High-residual-strength glass fiber reinforced resin composite material and preparation method thereof
By using phosphoric acid and organotin catalyst to mix Si/EP silicone modified epoxy resin and phenolic resin in composite materials, the problem of contradiction between the residual strength of the composite material and the strength of the room temperature is solved, and the high temperature and room temperature are achieved The excellent mechanical properties and flame retardancy are suitable for fire and fire rescue scenarios.
Patent Information
- Application Number
- CN202310563086.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-22
AI Technical Summary
There is a contradiction between the remaining strength and room temperature strength of existing composite materials after high temperature treatment, which cannot meet the needs of fire and fire rescue scenarios, and the application of inorganic additives or modified resins has problems of uniform distribution and poor processability.
By catalyzing the copolymerization reaction of terminal hydroxy polyphenylpropyl siloxane with epoxy resin using phosphoric acid and organotin catalyst in toluene, Si/EP siloxane modified epoxy resin is formed, and it is adjusted with phenolic resin and thermal stiffness. The agent and co-sintering aid are mixed to form a Si/EP-PF resin mixture and are compounded with glass fibers to achieve uniform distribution of inorganic elements and increase the residual strength of high temperature.
It realizes excellent mechanical properties of composite materials at high temperature and room temperature, with high temperature residual strength and room temperature strength, and has excellent flame retardancy and low smoke generation.
Smart Images

Figure CN118994658A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flame-retardant composite materials, and particularly relates to a high residual strength glass fiber reinforced resin composite material and a preparation method thereof. Background Art
[0002] Flame retardant indicators such as oxygen index, heat release, and vertical combustion cannot characterize the mechanical properties of composite materials after high-temperature treatment, and cannot meet the use requirements of fire rescue and other scenarios. The international standard ASTM F3059-18 puts forward detailed assessment requirements for the high-temperature residual mechanical properties of marine fiberglass materials.
[0003] Regarding the high-temperature residual performance of composite materials, early foreign scholars studied the performance of FRP products exposed to short-term, high-intensity thermal radiation and found that polyester or epoxy resin FRP was completely destroyed, and phenolic resin composites showed higher integrity after high-temperature treatment, but their residual strength performance still could not meet emergency needs. It is necessary to introduce inorganic additives or further modify the resin to improve the residual performance of phenolic resin composites.
[0004] By utilizing the high-temperature sinterable properties of inorganic fillers to form a ceramic surface on the composite material, the high-temperature rigidity and structural integrity of the composite material can be improved. However, this technical approach has limited effect on improving the residual performance of the composite material, and has disadvantages such as poor mechanical properties at room temperature and poor processability. The advantages and disadvantages of synthesizing high-temperature resistant phenolic resins are similar to those of introducing inorganic additives. The advantage is that the residual rate can be increased, but the structure of the residual carbon is not changed, so it is difficult to significantly improve the residual performance of the composite material. Summary of the invention
[0005] In view of the fact that the phenolic resin composite material with added powder in the prior art cannot solve the problem of uniform distribution of powder and the contradiction between high temperature residual strength and room temperature strength, the present invention uses the means of polymer elementization to achieve uniform distribution of inorganic elements. After combustion, the inorganic elements form a hybrid structure with oxygen and carbon. The hybrid structure has good compatibility with the thermal stiffness additive and co-sintering additive added later to form a co-sintering phase, thereby improving the high temperature residual strength of the composite material and solving the contradiction between high temperature residual strength and room temperature strength. According to this idea, after experimental research, the present invention provides a high residual strength glass fiber reinforced resin composite material and a preparation method thereof, wherein the glass fiber reinforced resin composite material has both excellent room temperature strength and residual strength.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The invention provides a method for preparing a glass fiber reinforced resin composite material with high residual strength. The method comprises the following steps: in toluene, phosphoric acid and an organic tin catalyst are used to catalyze a copolymerization reaction between terminal hydroxyl polyphenylpropylsiloxane and epoxy resin to obtain Si / EP siloxane modified epoxy resin; then, the Si / EP siloxane modified epoxy resin is mixed with a phenolic resin, a thermal stiffness regulator and a co-sintering aid to obtain a Si / EP-PF resin mixture; and finally, the Si / EP-PF resin mixture is composite-molded with a glass fiber cloth to obtain a glass fiber reinforced resin composite material with high-temperature residual strength.
[0008] The inventors found that the room temperature strength of epoxy resin is significantly higher than that of phenolic resin, but its high temperature residual performance is significantly lower than that of phenolic resin. If ordinary unmodified epoxy resin is directly mixed with phenolic resin as the matrix of composite material, only the room temperature strength can be improved, but the high temperature residual strength of the composite material cannot be improved or even reduced. The present invention elementizes epoxy resin by grafting epoxy resin with terminal hydroxyl polyphenyl propyl siloxane, uses Si / EP siloxane copolymer modified epoxy resin as a precursor for introducing inorganic elements, and at the same time as a toughening agent for phenolic resin (PF), and introduces inorganic powder as a thermal stiffness regulator, and mixes it with Si / EP siloxane modified epoxy resin and phenolic resin to obtain Si / EP-PF resin mixture, and finally the Si / EP-PF resin mixture is compounded with glass fiber to obtain a glass fiber reinforced resin composite material having both excellent room temperature strength and residual strength, and also excellent flame retardancy and low smoke generation.
[0009] In the prior art, it is difficult to increase the copolymerization degree of siloxane-modified epoxy resins, and the phase separation characteristics are obvious. In addition to the advantages of low weight loss at high temperature (800°C) and low weight loss rate in the middle and late stages, there are the following problems: (1) The product has poor transparency; (2) The mechanical strength is lower than that of epoxy; (3) The 5% weight loss temperature is advanced; (4) The first thermal oxidation degradation peak is similar to that of epoxy, so the residual strength of the composite material cannot be enhanced.
[0010] In the present invention, phosphoric acid and organic tin catalyst are used to catalyze the copolymerization of terminal hydroxyl polyphenylpropylsiloxane and epoxy resin in toluene solvent. The infrared image and nuclear magnetic resonance image of the product are shown in the attached Figure 2 , indicating that the copolymerization reaction did occur.
[0011] Figure 3This is the viscosity curve of copolymers with different siloxane ratios. Phenylpropylsiloxane is a solid phase at room temperature. If there are more independent siloxane phases in the synthetic material, the viscosity should increase with the increase in the amount of siloxane added. Using phosphazene catalysts, the viscosity of the resulting synthetic product decreases with the increase in the amount of phenylpropylsiloxane added. If the siloxane group is connected to the epoxy molecular chain, it can theoretically reduce the molecular force between the epoxy molecular chains, thereby reducing the viscosity. From a theoretical analysis, this phenomenon should be relatively reliable evidence.
[0012] Figure 4 It is the tensile strength of the copolymer with different siloxane ratios. At 20% and 30% siloxane ratios, the strength of the copolymer is higher than that of the unmodified epoxy. This is the uniqueness of the present invention.
[0013] Figure 5 This is an atomic force microscope micrograph and elastic modulus distribution of 30% siloxane-modified epoxy. It can be seen that the cross section of the modified epoxy is obviously rougher than that of the epoxy. From the elastic modulus distribution, except for a small amount of phenylpropyl siloxane that did not react, the entire interface is basically a dual-continuous phase structure, with the two phases being the copolymer and the unmodified epoxy resin.
[0014] Figure 6 The air environment weight loss curves and DTG curves of 30% Si / EP (new catalyst), 30% Si / EP (old catalyst) and E-51 are shown. It can be seen that the new catalytic scheme (solvent method, phosphoric acid and organotin co-catalysis) solves the problem of early weight loss.
[0015] The inventors found that using phosphoric acid and an organic tin catalyst together as catalysts will form more copolymer products than using a single catalyst, and using toluene as a solvent can inhibit the self-polymerization reaction of phenylpropyl siloxane, thereby avoiding the problem of poor uniformity of the obtained material due to the self-polymerization reaction of phenylpropyl siloxane being too rapid, which is a problem of poor transmittance in appearance.
[0016] Further preferably, the mass ratio of the terminal hydroxyl polyphenylpropyl siloxane to the epoxy resin is 25-100:100, preferably 30:70. When the terminal hydroxyl polyphenylpropyl siloxane and the epoxy resin are controlled within the above range, the mechanical properties of the composite material finally obtained are optimal.
[0017] Further preferably, the added amount of toluene is 73-77% of the mass of the epoxy resin.
[0018] Further preferably, the phosphoric acid is added in an amount of 0.15-0.25% of the mass of the epoxy resin, and the organotin catalyst is added in an amount of 0.4-0.6% of the mass of the epoxy resin.
[0019] Further preferably, the copolymerization reaction temperature is 64-68° C., and the copolymerization reaction time is 95-110 min.
[0020] In the present invention, by controlling the heating temperature and time of the copolymerization reaction, the self-polymerization side reaction is more effectively reduced, the grafting rate is improved, the structure of the polymer is adjusted, and the mechanical properties, low smoke density, compatibility and other properties of the prepared polymer are improved.
[0021] Further preferably, the Si / EP siloxane-modified epoxy resin has the following raw material composition by mass: 100 parts of epoxy resin, 25-100 parts of terminal hydroxyphenylpropyl siloxane, 73-77 parts of toluene, 0.15-0.25 parts of phosphoric acid, and 0.4-0.6 parts of dibutyltin dilaurate.
[0022] Further preferably, the epoxy resin is selected from bisphenol A glycidyl ether epoxy resin, including E51 and E44 liquid epoxy resins, such as the standard bisphenol A type E-51 epoxy resin CYD-128 produced by Yueyang Baling Petrochemical.
[0023] More preferably, the terminal hydroxyl polyphenylpropyl siloxane is a siloxane whose side group is a phenylpropyl group, and the molecular weight of the terminal hydroxyl polyphenylpropyl siloxane is 1000-1200.
[0024] Further preferably, the terminal hydroxyl polyphenylpropylsiloxane is mixed with epoxy resin and toluene to obtain a mixed solution, which is first heated to 64-68°C and kept warm for 25-30 minutes, and then phosphoric acid is added dropwise to the mixed solution while nitrogen is introduced. The mixture is reacted for 25-30 minutes, and then an organic tin catalyst is added dropwise, and the reaction is continued for 90-110 minutes. The mixture is then heated to 115-125°C, the introduction of nitrogen is stopped, and the solvent is removed by vacuum for 55-65 minutes. The resulting product is then dried at 85-95°C for 120 minutes under a vacuum environment to obtain Si / EP siloxane-modified epoxy resin.
[0025] In the actual operation process, the entire reaction system is carried out under stirring at a stirring speed of 295-305r / min. If the stirring speed is too fast, the two-phase materials with large viscosity differences will separate under the action of centrifugal force, resulting in a decrease in the degree of copolymerization, low transparency of the obtained product, and long-term static stratification. The stirring speed parameter is a key parameter.
[0026] In a preferred embodiment, the phenolic resin is a thermosetting phenolic resin, preferably a barium-catalyzed phenolic resin.
[0027] In the actual operation process, the phenolic resin used is a commercial barium hydroxide-catalyzed thermosetting phenolic resin, and the solid content of the barium hydroxide-catalyzed phenolic resin is 80%.
[0028] In a preferred embodiment, the co-sintering aids are kaolin and boron carbide; the thermal stiffness regulator is zirconium boride; and in the Si / EP-PF resin mixture, the mass ratio of kaolin: boron carbide: zirconium boride is 8-10:18-22:1.
[0029] As is known to all, high temperature resistant inorganic powder can improve the high temperature rigidity of composite materials, but it is difficult to disperse evenly in ordinary resins, and it is also incompatible with pyrolysis carbon products, and it is even more impossible to form sintering, so it is impossible to form a dense structure after sintering. In the siloxane modified resin system used in the present invention, even if the inorganic powder is not easy to disperse, the hybrid pyrolysis product of the modified resin contains a large amount of uniformly distributed inorganic elements, resulting in good compatibility between the inorganic powder and the hybrid pyrolysis product, and even possible co-sintering, which can form a dense structure with high residual strength. This idea is confirmed in the experimental data below. Kaolin and boron carbide contain a large amount of silicon oxide compounds, which are similar to the pyrolysis products of the resin system of the present invention in chemical composition, so they have good compatibility and good sinterability at about 1000 ° C, and can be used as a co-sintering aid. Zirconium boride is similar to the pyrolysis product of the resin system of the present invention in composition, has good compatibility, is easy to form a good interface, and has a higher melting point, which can further enhance high temperature rigidity as a thermal rigidity aid.
[0030] The kaolin is a commercial product with a particle size of 1000 meshes, the boron carbide is commercial grade 1 boron carbide, and the zirconium boride is 1000 meshes zirconium boride.
[0031] In a preferred embodiment, in the Si / EP-PF resin mixture, the mass ratio of phenolic resin: Si / EP siloxane-modified epoxy resin: (co-sintering aid + thermal stiffness regulator) is 58-62:37-41:31.
[0032] In a preferred embodiment, the mass ratio of the Si / EP-PF resin mixture to the glass fiber cloth is 35-45:55-65.
[0033] In a preferred embodiment, the composite molding pressure is 9-11 MPa, the temperature is 165-175° C., and the time is 115-125 min.
[0034] The present invention prepares a high residual strength glass fiber reinforced resin composite material according to the preparation method.
[0035] Principles and advantages:
[0036] principle:
[0037] The preparation method of the present invention firstly synthesizes a terminal hydroxyl polyphenyl propyl siloxane graft copolymerized epoxy resin by a solvent method under the synthesis parameters determined by experimental optimization through an innovative catalyst system of phosphoric acid and organotin, and is named Si / EP siloxane modified epoxy resin. Due to the flexibility and high temperature resistance of the siloxane group, the obtained resin has both room temperature toughening and excellent comprehensive performance of high temperature resistance. Using it as a precursor for introducing inorganic elements can achieve uniform distribution of inorganic elements and significantly improve the toughness of phenolic resin. In the resin mixture, an inorganic thermal stiffness regulator and a co-sintering aid (Inorganic Fillers) of specific components are introduced to achieve good compatibility with the hybrid pyrolysis product (M1: C / O / Si) of the modified resin, which helps to form a good pyrolysis product interface (M2: C / O / Si / IF). Finally, the Si / EP-PF resin mixture is compounded with glass fiber to obtain a glass fiber reinforced resin composite material having both excellent room temperature strength and residual strength, and also excellent flame retardancy and low smoke generation.
[0038] Advantages: The obtained siloxane-modified epoxy resin has high and uniform silicon content, high degree of polymerization, high transparency and low viscosity; the obtained composite material has high mechanical properties at room temperature and high residual strength at high temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Heat treatment specification curve for composite materials (ASTM F3059-18).
[0040] Figure 2 Example 2 IR spectra and NMR spectra of epoxy resin, polysiloxane and Si / EP-30
[0041] Figure 3 Example 2 Viscosity of Si / EP resins with different silicon contents.
[0042] Figure 4 Mechanical properties of Si / EP resin castings with different silicon contents in Example 2.
[0043] Figure 5 Atomic force microfracture and modulus distribution of Si / EP-30 and E-51.
[0044] Figure 6 Thermal gravimetric loss curves of new catalyst, old catalyst Si / EP-30 and E-51 in air environment.
[0045] Figure 7 In Example 3, the effect of the amount of Si / EP-PF resin mixture added on the properties of the composite material.
[0046] Figure 8 SEM image of the cross-section of the ablated sample of the PF sample in Example 4.
[0047] Fig. 9 SEM image of the cross-section of the ablated sample of the PF+additive sample in Example 4.
[0048] Fig.10 SEM image of the cross-section of the ablated Si / EP-PF sample in Example 4.
[0049] Fig.11 SEM image of the cross-section of the ablated sample of the Si / EP-PF+additive sample in Example 4.
[0050] Fig.12 Appearance of Si / EP siloxane-modified epoxy resin.
[0051] Fig.13 Schematic diagram of the principle of the present invention. DETAILED DESCRIPTION
[0052] In order to understand the content of this experiment, the experiment will be further explained in combination with specific implementation cases.
[0053] In the following cases, the parts of each material mentioned are parts by weight.
[0054] In the following examples,
[0055] The Si / EP-PF sample is a glass fiber reinforced resin composite material (without inorganic additives) prepared according to the scheme of the present invention.
[0056] The PF sample is a glass fiber reinforced resin composite material obtained by directly compounding and pressing barium-catalyzed phenolic resin and glass fiber cloth.
[0057] The EP / PF sample was directly mixed with unmodified epoxy resin and phenolic resin, and then composite molded with glass fiber cloth to obtain a glass fiber reinforced resin composite material.
[0058] Whether thermal stiffness regulator and co-sintering aid are added to the above samples will be explained separately in the text.
[0059] Example 1
[0060] Preparation of Si / EP siloxane modified epoxy resin:
[0061] Bisphenol A glycidyl ether epoxy resin E-51: 120g
[0062] Terminal hydroxyphenylpropylsiloxane: 30g
[0063] Toluene: 105g
[0064] Phosphoric acid: 0.4 g (E-51 mass 0.2%)
[0065] Dibutyltin dilaurate: 0.6 g (E-51 mass 0.5%)
[0066] Put E-51 and terminal hydroxyphenylpropylsiloxane into a four-necked flask in proportion, put a stirring rod in the middle of the flask, and put a thermometer, a nitrogen inlet tube and a condenser (nitrogen comes out of the condenser) in the other three flasks. Stir at a speed of 300r / min and heat to
[0067] Stir at 67°C for 0.5h, then add phosphoric acid dropwise, introduce nitrogen, react for 0.5h, then add dibutyltin dilaurate dropwise, react for 2.5h, finally raise the temperature to 120°C, stop introducing nitrogen, change the reaction apparatus to vacuum, vacuum for 1h to expel the solvent, and obtain a transparent and uniform liquid. Put the poured resin into a vacuum oven at 90°C and vacuum for 2h to obtain SI / EP silicon.
[0068] Oxyalkyl modified epoxy resin;
[0069] Preparation of Si / EP-PF resin mixture:
[0070] 40 parts of Si / EP siloxane modified epoxy resin (ES-20), 60 parts of barium catalyzed phenolic resin, 10 parts of kaolin,
[0071] Mix 20 parts of boron carbide and 1 part of zirconium boride to obtain Si / EP-PF resin mixture
[0072] Composite material preparation:
[0073] Cut a 400*400 glass fiber cloth, lay the fibers flat in the same direction in the mold, then pour in an appropriate amount of evenly mixed SI / EP-PF resin mixture, push along the fiber direction with a scraper to fully infiltrate the fiber with the resin, and then complete the layer thickness in the same way again. Using a hot pressing process, the pressure is set to 10MPa, the temperature is 170℃, and the curing time is 2h to prepare a composite material board.
[0074] Performance Testing:
[0075] The Si / EP siloxane modified epoxy resin was separated by gel permeation chromatography and the molecular weight distribution was tested. The structure of the separated product was determined by infrared spectroscopy and mass spectrometry. The degree of polymerization of the product was tested.
[0076] The composite material sample was placed on a hollow iron frame (span of 40 mm) in a muffle furnace and heated according to the heating curve required by ASTM 3059 ( Figure 1 ) is heated from room temperature to 927°C. After the treatment, when the temperature in the furnace drops to about 850°C, take out the sample, air-cool it to room temperature, weigh and record the sample mass, and place it in a dry environment for later use.
[0077] Then, an engraving machine was used to process it into a bending test specimen of standard size and put it into a drying oven for use. In order to prevent the resin content from affecting the high-temperature residual strength of the composite material, composite samples prepared from the same formulation and the same batch were taken and the resin content of the samples was measured according to GB / T 2577 to ensure that the average value of the resin content of the composite material before high-temperature heat treatment was 35% ± 1%.
[0078] It can be seen that the Si / EP siloxane-modified epoxy resin prepared in Example 1 has high transparency, good uniformity and high degree of polymerization; the composite material has a room temperature flexural strength of 384 MPa and a high temperature residual flexural strength of 87 MPa.
[0079] Example 2
[0080] The process of exploring the optimal performance of Si / EP siloxane modified epoxy resin
[0081] Experimental materials and equipment:
[0082] Epoxy resin (E-51), hydroxy-terminated polyphenylpropylsiloxane, dibutyltin dilaurate, phosphoric acid, toluene. 500ml four-necked flask, nitrogen bottle, stirrer, thermometer, gas inlet and outlet pipes, condenser, vacuum pump.
[0083] Synthesis process:
[0084] A stirring rod is placed in the middle of the four-necked flask, and a thermometer, a nitrogen inlet pipe and a condenser are placed in the other three flasks (nitrogen comes out of the condenser). 140g E-51, 60g phenylpropylsiloxane and 105g toluene (epoxy resin 75%) are added to the flask at a stirring speed of 300r / min, and the temperature is raised to 67°C and stirred for 0.5h. Then 0.28g phosphoric acid (0.2% by mass of E-51) is added dropwise, nitrogen is introduced, and the reaction is carried out for 0.5h. Then 0.7g dibutyltin dilaurate (0.5% by mass of E-51) is added dropwise, and the reaction is carried out for 2.5h. Finally, the temperature is raised to 120°C, the introduction of nitrogen is stopped, and the reaction device is changed to vacuum, and the solvent is discharged after vacuuming for 1h to obtain a transparent and uniform liquid. The poured resin is placed in a vacuum oven at 90°C and vacuumed for 2h.
[0085] The reaction formula of the synthesis mechanism is:
[0086]
[0087] Figure 1The infrared spectra of epoxy resin (CYD-128), terminal hydroxyl polyphenylpropyl siloxane and SI / EP siloxane modified epoxy resin (modified epoxy ES-30) prepared above. Analysis of the spectra: The reaction product showed characteristic peaks of Si-C6H5, Si-C3H7 and Si-OC. This indicates that polysiloxane was successfully grafted onto the epoxy resin. The relative proportion of the characteristic peak of epoxy was weakened, indicating that some of the epoxy end groups had a ring-opening reaction with Si-OH.
[0088] In addition, under the same conditions as in Example 1, only the ratio of epoxy resin (E-51) to terminal hydroxyl polyphenylpropylsiloxane was adjusted, and the mechanical properties of the composite material obtained were as follows: Figure 4 As shown, from Figure 4 It can be seen that the optimal mass ratio of the polyhydroxysiloxane to the epoxy resin is 30:70 from the perspective of strength. As mentioned above, from the viscosity data, strength data, atomic force microstructure and test modulus, and thermal gravimetric curve distribution, it can be seen that the catalytic system used in the present invention has a high degree of copolymerization.
[0089] Epoxy value of polysiloxane modified epoxy ES:
[0090] According to the hydrochloric acid / acetone method of GB-T1677-2008, the EEW values of a series of synthetic products ES-0 to ES-50 (ES stands for SI / EP siloxane-modified epoxy resin, and the following value represents the percentage of siloxane added relative to epoxy) were determined. As shown in Table 1, the actual epoxy values in ES-20 to ES-50 resins are all lower than the theoretical epoxy values, and the epoxy values are consumed. As the amount of modified component siloxane added increases, the consumption rate of epoxy groups gradually increases, further confirming that with the addition of polysiloxane, the probability of epoxy end groups in epoxy resins participating in the ring-opening reaction with Si-OH increases.
[0091] Table 1 Theoretical epoxy value, actual epoxy value and epoxy group consumption rate of ES-0 to ES-50
[0092]
[0093] Example 3
[0094] Effect of the addition amount of Si / EP-PF resin mixture on the properties of the composite material.
[0095] The other items will be the same as Example 1, only the content of Si / EP-PF is changed to optimize the ratio of Si / EP siloxane modified epoxy resin (ES) and barium catalyzed phenolic resin (PF).
[0096] Room temperature bending strength: Figure 7It can be seen that as SI / EP increases, the room temperature strength and residual strength of the sample first increase and then decrease. This shows that SI / EP has a good toughening and strengthening effect on phenolic resin at both room temperature and high temperature, verifying the material system design concept of the present invention. When SI / EP is 50%, the room temperature strength and residual strength of the sample begin to decrease, which is mainly because excessive SI / EP will produce agglomeration tendency, reducing the cross-linking curing density.
[0097] Example 4
[0098] Microscopic morphology analysis of composite materials after high-temperature treatment: After high-temperature treatment: PF samples experienced fiber melting and adhesion, indicating that the thermal oxidation degradation of the resin matrix could not properly coat and isolate the fibers. After adding thermal stiffness regulators and co-sintering aids, the PF samples retained a certain degree of integrity in the fiber structure. The inorganic additives protected the fibers, but the inorganic additives were not well compatible with the pyrolysis products and did not sinter. More resin pyrolysis products were retained between the fibers of the SI / EP-PF samples. On this basis, after introducing thermal stiffness regulators and co-sintering aids, the matrix pyrolysis residues had good compatibility with the inorganic powder and sintered with each other, making the overall structure more compact.
Claims
1. A method for preparing a high residual strength glass fiber reinforced resin composite material, characterized in that: In toluene solvent, phosphoric acid and organic tin catalyst are used to co-catalyze the copolymerization reaction of terminal hydroxyl polyphenylpropylsiloxane and epoxy resin to obtain Si / EP siloxane modified epoxy resin, and then the Si / EP siloxane modified epoxy resin is mixed with phenolic resin, thermal stiffness regulator and co-sintering aid to obtain Si / EP-PF resin mixture, and finally the Si / EP-PF resin mixture is composite-molded with glass fiber cloth to obtain a glass fiber reinforced resin composite material with high-temperature residual strength.
2. The method for preparing a high residual strength glass fiber reinforced resin composite material according to claim 1, characterized in that: The mass ratio of the terminal hydroxyl polyphenylpropylsiloxane to the epoxy resin is 25-100:
100.
3. The method for preparing a high residual strength glass fiber reinforced resin composite material according to claim 1, characterized in that: The amount of toluene added is 73-77% of the mass of the epoxy resin.
4. The method for preparing a high residual strength glass fiber reinforced resin composite material according to claim 1, characterized in that: The added amount of the phosphoric acid is 0.15-0.25% of the mass of the epoxy resin, and the added amount of the organic tin catalyst is 0.4-0.6% of the mass of the epoxy resin.
5. The method for preparing a high residual strength glass fiber reinforced resin composite material according to claim 1, characterized in that: The copolymerization reaction temperature is 64-68° C., and the copolymerization reaction time is 95-110 min.
6. The method for preparing a high residual strength glass fiber reinforced resin composite material according to claim 1, characterized in that: The epoxy resin is selected from bisphenol A glycidyl ether type epoxy resin; The terminal hydroxyl polyphenylpropyl siloxane is a siloxane whose side group is a phenylpropyl group, and the molecular weight of the terminal hydroxyl polyphenylpropyl siloxane is 1000-1200.
7. A method for preparing a high residual strength glass fiber reinforced resin composite material according to any one of claims 1 to 6, characterized in that: The terminal hydroxyl polyphenylpropylsiloxane is mixed with epoxy resin and toluene to obtain a mixed solution, which is first heated to 64-68°C and kept warm for 25-30 minutes, and then phosphoric acid is added dropwise to the mixed solution, and nitrogen is introduced at the same time, and the mixture is reacted for 25-30 minutes, and then an organic tin catalyst is added dropwise, and the reaction is continued for 90-110 minutes, and then the temperature is raised to 115-125°C, and the introduction of nitrogen is stopped. The solvent is discharged by vacuuming for 55-65 minutes, and the obtained product is then dried at 85-95°C for 120 minutes under a vacuum environment to obtain Si / EP siloxane modified epoxy resin.
8. The method for preparing a high residual strength glass fiber reinforced resin composite material according to claim 1, characterized in that: The phenolic resin is a thermosetting barium hydroxide catalyzed phenolic resin, The co-sintering aid is composed of kaolin and boron carbide, and the thermal stiffness regulator is zirconium boride. In the Si / EP-PF resin mixture, the mass ratio of kaolin: boron carbide: zirconium boride is 8-10:18-22:1; In the Si / EP-PF resin mixture, the mass ratio of phenolic resin: Si / EP siloxane-modified epoxy resin: (co-sintering aid + thermal stiffness regulator) is 58-62:37-41:
31. The mass ratio of the Si / EP-PF resin mixture to the glass fiber cloth is 35-45:55-65.
9. The method for preparing a high residual strength glass fiber reinforced resin composite material according to claim 1, characterized in that: The composite molding process is performed under a pressure of 9-11 MPa, a temperature of 165-175° C., and a time of 115-125 min.
10. A glass fiber reinforced resin composite material with high residual strength prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Chemical method for preparing organic silicon modified epoxy resin
CN102532556A
Preparation method of organosilicon modified epoxy resin
CN111499877A
Preparation and degradation methods of boride modified thermosetting phenolic resin and composite material thereof
CN113651934A
High strength pultrusion resin
US20030092866A1