A high-polymerization degree PVC specially used for foam injection molding and its preparation method

By using copolymerized soft monomers such as vinyl acetate and methyl acrylate and vinyl chloride monomers in high-polymer PVC materials, the melt strength and the fluidity are improved, and the high-polymerized materials cannot be foamed and injection-molded. The problem is that the strength and toughness of the product are improved, and the performance is better than that of the SG8 PVC resin.

CN118459645BActive Publication Date: 2024-11-19YUNNAN ZHENGBANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410580727.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2024-11-19
Estimated Expiration
2044-05-11

AI Technical Summary

Technical Problem

High-polymerization PVC materials cannot be foamed and injection-molded, while low-polymerization foamed injection-molded products do not have enough strength and toughness.

Method used

Copolymerized soft monomers such as vinyl acetate and methyl acrylate are used to coordinate the modification with vinyl chloride monomers to reduce the melt strength of the resin and improve the melt flowability. Through the combination of copolymerized soft monomers and vinyl chloride monomers in a specific proportion, Control the reaction temperature to prepare high-polymerization PVC materials with a polymerization degree greater than 750.

Benefits of technology

The normal foaming and injection molding of high-polymerization PVC materials has been achieved, which improves the strength and toughness of the product, solves the problem that high-polymerization materials cannot foam and injection molding, and improves the performance of SG8 type PVC resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a high-polymerization degree PVC for foaming injection molding and a preparation method thereof, and relates to the field of PVC polymerization technology, and specifically to a high-polymerization degree PVC for foaming injection molding and a preparation method thereof. The raw material components of the high-polymerization degree PVC include: vinyl chloride monomer, copolymerized soft monomer, dispersant, initiator, stabilizer, defoamer and terminator. The present invention adopts low-temperature polymerization and ternary copolymerization modification of soft monomers to prepare high-polymerization degree PVC for foaming injection molding. The polymerization temperature of the PVC of the present invention is between 59°C and 67°C, and the mass of the soft monomer in the copolymerized monomer accounts for 1% to 10% of the total mass of the monomer; the degree of polymerization of the finished product is above 750, and it can be foamed and injected normally; and the performance is stronger than the foaming injection molding materials currently on the market, which solves the problem of insufficient strength and toughness of the current foaming material SG8 type PVC resin, and has very excellent market value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PVC polymerization, and in particular relates to a high-polymerization degree PVC specially used for foaming injection molding and a preparation method thereof. Background Art

[0002] At present, the PVC resin used for injection molding and foaming in China is basically SG8 type (polymerization degree 740~650) resin with relatively low polymerization degree, which is easy to foam and injection mold. However, its polymerization degree is low, the strength and toughness of the products are insufficient, and the adjustable space of formula design is insufficient. While the SG7 type (polymerization degree 845~741), SG6 type (polymerization degree 980~846), and SG5 type (polymerization degree 1135~981) resins with higher polymerization degree, although the product strength and toughness are high, are not suitable for foaming and injection molding due to high melt strength and poor melt fluidity. The present invention aims to prepare a polymer resin with high strength and toughness and a polymerization degree greater than 750, and adopts copolymerization modification of the second and third monomers to reduce the melt strength of the resin and improve the melt fluidity, so that the PVC resin with a higher polymerization degree can be foamed and injection molded normally, solving the problem that the high polymerization degree PVC resin cannot be foamed and injection molded, and the low polymerization degree foamed and injection molded products have insufficient strength and toughness. Summary of the invention

[0003] In view of the above deficiencies in the prior art, one of the purposes of the present invention is to develop a high polymerization degree PVC material to solve the problem that high polymerization degree PVC cannot be foamed or injection molded, while low polymerization degree foamed or injection molded products have insufficient strength and toughness.

[0004] To achieve the above purpose, the specific technical solutions of the present invention are as follows:

[0005] A high-polymerization degree PVC material specially used for foam injection molding, the raw material components of the material include: vinyl chloride monomer, copolymer soft monomer, dispersant, initiator, stabilizer, terminator and defoamer; wherein the copolymer soft monomer is composed of vinyl acetate and at least one of methyl acrylate, ethyl acrylate, 2-methyl methacrylate or 2-ethyl methacrylate, and the mass of the copolymer soft monomer accounts for 1-10% of the total monomer amount; the vinyl acetate monomer accounts for 1-5% of the total monomer amount.

[0006] The total amount of monomers is the sum of the masses of vinyl chloride monomer and copolymerized soft monomer.

[0007] The polymerization degree of the above-mentioned high-polymerization PVC material is greater than 750, and the strength and toughness of its products are high. The copolymerized soft monomer selected by the PVC material of the present invention is a mixture of vinyl acetate and methyl acrylate, ethyl acrylate, 2-methyl methacrylate or 2-ethyl methacrylate in a certain proportion. The present invention modifies the PVC material by using a specific proportion of copolymerized soft monomer and vinyl chloride monomer to reduce the melt strength of the resin, so that the melt fluidity of the prepared PVC material is better, and it is easier to foam and injection mold, which solves the problem that the high-polymerization PVC material in the prior art cannot be foamed and injection molded.

[0008] Furthermore, the dispersant includes a main dispersant 1, a main dispersant 2 and an auxiliary dispersant, and the added amount is 550-1550 ppm of the total amount of monomers.

[0009] The main dispersant 1 is polyvinyl alcohol (PVA) with an alcoholysis degree in the range of 71-89 mol%, and the addition amount is 400-800 ppm of the total monomer amount; the main dispersant 2 is at least one of methyl cellulose (MC), hydroxymethyl cellulose (CMC), hydroxyethyl cellulose (HEC), and hydroxypropyl methyl cellulose (HPMC), and the addition amount is 100-500 ppm of the total monomer amount; the auxiliary dispersant is PVA with an alcoholysis degree in the range of 45-55 mol%, and the addition amount is 50-250 ppm of the total monomer amount.

[0010] Furthermore, the initiator is at least one of tert-butyl peroxyneodecanoate, cumyl peroxyneodecanoate, di(3,3,5-trimethylhexanoyl) peroxide, and bis(2-ethylhexyl) peroxydicarbonate, and the added amount is 250-750 ppm of the total monomer amount.

[0011] Furthermore, the stabilizer is at least one of ammonia water, sodium carbonate and sodium bicarbonate, and the added amount is 100-400 ppm of the total amount of the monomers.

[0012] Furthermore, the terminator is bisphenol A, and the added amount is 300-700 ppm of the total amount of monomers.

[0013] Furthermore, the defoaming agent is at least one of polysiloxane, organic modified polysiloxane and polyether modified silicone, and the added amount is 100-300 ppm of the total amount of monomers.

[0014] Another object of the present invention is to provide a method for preparing a high-polymerization degree PVC material dedicated to foam injection molding, comprising the following steps:

[0015] Dispersant, stabilizer, pure water and initiator are added to the reactor in proportion; nitrogen is passed through, vinyl chloride monomer is added, and then copolymer soft monomer is added; the reaction is carried out at 59-67°C, and water needs to be continuously added during the reaction process according to the volume reduction during polymerization; the pressure drop is 1 bar, defoamer and terminator are added, and the material is cooled and discharged after stirring; after drying, a high-polymerization degree PVC finished product is obtained.

[0016] In the process of preparing high-polymerization PVC, reaction temperature is an important indicator for controlling the degree of polymerization. If the reaction temperature is too high and the initiator's initiation rate is too fast, the degree of polymerization of the prepared PVC product will be low, even lower than 750; if the reaction temperature is too low, the degree of polymerization of the polymer resin will be too high, resulting in poor melt fluidity and unsuitable for foaming and injection molding.

[0017] Furthermore, the average polymerization degree of the high-polymerization PVC finished product is above 750. The present invention modifies the resin by vinyl chloride monomer and copolymerized soft monomer, so that the high-polymerization PVC material can be foamed and injection molded normally; and the performance of the PVC finished product prepared by the method of the present invention is stronger than that of the foaming injection molding material on the current market, which solves the problem that the high-polymerization PVC material cannot be foamed and injection molded, and solves the problem that the current foaming material SG8 type PVC resin has insufficient strength and toughness, and has very excellent market value.

[0018] The present invention also establishes a set of evaluation systems for foaming and injection molding of high-polymerization PVC resin prepared by the method. The method includes replacing SG8 resin with the resin of the present invention under the condition that the existing mature SG8 injection molding and foaming formula and processing technology remain unchanged, and performing injection molding and foaming experiments, and judging the adaptability of the resin of the present invention in the field of injection molding and foaming by paying attention to the injection molding pressure and foaming conditions.

[0019] Compared with the prior art, the present invention is beneficial in that:

[0020] (1) The present invention provides a high-polymerization degree PVC material specially used for foaming and injection molding. The PVC material is modified at a specific temperature with a specific ratio of copolymerized soft monomer and vinyl chloride monomer, thereby reducing the melt strength of the resin, making the melt fluidity of the prepared PVC material better and easier to foam and inject, thereby solving the problem that the high-polymerization degree PVC material in the prior art cannot be foamed and injected; (2) The preparation method of the present invention is simple, easy to operate, and easy to industrialize. In the preparation process of the high-polymerization degree PVC material, by controlling the ratio of the copolymerized monomer to the vinyl chloride monomer and the reaction temperature, the high-polymerization degree PVC material prepared by the present invention can reach a polymerization degree of more than 750, having a higher polymerization degree than SG8, ​​being able to be normally injected and foamed, and having stronger performance than SG8, ​​and having broad market application prospects. DETAILED DESCRIPTION

[0021] The following is a clear and complete description of the technical solution of the present invention in combination with the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention. Any equivalent transformation or substitution made by those skilled in the art based on the following implementation methods belongs to the protection scope of the present invention.

[0022] The reagents or instruments used in the following examples without indicating the manufacturer are all conventional reagent products that can be obtained through commercial purchase.

[0023] The present invention discloses a high-polymerization degree PVC material for foam injection molding, wherein the raw material components of the material include: vinyl chloride monomer, copolymer soft monomer, dispersant, initiator, stabilizer, terminator and defoamer; the copolymer soft monomer can be composed of vinyl acetate and at least one of methyl acrylate, ethyl acrylate, 2-methyl methacrylate or 2-ethyl methacrylate, the mass of the copolymer soft monomer accounts for 1-10% of the total mass of the monomer, and the vinyl acetate monomer accounts for 1-5% of the total mass of the monomer. The reaction temperature is preferably 59-67°C. The high-polymerization degree PVC material of the present invention can be obtained by using the above copolymer soft monomers, so in the following embodiments, unless otherwise specified, the copolymer soft monomer is composed of vinyl acetate and 2-methyl methacrylate monomers.

[0024] The dispersant includes a main dispersant 1, a main dispersant 2 and an auxiliary dispersant, and the addition amount is 550-1550ppm of the total monomer amount. Among them, the main dispersant 1 can be PVA with an alcoholysis degree in the range of 71-89mol%, and the addition amount is 400-800ppm of the total monomer amount; the main dispersant 2 can be at least one of methyl cellulose (MC), hydroxymethyl cellulose (CMC), hydroxyethyl cellulose (HEC), and hydroxypropyl methyl cellulose (HPMC), and the addition amount is 100-500ppm of the total monomer amount; the auxiliary dispersant can be PVA with an alcoholysis degree in the range of 45-55mol%, and the addition amount is 50-250ppm of the total monomer amount.

[0025] The initiator may be at least one of tert-butyl peroxyneodecanoate, cumyl peroxyneodecanoate, di(3,3,5-trimethylhexanoyl)peroxide, and bis(2-ethylhexyl)peroxydicarbonate, and the added amount is 250-750 ppm of the total monomer amount.

[0026] The stabilizer may be at least one of ammonia water, sodium carbonate and sodium bicarbonate, and the added amount is 100-400 ppm of the total amount of the monomers.

[0027] The terminator can be any existing terminator, and the added amount is 300-700 ppm of the total amount of monomers. In the following examples, unless otherwise specified, the terminator is bisphenol A.

[0028] The defoamer can be at least one of polysiloxane, organic modified polysiloxane and polyether modified silicone, and the added amount is 100-300 ppm of the total monomer amount. In the following examples, unless otherwise specified, the defoamer used is polysiloxane.

[0029] The embodiments described below are only some embodiments of the present invention, rather than all embodiments.

[0030] Example 1

[0031] This embodiment provides a method for preparing high-polymerization degree PVC for foam injection molding, comprising the following steps:

[0032] S1. Clean the reactor, add the adjusted dispersant to the reactor, the main dispersant 1 is a PVA solution with a degree of alcoholysis of 72 mol%, a PVA concentration of 1.0%, and an addition amount of 550 g, the main dispersant 2 is an HPMC solution, an HPMC concentration of 1.0%, and an addition amount of 275 g, and the auxiliary dispersant is a PVA solution with a degree of alcoholysis of 55 mol%, a PVA concentration of 40.0%, and an addition amount of 2.50 g;

[0033] S2. Add sodium bicarbonate stabilizer to the reactor in an amount of 2.50g;

[0034] S3. Add pure water to the reactor in an amount of 12000g;

[0035] S4 initiator was added to the reactor, initiator 1 was tert-butyl peroxy neodecanoate, added in an amount of 4.5g, initiator 2 was cumyl peroxy neodecanoate, added in an amount of 4.5g;

[0036] S5. Nitrogen was passed to replace the air in the reactor, nitrogen was replaced 4 times, stirring was turned on, vinyl chloride monomer was added, the addition amount was 7520g, 2-methyl methacrylate monomer was added, the addition amount was 400g, and vinyl acetate monomer was added 80g;

[0037] S6. Raise the temperature to 59°C and start the reaction. During the reaction, water needs to be continuously added according to the volume reduction during the polymerization;

[0038] S7. Add the terminator at a pressure drop of 1 bar in an amount of 10 g, add the defoamer in an amount of 2.5 g, stir for 10 min and then cool and discharge;

[0039] S8. Drying: drying at 65°C for 48h to obtain a high polymerization degree PVC finished product.

[0040] After testing, the degree of polymerization of the high-polymerization degree PVC product prepared in Example 1 is 1000.

[0041] The foaming performance of the high polymerization degree PVC prepared in Example 1 was verified, wherein the formula, extruder foaming conditions and results are shown in Table 1.

[0042] Table 1: Foaming conditions and results of the finished product obtained in Example 1 and SG8 type resin

[0043]

[0044] The injection molding performance of the high polymerization degree PVC prepared in Example 1 was verified, wherein the formula, injection molding conditions of the injection molding machine and the results are shown in Table 2.

[0045] Table 2: Injection molding conditions and results of the finished product obtained in Example 1 and SG8 type resin

[0046]

[0047] Example 2

[0048] This example is implemented according to the steps of Example 1, except that the polymerization temperature of Example 2 is 60° C. After inspection, the polymerization degree of the high-polymerization-degree PVC product prepared in Example 2 is 956.

[0049] Example 3

[0050] This embodiment is implemented according to the steps of embodiment 1, except that the polymerization temperature of embodiment 3 is 63° C. After inspection, the polymerization degree of the high polymerization degree PVC product prepared in embodiment 3 is 867.

[0051] Example 4

[0052] This embodiment is implemented according to the steps of embodiment 1, except that the copolymerized soft monomer in embodiment 4 is 616g of 2-methyl methacrylate. After inspection, the polymerization degree of the high polymerization degree PVC product prepared in embodiment 4 is 998.

[0053] Example 5

[0054] This example is implemented according to the steps of Example 1, except that the copolymerized soft monomer in Example 5 is 844 g of 2-methyl methacrylate. After testing, the degree of polymerization of the high-polymerization PVC product prepared in Example 5 is 995.

[0055] See Table 3 for the foaming and injection molding results of Examples 1-5.

[0056] Table 3: Foaming and injection molding results of Examples 1-5

[0057]

[0058] Comparative Example 1

[0059] This comparative example provides a method for preparing PVC, which is implemented according to the steps of Example 1, except that step S5 of Comparative Example 1 is: nitrogen is passed to replace the air in the reactor, nitrogen is replaced 4 times, stirring is turned on, and vinyl chloride monomer is added in an amount of 8000g. That is, all vinyl chloride monomer is added, and no comonomer is added. The PVC prepared in Comparative Example 1 cannot be foamed.

[0060] Comparative Example 2

[0061] This comparative example was implemented according to the steps of Example 1, except that step S5 of comparative example 2 was: nitrogen was introduced to replace the air in the reactor, nitrogen was replaced 4 times, stirring was turned on, vinyl chloride monomer was added in an amount of 7040 g, 2-methyl methacrylate monomer was added in an amount of 800 g, and vinyl acetate monomer was added in an amount of 160 g. That is, the mass of the comonomer accounted for 12% of the total amount of the monomers. The PVC prepared in comparative example 2 showed foaming and stratification.

[0062] Comparative Example 3

[0063] This comparative example is implemented according to the steps of Example 1, except that step S5 of comparative example 3 is: nitrogen is passed to replace the air in the reactor, nitrogen is replaced 4 times, stirring is turned on, vinyl chloride monomer is added, the addition amount is 7520g, and vinyl acetate monomer is added 480g. That is, only single vinyl acetate monomer is added, and no copolymerized soft monomer is added. The PVC prepared in comparative example 3 is not uniformly foamed and has a bulging problem.

[0064] In summary, the present invention modifies the resin by using vinyl chloride monomer and copolymerized soft monomer together and controls the reaction temperature, so as to prepare a PVC finished product which can be foamed and injected normally and has a polymerization degree of 750 or above, and the performance of the PVC finished product is stronger than that of the foaming injection molding material currently on the market, which solves the problem that the existing high-polymerization-degree PVC material cannot be foamed and injected, and also solves the problem that the current foaming material SG8 type PVC resin has insufficient strength and toughness.

[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high polymerization degree PVC material specially used for foam injection molding, characterized in that: The material is formed by reacting raw materials including vinyl chloride monomer, copolymerized soft monomer, dispersant, initiator, stabilizer, terminator and defoamer; wherein the mass of the copolymerized soft monomer accounts for 1-10% of the total monomer amount, and the copolymerized soft monomer is composed of vinyl acetate and at least one of methyl acrylate, ethyl acrylate, 2-methyl methacrylate or 2-ethyl methacrylate, wherein the vinyl acetate monomer accounts for 1-5% of the total monomer amount; The amount of the dispersant added is 550 to 1550 ppm of the total amount of the monomer; The amount of the initiator added is 250 to 750 ppm of the total amount of monomers; The amount of the stabilizer added is 100 to 400 ppm of the total amount of the monomer; The amount of the defoamer added is 100 to 300 ppm of the total amount of the monomer; The amount of the terminator added is 300 to 700 ppm of the total amount of the monomers; The reaction temperature is 59°C to 67°C; The dispersant includes a main dispersant 1, a main dispersant 2 and an auxiliary dispersant; wherein, The main dispersant 1 is PVA with an alcoholysis degree in the range of 71 to 89 mol%, and the added amount is 400 to 800 ppm of the total monomer amount; The main dispersant 2 is at least one of methyl cellulose (MC), hydroxymethyl cellulose (CMC), hydroxyethyl cellulose (HEC), and hydroxypropyl methyl cellulose (HPMC), and the added amount is 100 to 500 ppm of the total amount of the monomers; The auxiliary dispersant is PVA with an alcoholysis degree in the range of 45 to 55 mol%, and the added amount is 50 to 250 ppm of the total monomer amount; The preparation method of the high-polymerization degree PVC material dedicated to foaming injection molding comprises the following steps: adding a dispersant, a stabilizer, pure water and an initiator into a reaction kettle in proportion; passing nitrogen, adding vinyl chloride monomer, and then adding a copolymerized soft monomer; reacting at 59-67° C., and continuously replenishing water during the reaction according to the volume reduction during polymerization; adding a defoamer and a terminator when the pressure drops by 1 bar, stirring, cooling and discharging the material; and obtaining a high-polymerization degree PVC finished product after drying.

2. The high polymerization degree PVC material for foam injection molding according to claim 1, characterized in that: The initiator is at least one of tert-butyl peroxyneodecanoate, cumyl peroxyneodecanoate, di(3,3,5-trimethylhexanoyl)peroxide, and bis(2-ethylhexyl)peroxydicarbonate.

3. The high polymerization degree PVC material specially used for foam injection molding according to claim 1, characterized in that: The stabilizer is at least one of ammonia water, sodium carbonate and sodium bicarbonate.

4. The high polymerization degree PVC material for foam injection molding according to claim 1, characterized in that: The terminator is bisphenol A.

5. The high polymerization degree PVC material specially used for foam injection molding according to claim 1, characterized in that: The defoaming agent is at least one of polysiloxane, organic modified polysiloxane and polyether modified silicone.