is 25~30 min, and the required evaporation time is 3~7 days.
6. The infrared nonlinear optical crystal according to claim 5, characterized in that: In step S3, the pretreatment method of the C-surface sapphire is: immerse the silicon wafer substrate in the corresponding washing liquid in the order of acetone, ethanol and water, and ultrasonicate for 20-25 minutes respectively; the evaporation temperature is set to 40-50°C.
7. Use of the infrared nonlinear optical crystal according to any one of claims 1 to 6, characterized in that: The infrared nonlinear optical crystal is used for preparing infrared band laser frequency conversion crystal devices and remote sensor devices.
Citation Information
Patent Citations
Organic-inorganic hybrid chiral perovskite helical structure micron sheet and preparation method and application thereof
CN114875472A
Lead-free double perovskite luminescent material and preparation method thereof
CN115449364A
Organic-inorganic hybrid antimony oxyfluoride second-order nonlinear optical crystal material and preparation and application thereof
CN117987918A
Chiral cheating agent and chiral catlyst
US20040176243A1
Perovskite crystal, preparation method therefor, and x-ray detector
WO2022033501A1