Preparation method of magnesium high performance concrete anti-cracking agent

By using magnesium high-performance anti-cracking agents prepared from materials such as light-burned magnesium oxide, the problem of cracks caused by shrinkage and deformation of concrete during the hardening process is solved, the crack resistance and durability are improved, and production costs are reduced.

CN118439816BActive Publication Date: 2024-10-08QINGHAI SANKUN BUILDING MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410537612.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2024-10-08
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

During the hardening process of existing concrete, shrinkage deformation caused by changes in temperature and humidity causes cracks. The reaction rate of existing magnesium expansion agents is poor and the production process is complex, resulting in limited anti-crack effects and high costs.

Method used

It uses materials such as light-burned magnesia, magnesium slag, fly ash, silica fume and sodium borate, and is mixed and calcined at low and high temperatures to form a magnesium high-performance anti-cracking agent with a porous structure, which can regulate the expansion performance of concrete and reduce the heat release of hydration reaction. , enhance crack resistance and durability.

Benefits of technology

Effectively compensates for the shrinkage deformation of concrete, enhances crack resistance and impermeability, reduces production costs, improves the stability and durability of concrete, and optimizes construction performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118439816B_ABST
    Figure CN118439816B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a magnesium high-performance concrete anti-cracking agent. The anti-cracking agent consists of: 80-85 parts of light-burned magnesium oxide, 8-10 parts of magnesium slag, 5-8 parts of fly ash, 4-7 parts of silica fume, 2-3 parts of sodium borate and 1-3 parts of sodium polycarboxylate. The preparation method comprises the following steps: crushed magnesia ore and dolomite ore are calcined in a rotary kiln respectively and then ball-milled, mixed in proportion to obtain light-burned magnesium oxide, and then mixed with fly ash, silica fume, magnesium slag after ball milling, sodium borate and sodium polycarboxylate, and homogenized to obtain a finished product. The anti-cracking agent prepared by the invention has crack resistance, impermeability, compression resistance and tensile resistance, improves the stability and durability of concrete, adds solid waste raw materials, saves energy and protects the environment, and is easy to promote.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of concrete admixtures, and in particular to a method for preparing a magnesium high-performance concrete anti-cracking agent. Background Art

[0002] Concrete for construction is a hydraulic cementitious material. It is widely used in roads, bridges, and the construction industry because of its economy and compression resistance. When concrete cementitious materials undergo hydration reaction from pouring to final setting, they are easily affected by changes in factors such as temperature and humidity inside and outside the concrete structure, causing the concrete to shrink in volume during hardening and use. When the tensile stress formed by the shrinkage deformation of concrete exceeds the ultimate tensile strength of concrete, it will cause cracks in concrete buildings, which will not only affect the appearance quality of the concrete building, but also reduce its bearing capacity and durability.

[0003] Shrinkage deformation is the phenomenon that the volume of concrete shrinks due to the evaporation of water during the hardening process. Concrete shrinkage mainly includes chemical shrinkage, drying shrinkage and temperature shrinkage. Chemical shrinkage refers to the shrinkage caused by the reaction between the cementitious material in the concrete and water, because the total volume of the generated substances is less than the total volume of the substances before the reaction. It is the phenomenon that the volume of substances shrinks during chemical reactions. Drying shrinkage is due to the continuous evaporation and loss of internal water after the concrete is dried or affected by high temperature outside after hardening, causing the concrete to become dry from the inside out. Temperature shrinkage is the phenomenon that after the concrete is poured, the cement hydration reaction releases heat, causing the concrete temperature to rise. As the concrete hydration reaction rate decreases until the hydration reaction ends, the concrete enters a cooling process due to the continuous loss of heat. In this process, the volume reduction accompanied by the temperature drop is called temperature drop shrinkage. Chemical shrinkage, drying shrinkage and temperature shrinkage of concrete are the main causes of non-load cracking of concrete.

[0004] When an expansive agent is added to concrete, it generates crystals during the hydration process, which causes volume expansion and compensates for the shrinkage of concrete over time, thereby improving the crack resistance of concrete and reducing the risk of structural cracking. The expansive agents currently used in concrete are mainly calcium expansive agents and magnesium expansive agents. Calcium expansive agents mainly include calcium oxide and calcium sulfoaluminate, but their reaction rate is relatively fast, and the adjustability of the expansion process is poor. The hydration heat of concrete is increased during the expansion process, and the shrinkage of concrete in the temperature drop stage cannot be effectively compensated. The anti-cracking effect is general. Although the reaction rate of magnesium expansive agents can be adjusted by the calcination temperature to match the shrinkage temperature of concrete in the temperature drop stage, it has a long hydration cycle, an adjustable expansion process, and stable properties of hydration products. However, unmodified magnesium oxide has a porous structure, and its adsorption of water and water reducers is large, which will affect the construction and workability of concrete.

[0005] Announcement No. CN 108147705 B discloses a magnesium-based high-efficiency anti-cracking agent for cement concrete, a preparation method thereof, and an application thereof. The magnesium-based expansion component and a layer of cement hydration heat regulating component dextrin covered on the surface are used to improve the expansion performance of magnesium oxide, enhance the regulating efficiency of cement hydration heat regulating materials, achieve the coordinated effect of compensating shrinkage and temperature control, and improve the anti-cracking performance of concrete. However, this method uses a spray drying tower to spray and disperse the magnesium-based expansion component, and uses a high-speed centrifugal atomizing disk to atomize the cement hydration heat regulating material component into micro-liquid beads with a droplet diameter of 10 to 50 μm. The cement hydration heat regulating component is adsorbed in the pores of the magnesium-based expansion component particles and covers the particle surface by physical adsorption and chemical reaction during the spray drying process. The water in the micro-liquid beads is quickly dried by the high-temperature airflow to obtain a magnesium-based high-efficiency anti-cracking agent. However, this method has a complicated production process and a relatively high cost for large-scale application.

[0006] Announcement No. CN 111377648 B discloses a magnesium-based, temperature-controlling and moisture-controlling high-efficiency anti-cracking agent for cement concrete, and its preparation method and application. The agent adopts a magnesium expansion component, a zeolite component containing water in the pores, and a layer of temperature-sensitive material coated on the surface of the magnesium and zeolite. The anti-cracking agent prepared by this method overcomes the adverse effects of internal curing materials and magnesium oxide on the workability of concrete, realizes the coordinated effect of shrinkage compensation and temperature control, and improves the anti-cracking performance of concrete. However, the anti-cracking agent is suitable for concrete structures with side walls, bottom plates and top plates of C50 and above strength grade with mold entry temperature reaching above 25°C and temperature rise value reaching above 20°C, and with shrinkage compensation, crack resistance, impermeability and temperature control requirements. The use of the agent has limitations, and the paraffin liquid is atomized into micro-liquid beads by a spray device in a fluidized bed and added to the magnesium expansion component. The preparation process is also relatively complicated.

[0007] Therefore, it is an urgent problem to be solved in the current concrete industry to modify magnesium oxide and find a concrete anti-cracking agent with controllable expansion rate and cycle, so as to compensate for the shrinkage of concrete expansion, improve the crack resistance, stability and durability of concrete, and reduce production costs. Summary of the invention

[0008] The purpose of the present invention is to provide a method for preparing a magnesium high-performance concrete anti-cracking agent to solve the problem of shrinkage cracking of concrete during the hardening process proposed in the above background technology.

[0009] To achieve the above object, the present invention provides the following technical solution: a method for preparing a magnesium high-performance concrete anti-cracking agent, wherein the concrete anti-cracking agent comprises the following parts by weight: 80-85 parts of light-burned magnesium oxide, 8-10 parts of magnesium slag, 5-8 parts of fly ash, 4-7 parts of silica fume, 2-3 parts of sodium borate, and 1-3 parts of sodium polycarboxylate, and the preparation steps are as follows:

[0010] Step 1: Preparation of light-burned magnesium oxide:

[0011] (1) Crushing: magnesite and dolomite are crushed in a crusher respectively, the screen diameter is 10 mm, and the speed of the crusher is 550-600 rpm;

[0012] (2) adding the crushed magnesite and dolomite to a rotary kiln for calcination and cooling, wherein the temperature of the rotary kiln is set to 370-400° C. in the low temperature section, the calcination time is 15-20 minutes, and the high temperature section is 850-900° C., the calcination time is 35-45 minutes, and the rotation speed of the rotary kiln is 0.5-0.6 rpm. The calcined material is transferred to a cooling device for cooling, and the material temperature after cooling is ≤35° C., thereby obtaining magnesite and dolomite clinker;

[0013] (3) The calcined and cooled magnesite and dolomite raw materials are respectively put into a ball mill to be ball-milled into 600 mesh fine powder raw materials, and then mixed in a mass ratio of 5 to 6:1 to obtain a light-burned magnesium oxide raw material;

[0014] Step 2: respectively grinding magnesium slag, sodium borate and sodium polycarboxylate in a ball mill to obtain a 600-mesh raw material;

[0015] Step 3: Mix and homogenize the light-burned magnesium oxide, magnesium slag, fly ash, silica ash, sodium borate and sodium polycarboxylate obtained in steps 1 and 2 in a certain proportion to obtain a finished product.

[0016] As a preferred technical solution of the present invention, the light-burned magnesium oxide has a magnesium oxide content of ≥90% and a specific surface area of

[0017] ≥800m2 / kg.

[0018] As a preferred technical solution of the present invention, the fly ash particle size is 10-25 μm, the silica fume particle size is 0.1-0.3 μm, and the specific surface area is ≥20m 2 / g.

[0019] As a preferred technical solution of the present invention, the rotation speed of the ball mill is 90 to 95 rpm.

[0020] As a preferred technical solution of the present invention, the setting parameters of the homogenizer are pressure 8.5-10 MPa, rotation speed 3500-4000 rpm, and homogenization time 15-20 minutes.

[0021] As a preferred technical solution of the present invention, the cooling is carried out by using a cooling device equipped with a cooling fan. The cooling device is connected to the outlet of the rotary kiln through a conveyor belt. The material fired in the rotary kiln is conveyed to the cooling device via the conveyor belt for cooling. The cooling fan is installed every 50 to 60 cm at a height of 70 to 80 cm above the conveyor belt of the cooling device, and the fan speed is 2000-2200 rpm.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The light-burned magnesium oxide raw material of the present invention is prepared by mixing magnesite and dolomite after calcination in a certain proportion, which can increase and enhance the active components of the light-burned magnesium oxide. In the calcination process, a low temperature of 370-400° C. and a high temperature of 850-900° C. are used to mix and calcine the magnesium oxide so that the magnesium oxide can form a more porous crystal structure, improve the specific surface area, activity and dispersibility of the magnesium oxide, and the light-burned magnesium oxide undergoes a hydration reaction in concrete, so that the volume of the concrete is increased and the shrinkage of the cement concrete during the drying process is reduced. The light-burned magnesium oxide obtained by light-burning magnesite and dolomite ore and the magnesium oxide expansion sources with different activities in the magnesium slag are flexibly matched, and the high activation reaction time of the magnesite and the low activation reaction time of the dolomite ore are matched, so that the expansion performance of the concrete is synchronized with the shrinkage of the concrete, and the concrete structure is more compact, thereby enhancing the crack resistance, impermeability and tensile resistance of the concrete, and improving the stability and durability of the concrete.

[0024] 2. The present invention adds magnesium slag, fly ash and silicon powder solid waste to the raw materials in proportion, which can reduce the amount of calcined magnesium oxide and cement, turn waste into treasure, reduce production costs, and at the same time improve the activity of light-burned magnesium oxide, slow down the hydration reaction of concrete, reduce heat release, increase the toughness of concrete, reduce the cracking of concrete under load, improve the strength and durability of concrete, and optimize the working performance of concrete.

[0025] 3. The sodium borate added in the present invention reacts with the silicate in fly ash and silica fume to generate silicate borate, which improves the compactness and strength of concrete while reducing the hydration reaction rate of cement, thereby delaying the release of hydration heat. The sodium polycarboxylate reacts with calcium ions in cement, etc., improves the fluidity of concrete, and slows down the hydration process of concrete. At the same time, the sodium polycarboxylate can disperse materials such as silica fume, cement, fly ash, etc. in concrete, so that the materials are mixed more evenly, and the corresponding chemical reactions of the components are more effectively generated, which reduces the agglomeration of materials, improves the compressive and tensile strength and toughness of concrete, and inhibits the cracking process of concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of a method for preparing a magnesium high performance concrete anti-cracking agent of the present invention.

[0027] Figure 2 This is a line graph showing the effect of calcination temperature on the specific surface area of ​​magnesite and dolomite.

[0028] Figure 3 This is a line graph showing the effect of calcination temperature on the active reaction time of magnesite and dolomite. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Magnesite is an important magnesium source mineral belonging to the trigonal crystal system. Its main chemical component is magnesium carbonate (MgCO3). Dolomite is a carbonate mineral. Its main chemical component is CaMg(CO3)2. Magnesium slag is a common waste in the production of magnesium and its alloys. Its main components are magnesium oxide (8-10%), calcium oxide (40-50%), silicon dioxide (20-30%), aluminum oxide (2-5%), and iron oxide (6-9%).

[0031] Magnesium oxide (MgO) reacts with water in concrete to form magnesium hydroxide Mg(OH)2. Because the crystal structure of Mg(OH)2 is looser than that of MgO, it occupies more space, thereby increasing its volume. Magnesium oxide expansion agent has the advantages of low hydration water requirement, stable physical and chemical properties of hydration products, and adjustable expansion process. It improves the adverse effects of MgO on the fluidity of concrete and regulates the hydration expansion time of light-burned MgO in concrete, reduces temperature changes in concrete, and inhibits the temperature rise of concrete. It is a way to reduce the risk of shrinkage and cracking of concrete due to temperature drop.

[0032] Fly ash is a volcanic ash-like mixed material formed by high-temperature combustion of coal powder. The content of silicon dioxide in fly ash is 40-60%, aluminum oxide is 20-30%, calcium oxide is 10-20%, magnesium oxide is 5-10%, sodium oxide is 1-4%, and potassium oxide is 1-2%. In the initial stage of concrete hydration, fly ash participates less in the hydration reaction, but as the concrete hydration process advances, the concentration of calcium hydroxide in the medium increases, and it begins to react with fly ash particles to form hydrated calcium silicate gel. This reaction releases less heat and reacts slowly.

[0033] Silica fume is produced in the process of high-temperature smelting of industrial silicon and ferrosilicon in industrial electric furnaces. The particle size of silica fume is 0.1-0.3 μm, and the specific surface area is large, about 16000-23000 m 2 / kg, it is very active. The silica content in silica fume is 90-95%, alumina is 0.8-1%, iron oxide is 0.8-1.5%, calcium oxide is 1.2-1.5%, and magnesium oxide is 1-1.2%. The loss on ignition of silica fume is about 1.5%-3%. The silicon dioxide, calcium oxide and other components in silica fume can react with calcium hydroxide in cement to form hydrated calcium silicate gel, which can improve the strength and durability of concrete. The fine particles in silica fume have a filling effect on concrete, can reduce the porosity of concrete, and optimize the working performance of concrete. The strength effect of silica fume can increase the toughness of concrete and reduce the cracking tendency of concrete under load.

[0034] Sodium borate reacts with silicates in fly ash and silica ash to form borosilicate, which can fill cement pores, improve cement density and hardness, reduce cement hydration reaction rate, and delay the release of hydration heat. At the same time, sodium borate can delay the setting time of concrete, reduce the viscosity and surface tension of concrete, thereby improving the fluidity of concrete, making it easier for concrete to fill gaps and holes in the formwork, and ensuring the density and impermeability of concrete.

[0035] Sodium polycarboxylate can improve the microstructure of concrete, making it more compact and uniform. As a water reducer, sodium polycarboxylate can significantly reduce the water consumption of concrete. Sodium polycarboxylate has good dispersibility and water retention. It can dissolve in water and adsorb on the surface of cement particles to form a stable charge barrier. This charge barrier can prevent the agglomeration of cement particles and make cement particles better dispersed in water, thereby improving the fluidity of concrete. The molecules of sodium polycarboxylate contain carboxylic acid groups, which can react with calcium ions in cement, slow down the hydration process of cement, and delay and reduce the release of hydration heat.

[0036] The light-burned magnesium oxide raw material of the invention is prepared by mixing magnesite and dolomite after calcination in a certain proportion, so that the active components of the light-burned magnesium oxide can be increased and enhanced. In the calcination process, a mixed calcination method of low temperature 370-400 DEG C and high temperature 850-900 DEG C is adopted, so that the magnesium oxide can form a more porous crystal structure, improve the specific surface area, activity and dispersibility of the magnesium oxide, and the light-burned magnesium oxide undergoes a hydration reaction in concrete to generate a looser crystal structure of magnesium hydroxide, which occupies a larger space, thereby increasing the volume of the concrete and reducing the shrinkage of the cement concrete during the drying process. The light-burned magnesium oxide obtained by light-burning magnesite and dolomite ore and magnesium oxide expansion sources with different activities in magnesium slag are flexibly matched, and the high activation reaction time of the magnesite and the low activation reaction time of the dolomite ore are matched, so that the expansion performance of the concrete is regulated, the expansion performance of the concrete is synchronized with the shrinkage of the concrete, and the concrete structure is made denser, thereby enhancing the crack resistance, impermeability and tensile resistance of the concrete, and improving the stability and durability of the concrete.

[0037] The present invention adds magnesium slag, fly ash and silicon powder solid waste into the raw materials in proportion, which can reduce the amount of calcined magnesium oxide and cement, turn waste into treasure, reduce production costs, and at the same time improve the activity of light-burned magnesium oxide, slow down the hydration reaction of concrete, reduce heat release, increase the toughness of concrete, reduce the cracking of concrete under load, improve the strength and durability of concrete, and optimize the working performance of concrete.

[0038] The sodium borate added in the present invention reacts with silicates in fly ash and silica fume to generate borosilicate, which can fill the pores of cement concrete, improve the compactness and strength of concrete, reduce the hydration reaction speed of cement, thereby delaying the release of hydration heat and reducing the cracking of concrete caused by temperature. The sodium polycarboxylate reacts with calcium ions in cement, etc., improves the fluidity of concrete, slows down the hydration process of concrete, delays and reduces the release of hydration heat. At the same time, the sodium polycarboxylate can disperse materials such as silica fume, cement, fly ash and the like in concrete, so that the materials are mixed more evenly, the corresponding chemical reactions of the components are more effectively generated, the agglomeration and condensation of materials are reduced, the compressive and tensile strengths and toughness of concrete are improved, and the cracking process of concrete is inhibited.

[0039] The raw materials used in the present invention are all commercially available raw materials.

[0040] Embodiment 1:

[0041] A method for preparing a magnesium high-performance concrete anti-cracking agent, the specific steps of which are:

[0042] Step 1: Preparation of light-burned magnesium oxide:

[0043] (1) Crushing: magnesite and dolomite are crushed in a crusher respectively, the screen diameter is 10 mm, and the speed of the crusher is 600 rpm;

[0044] (2) The crushed magnesite and dolomite are put into a rotary kiln for calcination and cooling. The temperature of the rotary kiln is set to 400° C. in the low temperature section for 15 minutes and 900° C. in the high temperature section for 35 minutes. The rotation speed of the rotary kiln is 0.5 rpm. The calcined material is transferred to a cooling device for cooling. The temperature of the cooled material is ≤35° C. to obtain magnesite and dolomite clinker. The cooling device is connected to the outlet of the rotary kiln through a conveyor belt. The material fired in the rotary kiln is conveyed to the cooling device for cooling via the conveyor belt. A cooling fan is installed every 60 cm at a height of 80 cm above the conveyor belt of the cooling device. The fan speed is 2000 rpm.

[0045] (3) The calcined and cooled magnesite and dolomite raw materials are respectively put into a ball mill and ground into 600 mesh fine powder raw materials at a speed of 90 rpm, and then mixed in a mass ratio of 5:1 to obtain light-burned magnesium oxide raw materials.

[0046] Step 2: respectively grind magnesium slag, sodium borate and sodium polycarboxylate in a ball mill to obtain 600-mesh raw materials.

[0047] Step 3: Mix and homogenize 85 parts of light-burned magnesium oxide obtained in steps 1 and 2, 8 parts of magnesium slag, 8 parts of fly ash, 4 parts of silica fume, 2 parts of sodium borate, and 3 parts of sodium polycarboxylate. The parameters of the homogenizer are set as pressure 10 MPa, speed 3500 rpm, and homogenization time 15 minutes to obtain a finished product.

[0048] Embodiment 2:

[0049] A method for preparing a magnesium high-performance concrete anti-cracking agent, the specific steps of which are:

[0050] Step 1: Preparation of light-burned magnesium oxide:

[0051] (1) Crushing: magnesite and dolomite are crushed in a crusher respectively, the screen diameter is 10 mm, and the speed of the crusher is 600 rpm;

[0052] (2) The crushed magnesite and dolomite are put into a rotary kiln for calcination and cooling. The temperature of the rotary kiln is set to 370° C. in the low temperature section for 20 minutes and 850° C. in the high temperature section for 45 minutes. The rotation speed of the rotary kiln is 0.6 rpm. The calcined material is transferred to a cooling device for cooling. The temperature of the cooled material is ≤35° C. to obtain magnesite and dolomite clinker. The cooling device is connected to the outlet of the rotary kiln through a conveyor belt. The material fired in the rotary kiln is conveyed to the cooling device for cooling via the conveyor belt. A cooling fan is installed every 60 cm at a height of 80 cm above the conveyor belt of the cooling device. The fan speed is 2000 rpm.

[0053] (3) The calcined and cooled magnesite and dolomite raw materials are respectively put into a ball mill and ground into 600 mesh fine powder raw materials at a speed of 95 rpm, and then mixed in a mass ratio of 6:1 to obtain light-burned magnesium oxide raw materials.

[0054] Step 2: respectively grind magnesium slag, sodium borate and sodium polycarboxylate in a ball mill to obtain 600-mesh raw materials.

[0055] Step 3: Mix and homogenize 80 parts of light-burned magnesium oxide obtained in steps 1 and 2, 10 parts of magnesium slag, 5 parts of fly ash, 7 parts of silica fume, 3 parts of sodium borate, and 1 part of sodium polycarboxylate. The parameters of the homogenizer are set as pressure 8.5 MPa, speed 4000 rpm, and homogenization time 20 minutes to obtain a finished product.

[0056] Embodiment three:

[0057] A method for preparing a magnesium high-performance concrete anti-cracking agent, the specific steps of which are:

[0058] Step 1: Preparation of light-burned magnesium oxide:

[0059] (1) Crushing: magnesite and dolomite are crushed in a crusher respectively, the screen diameter is 10 mm, and the speed of the crusher is 600 rpm;

[0060] (2) The crushed magnesite and dolomite are put into a rotary kiln for calcination and cooling. The temperature of the rotary kiln is set to 390° C. in the low temperature section, the firing time is 18 minutes, and the high temperature section is 880° C., the firing time is 40 minutes. The rotation speed of the rotary kiln is 0.5 rpm. The calcined material is transferred to a cooling device for cooling. The temperature of the cooled material is ≤35° C. to obtain magnesite and dolomite clinker. The cooling device is connected to the outlet of the rotary kiln through a conveyor belt. The material fired in the rotary kiln is conveyed to the cooling device via the conveyor belt for cooling. A cooling fan is installed every 60 cm at a height of 80 cm above the conveyor belt of the cooling device. The fan speed is 2000 rpm.

[0061] (3) The calcined and cooled magnesite and dolomite raw materials are respectively put into a ball mill and ground into 600 mesh fine powder raw materials at a speed of 95 rpm, and then mixed in a mass ratio of 6:1 to obtain light-burned magnesium oxide raw materials.

[0062] Step 2: respectively grind magnesium slag, sodium borate and sodium polycarboxylate in a ball mill to obtain 600-mesh raw materials.

[0063] Step 3: Mix and homogenize 82 parts of light-burned magnesium oxide obtained in steps 1 and 2, 9 parts of magnesium slag, 6 parts of fly ash, 5 parts of silica fume, 2.5 parts of sodium borate, and 2 parts of sodium polycarboxylate. The parameters of the homogenizer are set as pressure 9 MPa, speed 3600 rpm, and homogenization time 18 minutes to obtain a finished product.

[0064] Comparative Example 1:

[0065] The step (2) in step 1 is changed to adding the crushed magnesite and dolomite to a rotary kiln for calcination and cooling. The temperature of the rotary kiln is set to a low temperature of 400° C., the firing time is 65 minutes, the rotation speed of the rotary kiln is 0.6 rpm, and the calcined material is transferred to a cooling device for cooling. The temperature of the cooled material is ≤35° C. to obtain magnesite and dolomite clinker. The cooling device is connected to the outlet of the rotary kiln through a conveyor belt. The material fired in the rotary kiln is conveyed to the cooling device via the conveyor belt for cooling. A cooling fan is installed every 60 cm at a height of 80 cm above the conveyor belt of the cooling device. The fan speed is 2000 rpm. The remaining steps are the same as those in Example 2.

[0066] Comparative Example 2:

[0067] The step (2) in step 1 is changed to adding the crushed magnesite and dolomite to a rotary kiln for calcination and cooling. The temperature of the rotary kiln is set to a high temperature of 850° C., the firing time is 65 minutes, the rotation speed of the rotary kiln is 0.6 rpm, and the calcined material is transferred to a cooling device for cooling. The temperature of the cooled material is ≤35° C. to obtain magnesite and dolomite clinker. The cooling device is connected to the outlet of the rotary kiln through a conveyor belt. The material fired in the rotary kiln is conveyed to the cooling device via the conveyor belt for cooling. A cooling fan is installed every 60 cm at a height of 80 cm above the conveyor belt of the cooling device. The fan speed is 2000 rpm. The remaining steps are the same as those in Example 2.

[0068] Comparative Example 3:

[0069] Remove the fly ash and silica fume in step three, and the remaining steps are the same as those in embodiment two.

[0070] Comparative Example 4:

[0071] The sodium borate and sodium polycarboxylate in step three are removed, and the remaining steps are the same as those in embodiment two.

[0072] Comparative Example 5:

[0073] Remove the fly ash, silica fume, sodium borate and sodium polycarboxylate in step three, and the remaining steps are the same as those in embodiment two.

[0074] 11 parts of the anti-cracking agent prepared by Examples 1, 2, 3 and Comparative Examples 1, 2, 3, 4 and 5 were added with 70 parts of cement, 80 parts of fine sand, 65 parts of coarse sand and 90 parts of gravel, and 105 parts of water were added and stirred evenly. The mixture was stirred and cured according to GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures" and GB8076-2008 "Concrete Admixtures". The compressive strength and axial tensile strength of the concrete were tested according to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete"; the anti-seepage pressure of the concrete and the cracking area of ​​the concrete were tested according to GB / T50082-2019 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete", and the axial tensile strength of the concrete was tested according to GB / T50081-2016 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete". The test results are shown in Table 1, and the blank group is concrete without the addition of anti-cracking agent.

[0075] The cement is Conch brand P·O42.5 cement, the fine sand particle size is 0.35~0.25mm, the coarse sand particle size is 0.6~1.2mm, and the stone size is 7~20mm.

[0076] Table 1

[0077]

[0078] As shown in Table 1, the compressive strength, anti-seepage pressure, axial tensile strength and anti-cracking effect of Examples 1, 2 and 3 in which an anti-cracking agent is added are greatly improved. Comparative Example 1 adopts low-temperature calcination at 400°C, and the activity of magnesium oxide is not completely released, and the specific surface area is small, resulting in a relatively poor expansion compensation shrinkage effect when added to concrete. In Comparative Example 1, continuous high-temperature calcination may cause partial sintering or agglomeration of light-burned magnesium oxide, affecting its hydration reaction in concrete. In Comparative Example 3, fly ash and silica fume are not added, and the activity of cement in concrete is strong, and the hydration reaction releases heat, resulting in shrinkage and cracking of concrete due to temperature changes. In Comparative Example 4, sodium borate and sodium polycarboxylate are not added, and its tensile strength and anti-seepage pressure are relatively low.

[0079] The present invention adopts GB / T 19587-2017 "Determination of specific surface area of ​​solid matter by gas adsorption BET method" and CBMF19-2017 "Magnesium oxide expansion agent for concrete" to determine the specific surface area and active reaction time of light-burned magnesium oxide obtained by different calcination methods for magnesite and dolomite ore.

[0080] like Figure 2 and Figure 3 As shown in the figure, after calcining magnesite and dolomite after crushing, the specific surface area of ​​magnesite and dolomite increases with the increase of calcination temperature at 300-900℃. After calcination at 900℃, the specific surface area reaches the maximum, and the specific surface area of ​​magnesite is 350m 2 / kg, dolomite ore is 355m 2 / kg, then the higher the calcination temperature, the greater the decrease in specific surface area. Due to the intensified sintering and agglomeration of magnesium oxide particles at high temperature, its specific surface area decreases. The active reaction time increases with the stable increase at 300-900℃. The active reaction time of dolomite and dolomite is the largest at 900℃, which are 250s and 170s respectively. With the increase of calcination temperature, the active reaction time decreases. The longer the active reaction time, the higher the later expansion of light-burned magnesium oxide, and the smaller the early expansion. Low reaction activity time means that the early expansion rate is faster and the later expansion is slightly smaller.

[0081] Magnesite and dolomite were calcined by the following calcination methods respectively, and then mixed in proportion to obtain light-burned magnesium oxide. The specific surface area and active reaction time of the light-burned magnesium oxide were measured. Figure 2 and Figure 3 The light-burned magnesium oxide obtained by calcination method 1 has a larger specific surface area of ​​920m 2 / kg, the active reaction time is relatively long, which is 220s. The light-burned magnesium oxide obtained by calcining at low temperature of 400℃ has a small specific surface area of ​​350m 2 / kg, the active reaction time is short, which is 100s. Under low-temperature calcination conditions, the active content of magnesium oxide is low and its activity is not fully released. Magnesium oxide particles calcined at a high temperature of 900℃ may partially sinter or agglomerate. The specific surface area and activity of light-burned magnesium oxide are not as high as those calcined at low and high temperatures.

[0082] Calcination method 1: (1) Crushing: magnesite and dolomite ore are crushed in a crusher respectively, the screen diameter is 10 mm, and the speed of the crusher is 550-600 rpm;

[0083] (2) adding the crushed magnesite and dolomite to a rotary kiln for calcination and cooling, wherein the temperature of the rotary kiln is set to 400° C. in the low temperature section, the firing time is 15 minutes, and the high temperature section is set to 900° C., the firing time is 35 minutes, and the rotation speed of the rotary kiln is 0.5 rpm. The calcined material is transferred to a cooling device for cooling, and the temperature of the cooled material is ≤35° C., thereby obtaining magnesite and dolomite clinker;

[0084] (3) The calcined and cooled magnesite and dolomite raw materials are respectively put into a ball mill and ground into 600 mesh fine powder raw materials, and then mixed in a mass ratio of 5:1 to obtain a light-burned magnesium oxide raw material;

[0085] Calcination method 2:

[0086] The calcination temperature of the rotary kiln is set to 400°C in the low temperature section, the firing time is 50 minutes, there is no high temperature section calcination, and the other steps are the same as the calcination method one.

[0087] Calcination method three:

[0088] The calcination temperature of the rotary kiln is set to 900°C in the low temperature stage, the firing time is 50 minutes, there is no low temperature stage calcination, and the other steps are the same as the calcination method one.

[0089] Table 2

[0090] <![CDATA[Specific surface area (m 2 / kg)]]> Active reaction time (s) Calcination method 1 920 220 Calcination method 2 350 100 Calcination method three 680 160

[0091] In summary, the light-burned magnesium oxide raw materials of the present invention, magnesite and dolomite, are mixed and calcined at low temperature of 370-400° C. and high temperature of 850-900° C. to improve the specific surface area, activity and dispersibility of magnesium oxide, and play a role in compensating shrinkage in concrete. At the same time, the added magnesium slag, fly ash and silica powder solid waste can reduce the amount of calcined magnesium oxide and cement, turning waste into treasure, reducing production costs, and at the same time improving the activity of light-burned magnesium oxide, slowing down the hydration reaction of concrete, reducing heat release, increasing the toughness of concrete, reducing the cracking of concrete under load, and enhancing the strength and Durability, sodium borate reacts with silicates in fly ash and silica fume to form silicate borate, which improves the density and strength of concrete while reducing the hydration reaction rate of cement and delaying the release of hydration heat. Sodium polycarboxylate reacts with calcium ions in cement to improve the fluidity of concrete and slow down the hydration process of concrete. At the same time, sodium polycarboxylate can disperse silica fume, cement, fly ash and other materials in concrete, making the materials mixed more evenly, allowing the corresponding chemical reactions of the components to occur more effectively, reducing the agglomeration of materials, improving the compressive and tensile strength and toughness of concrete, and inhibiting the cracking process of concrete.

[0092] The above are only specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent replacements or modifications made based on the present invention to solve basically the same technical problems and achieve basically the same technical effects are all included in the protection scope of the present invention.

Claims

1. A method for preparing a magnesium high performance concrete anti-cracking agent, characterized in that: Using light-burned magnesium oxide, magnesium slag, fly ash, silica fume, sodium borate and sodium polycarboxylate as raw materials, high-performance concrete anti-cracking agent is obtained by crushing, calcining, mixing and homogenizing. The process steps are as follows: Step 1: Preparation of light-burned magnesium oxide: (1) Crushing: crush the magnesite and dolomite ore separately in a crusher with a screen diameter of 10 mm; (2) The crushed magnesite and dolomite are added to a rotary kiln for calcination and cooling to obtain clinker of magnesite and dolomite. The temperature of the rotary kiln is set to 370-400°C in the low temperature section, the firing time is 15-20 minutes, and the high temperature section is 850-900°C, the firing time is 35-45 minutes, and the rotation speed of the rotary kiln is 0.5-0.6 rpm; (3) The calcined and cooled magnesite and dolomite raw materials are respectively put into a ball mill and ground into 600 mesh powders, and then mixed in a mass ratio of 5 to 6:1 to obtain light-burned magnesium oxide raw materials; Step 2: respectively grinding magnesium slag, sodium borate and sodium polycarboxylate in a ball mill to obtain a 600-mesh raw material; Step 3: 80-85 parts of light-burned magnesium oxide, 8-10 parts of magnesium slag and pulverized coal obtained in steps 1 and 2 are added. 5-8 parts of ash, 4-7 parts of silica fume, 2-3 parts of sodium borate and 1-3 parts of sodium polycarboxylate are mixed and homogenized in proportion to obtain a finished concrete anti-cracking agent.

2. The method for preparing a magnesium high performance concrete anti-cracking agent according to claim 1, characterized in that: In step 1, cooling is performed using a cooling device equipped with a cooling fan.

3. The method for preparing a magnesium high performance concrete anti-cracking agent according to claim 2, characterized in that: The cooling device is connected to the outlet of the rotary kiln through a conveyor belt, and the materials fired in the rotary kiln are conveyed to the cooling device for cooling through the conveyor belt. Cooling fans are installed every 50 to 60 cm at a height of 70 to 80 cm above the conveyor belt of the cooling device. The fan speed is 2000-2200 rpm, and the temperature of the light-burned material after cooling is ≤35°C.

4. The method for preparing a magnesium high performance concrete anti-cracking agent according to claim 1, characterized in that: The speed of the pulverizer is 550-600 rpm, and the speed of the ball mill is 90-95 rpm.

5. The method for preparing a magnesium high performance concrete anti-cracking agent according to claim 1, characterized in that: The particle size of fly ash is 10-25 μm, the particle size of silica fume is 0.1-0.3 μm, and the specific surface area is ≥20 m 2 / g.

6. The method for preparing a magnesium high performance concrete anti-cracking agent according to claim 1, characterized in that: The magnesium oxide content in light-burned magnesium oxide is ≥90%, and the specific surface area is ≥800m 2 / kg.

7. The method for preparing a magnesium high performance concrete anti-cracking agent according to claim 1, characterized in that: In step three, a horizontal homogenizer is used for homogenization, and the setting parameters of the homogenizer are pressure 8.5-10 MPa, rotation speed 3500-4000 rpm, and homogenization time 15-20 minutes.