Preparation method and application of long-lasting anti-fouling and high gas permeability poly 4-methyl-1-pentene membrane

By introducing fluoride into the poly-4-methyl-1-pentene membrane and adopting coating control separation layer technology, the gas permeability and blood compatibility problems of the oxygenation membrane are solved, and efficient gas exchange and long-term It has long-term anti-fouling and clogging properties and is suitable for extracorporeal membrane oxygenators.

CN118477498BActive Publication Date: 2024-10-18AQFILM MEMBRANE MATERIALS (JIAXING) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410923874.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-18
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Existing oxygenation membranes in extracorporeal membrane oxygenators have problems of insufficient gas permeability and poor blood compatibility, resulting in low gas exchange efficiency and frequent blood leakage or fouling, affecting the stable operation of the ECMO system.

Method used

By introducing fluoride into the poly-4-methyl-1-pentene membrane and adopting the method of coating a controlled separation layer, a composite layer structure with high permeability and high blood compatibility is formed. Combined with heat treatment technology, the gas content of the membrane is improved. Exchange performance and blood compatibility.

Benefits of technology

It achieves efficient gas exchange performance and long-term anti-fouling performance, significantly improves the stability and application life of the membrane, and meets the high-performance requirements of the ECMO system.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A method for preparing a long-lasting, anti-fouling and high-gas permeability poly 4-methyl-1-pentene membrane and its use belong to the field of membrane technology. The method includes: 1) dissolving poly 4-methyl-1-pentene in a diluent at high temperature, degassing online to obtain a casting solution, extruding and forming, and phase separation and solidification in a cooling bath to obtain a hollow fiber membrane; 2) dissolving poly 4-methyl-1-pentene, fluoride and alkane solvent into a homogeneous solution at room temperature, and then dip-coating the solution on the surface of the hollow fiber membrane to form an ultra-thin and dense functional separation layer; 3) placing the double-layer composite hollow fiber in a muffle furnace for heat treatment so that the two layers of polymer form a tight composite layer to obtain a poly 4-methyl-1-pentene hollow fiber membrane. The poly 4-methyl-1-pentene membrane has good gas permeability and anti-fouling performance, and can be efficiently used in oxygenators.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of membrane technology, and specifically relates to a preparation method and application of a long-lasting anti-fouling and high-gas permeability poly-4-methyl-1-pentene membrane. Background Art

[0002] Extracorporeal membrane oxygenation (ECMO) is an extracorporeal life support system that uses an extracorporeal circulation system as its basic equipment to drain venous blood from the body to the outside of the body, oxygenate it through the membrane oxygenator, and then pump the blood into the body using a blood pump. The entire process can complete the gas exchange of O2 and CO2 without the human heart and lungs, so it is also called an artificial lung. The oxygenation membrane (also called artificial lung membrane) is the core component of the ECMO system, and its function is to achieve the exchange of CO2 in the patient's blood and O2 in the air. The ideal oxygenation membrane should have: (1) efficient gas exchange capacity, with an O2 and CO2 gas exchange rate greater than 200mL / min; (2) high gas permeability and low blood leakage; (3) good blood compatibility to meet the requirements of medical devices that directly contact blood; (4) certain mechanical properties to resist the shear force generated when blood circulates. Polymethylpentene (PMP) is a semi-crystalline non-polar polyolefin resin. Due to the helical arrangement of the polymer and the bulky side chains, it is loosely packed (density is about 0.830 g / cm 3 , the smallest among all thermoplastic resins), giving it excellent gas permeability (about 10 times that of high-density polyethylene), making it an ideal oxygenation membrane material. In addition, PMP is resistant to boiling and chemicals (excellent durability against acids and alkalis), has a low surface tension (24 mN / m, second only to PTFE), and has high biosafety. The development of PMP hollow fiber oxygenation membranes mainly solves two problems: (1) membrane preparation, exploring the influence of the support layer and dense layer structure and different crystallization behaviors on the performance of the blood oxygenation process; (2) membrane blood compatibility modification research, requiring the side in contact with blood to have good blood compatibility, and the side in contact with air to be resistant to aging, have high tensile strength, and have a long service life. Summary of the invention

[0003] In view of the above-mentioned problems existing in the prior art, the purpose of the present invention is to design and provide a technical solution for a method for preparing a poly (4-methyl-1-pentene) membrane with long-lasting anti-fouling and high gas permeability and use thereof, wherein the thickness of the separation layer is regulated by coating so that the membrane has high permeability; by introducing fluorides with high blood compatibility, the compatibility between the membrane and the blood is improved to prevent blood leakage or blood fouling; the two aspects are combined to prepare high-performance membrane materials and realize their efficient application in ECMO.

[0004] The method for preparing a long-lasting anti-fouling and high-gas permeability poly-4-methyl-1-pentene membrane comprises the following steps:

[0005] 1) Dissolve 20-40 parts of poly-4-methyl-1-pentene in 60-80 parts of diluent at 220-250°C, degas online to obtain casting solution after uniform dissolution, extrude through a two-hole spinneret, the inner hole flows into the core solution, and the outer hole flows into the casting solution, and after forming, phase separation and solidification occur in a cooling bath, and after extraction and rinsing, a hollow fiber membrane is obtained;

[0006] 2) dissolving 1-5 parts of poly-4-methyl-1-pentene, 1-5 parts of fluoride and 90-98 parts of alkane solvent at room temperature into a homogeneous solution, wherein the fluoride is at least one of heptafluorobutyric acid, heptafluorobutanol, 1H, 1H, 2H-perfluoro-1-hexene, perfluoropentane, perfluorodecahydronaphthalene and chloroperfluorooctane; then dipping the solution on the surface of a clean hollow fiber membrane, and then placing the membrane in a solvent bath to induce the surface solvent to volatilize to form an ultra-thin dense functional separation layer of poly-4-methyl-1-pentene;

[0007] 3) The double-layer composite hollow fiber is placed in a muffle furnace for heat treatment, so that the two layers of polymer are embedded in each other to form a tight composite layer, thereby obtaining a poly-4-methyl-1-pentene hollow fiber membrane.

[0008] The method for preparing a long-lasting anti-fouling and high gas permeability poly 4-methyl-1-pentene membrane comprises the following steps: in step 1), the dissolution temperature is 230-240° C., 25-30 parts of poly 4-methyl-1-pentene and 65-75 parts of a diluent.

[0009] The method for preparing a long-lasting anti-fouling and high gas permeability poly 4-methyl-1-pentene membrane comprises the following steps: in step 1), the weight average molecular weight of the poly 4-methyl-1-pentene is between 180,000 and 230,000, preferably between 200,000 and 210,000; and the molecular weight distribution index is between 2.0 and 3.4, preferably between 2.5 and 3.

[0010] The method for preparing a long-lasting anti-fouling and high gas permeability poly 4-methyl-1-pentene membrane comprises the following steps: in step 1), the diluent is composed of two solvents, one of which is fixed as dioctyl phthalate, with a content of 60-80%, and the other solvent is one or two of diisobutyl phthalate, diisobutyl phthalate, tri(2-ethylhexyl) trimellitate, and dibutyl phthalate, with a content of 20%-40%.

[0011] The method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane, in step 1): the inner hole diameter of the spinneret is 0.2-0.4 mm, preferably 0.25-0.3 mm; the extrusion diameter of the casting liquid is 0.5-0.7 mm, preferably 0.6-0.65 mm; the size of the slit is controlled to be not less than 0.15 mm.

[0012] The method for preparing a long-lasting anti-fouling and high-gas permeability poly-4-methyl-1-pentene membrane comprises the following steps: in step 1), the extrusion core liquid is one of nitrogen, polyethylene glycol 200, diethylene glycol, triethylene glycol and polyethylene glycol 400; the cooling bath is one of a mixture of 70% triacetin and 30% glycerol, 80% triacetin and 20% polyethylene glycol 200, 50% polyethylene glycol 400 and 50% diethylene glycol; the temperature of the cooling bath is -20-20°C, preferably -10-10°C, and more preferably -5-5°C.

[0013] The method for preparing a long-lasting anti-fouling and high gas permeability poly 4-methyl-1-pentene membrane comprises: in step 2), 2-4 parts of poly 4-methyl-1-pentene, 2-3 parts of fluoride, and 92-95 parts of alkane solvent.

[0014] The method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane, in step 2): the alkane solvent is one or a combination of cyclohexane and trichloroethylene.

[0015] The method for preparing a long-lasting anti-fouling and high gas permeability poly 4-methyl-1-pentene membrane, in step 2): the ultra-thin thickness of the poly 4-methyl-1-pentene dense functional separation layer is 100 nanometers to 500 nanometers, preferably 200 nanometers to 400 nanometers, and more preferably 240 nanometers to 340 nanometers.

[0016] The method for preparing a long-lasting anti-fouling and high gas permeability poly 4-methyl-1-pentene membrane, in step 3): the heat treatment temperature is 130-180°C, preferably 140-170°C, more preferably 150-160°C; the heat treatment time is 2-6 hours, preferably 3-5 hours, more preferably 3.5-4.5 hours.

[0017] The present invention obtains a casting solution by selecting a suitable diluent to dissolve poly-4-methyl-1-pentene at high temperature, and then enters a cooling bath to induce phase inversion and solidify into a film. The polymer and diluent used in the present invention are optimized according to the Hansen solubility parameter theory, focusing on the system compatibility, and optimized by the dissolution temperature to prevent the inhomogeneity of the casting solution. In addition, the molecular weight, concentration and other parameter limitations of each component set in the present invention are based on the thermodynamic stability of poly-4-methyl-1-pentene as a consideration. Thermodynamic stability is a prerequisite for the preparation of high-performance hollow fiber membranes. The core of the present invention is an overall process design, including process steps and corresponding process parameters, which have their integrity and relevance, and the corresponding beneficial effects cannot be achieved if they are used separately.

[0018] The above-mentioned method for preparing a long-lasting anti-fouling and high-gas permeability poly-4-methyl-1-pentene membrane is to first dissolve it into a uniform solution by a high-temperature dissolution method of a thermotropic phase to achieve extrusion molding, and then use a surface coating method to give an ultra-thin separation layer, and enter a heat treatment to prepare a stable and high-performance hollow fiber membrane. The post-coating method used in the present invention can give the hollow fiber membrane a dense separation layer, solving the problem of blood leakage and fouling during application. Moreover, the curing process of the coated separation layer is placed in a solvent bath, which can reduce the volatilization rate of the solvent in the coating liquid, so that a relatively uniform, dense and defect-free separation layer can be formed, and the thickness can be adjusted, reducing the permeation resistance of the gas and improving the permeation efficiency of the gas. In addition, in order to ensure the firm bonding of the coating layer and the substrate, the present invention performs a heat treatment process. During the heat treatment process, as the temperature increases, the coated separation layer will fuse with the hollow fiber membrane to form an interlocking structure, so that it has high stability.

[0019] The present invention further improves the compatibility of the membrane with plasma during the application process by adding fluoride to the separation layer. In the traditional method, grafting macromolecules such as protein, heparin, and phosphorylcholine causes the pores to be easily blocked, resulting in a decrease in gas permeability. Perfluorocarbons are a class of chemically inert compounds with stable structure, corrosion resistance, poor solubility, insoluble in water, blood, oil, etc., high density, low surface tension, and no metabolism in the human body. Moreover, the compound has excellent solubility for non-polar gases, and its solubility for oxygen is more than 20 times that of water, 2-3 times that of whole blood, and more than 3 times that of carbon dioxide. The present invention adopts the method of adding fluoride to the separation layer to avoid the loss of gas permeability caused by grafting macromolecules, and to a certain extent improves the gas solubility and permeability rate; at the same time, it significantly improves the blood compatibility of the membrane and improves its application in ECMO. Moreover, the present invention forms a coating together with poly-4-methyl-1-pentene to fix it on the surface of the substrate, avoiding subsequent grafting, cross-linking and the like, greatly simplifying the fixation method of perfluorocarbon, and in the subsequent heat treatment process, the substance will also be embedded with the substrate together with the separation layer to form a whole with high stability. DETAILED DESCRIPTION

[0020] The present invention is described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Embodiment 1:

[0022] 1) At 220°C, 20 parts of poly-4-methyl-1-pentene with a weight average molecular weight of 180,000 and a distribution index of 2.0 are dissolved in 80 parts of a mixed diluent consisting of 60% dioctyl phthalate and 40% diisobutyl succinate. After being uniformly dissolved, the casting solution is degassed online, nitrogen is extruded through an inner hole with a diameter of 0.2 mm, and the casting solution is extruded through an outer hole with a diameter of 0.5 mm. The extrusion thickness of the casting solution is 0.15 mm. After being extruded into a hollow fiber shape, it is induced to phase separate and solidify in a mixed cooling bath of 70% triacetin and 30% glycerol at -20°C, and extracted and rinsed to obtain a hollow fiber membrane;

[0023] 2) 1 part of poly-4-methyl-1-pentene with a weight average molecular weight of 180,000 and a distribution index of 2.0, 1 part of heptafluorobutyric acid and 98 parts of cyclohexane were dissolved at room temperature to form a homogeneous solution, and then dip-coated on the surface of a clean hollow fiber membrane, and then placed in cyclohexane to induce the surface solvent to volatilize to form a 100 nanometer poly-4-methyl-1-pentene dense functional separation layer;

[0024] 3) The double-layer composite hollow fiber is placed in a muffle furnace and heat treated at 130°C for 2 hours to allow the two layers of polymer to be embedded in each other to form a tight composite layer, thereby obtaining a structurally stable and high-performance poly-4-methyl-1-pentene hollow fiber membrane.

[0025] Embodiment 2:

[0026] 1) At 250°C, 40 parts of poly-4-methyl-1-pentene with a weight average molecular weight of 230,000 and a distribution index of 3.4 were dissolved in 60 parts of a mixed diluent consisting of 80% dioctyl phthalate and 20% diisobutyl phthalate. After uniform dissolution, the casting solution was obtained by online degassing. Polyethylene glycol 200 was extruded through an inner hole with a diameter of 0.4 mm, and the casting solution was extruded through an outer hole with a diameter of 0.7 mm. The extrusion thickness of the casting solution was 0.15 mm. After being extruded into a hollow fiber shape, it was induced to phase separate and solidify in a mixed cooling bath of 80% triacetin and 20% polyethylene glycol 200 at 20°C. After extraction and rinsing, a hollow fiber membrane was obtained;

[0027] 2) 5 parts of poly-4-methyl-1-pentene with a weight average molecular weight of 230,000 and a distribution index of 3.4, 5 parts of 1H, 1H,2H-perfluoro-1-hexene and 90 parts of trichloroethylene were dissolved into a homogeneous solution at room temperature, and then dipped on the surface of a clean hollow fiber membrane, and then placed in trichloroethylene to induce the surface solvent to volatilize to form a 500 nanometer poly-4-methyl-1-pentene dense functional separation layer;

[0028] 3) The double-layer composite hollow fiber is placed in a muffle furnace and heat treated at 180°C for 6 hours to allow the two layers of polymer to be embedded in each other to form a tight composite layer, thereby obtaining a structurally stable and high-performance poly-4-methyl-1-pentene hollow fiber membrane.

[0029] Embodiment 3:

[0030] 1) At 230°C, 30 parts of poly-4-methyl-1-pentene with a weight average molecular weight of 200,000 and a distribution index of 2.8 were dissolved in 70 parts of a mixed diluent consisting of 70% dioctyl phthalate and 30% dibutyl sebacate. After being uniformly dissolved, the casting solution was degassed online, diethylene glycol was extruded through an inner hole with a diameter of 0.3 mm, and the casting solution was extruded through an outer hole with a diameter of 0.7 mm. The extrusion thickness of the casting solution was 0.2 mm. After being extruded into a hollow fiber shape, it was induced to phase separate and solidify in a mixed cooling bath of 50% polyethylene glycol 400 and 50% diethylene glycol at 10°C. After extraction and rinsing, a hollow fiber membrane was obtained;

[0031] 2) 3 parts of poly-4-methyl-1-pentene with a weight average molecular weight of 200,000 and a distribution index of 2.8, 4 parts of 1H, 1H,2H-perfluoro-1-hexene and 93 parts of cyclohexane were dissolved at room temperature to form a homogeneous solution, and then dip-coated on the surface of a clean hollow fiber membrane, and then placed in cyclohexane to induce the surface solvent to volatilize to form a 300 nanometer poly-4-methyl-1-pentene dense functional separation layer;

[0032] 3) The double-layer composite hollow fiber is placed in a muffle furnace and heat treated at 150°C for 4 hours to allow the two layers of polymer to be embedded in each other to form a tight composite layer, thereby obtaining a structurally stable and high-performance poly-4-methyl-1-pentene hollow fiber membrane.

[0033] Embodiment 4:

[0034] 1) At 220°C, 25 parts of poly-4-methyl-1-pentene with a weight average molecular weight of 215,000 and a distribution index of 3.2 were dissolved in 75 parts of a mixed diluent consisting of 65% dioctyl phthalate and 35% tri(2-ethylhexyl) trimellitate. After uniform dissolution, the casting solution was degassed online to obtain the casting solution. Polyethylene glycol 400 was extruded through an inner hole with a diameter of 0.2 mm, and the casting solution was extruded through an outer hole with a diameter of 0.7 mm. The extrusion thickness of the casting solution was 0.25 mm. After being extruded into a hollow fiber shape, it was induced to phase separate and solidify in a mixed cooling bath of 80% triacetin and 20% polyethylene glycol 200 at 0°C. After extraction and rinsing, the hollow fiber membrane was obtained;

[0035] 2) 2 parts of poly-4-methyl-1-pentene with a weight average molecular weight of 215,000 and a distribution index of 3.2, 3 parts of perfluorodecahydronaphthalene and 95 parts of trichloroethylene are dissolved at room temperature to form a homogeneous solution, and then dip-coated on the surface of a clean hollow fiber membrane, and then placed in trichloroethylene to induce the surface solvent to volatilize to form a 200 nanometer poly-4-methyl-1-pentene dense functional separation layer;

[0036] 3) The double-layer composite hollow fiber is placed in a muffle furnace and heat treated at 140°C for 3.5 hours to allow the two layers of polymer to be embedded in each other to form a tight composite layer, thereby obtaining a structurally stable and high-performance poly-4-methyl-1-pentene hollow fiber membrane.

[0037] Embodiment 5:

[0038] 1) At 250°C, 20 parts of poly-4-methyl-1-pentene with a weight average molecular weight of 230,000 and a distribution index of 3.4 were dissolved in 80 parts of a mixed diluent consisting of 60% dioctyl phthalate and 40% diisobutyl phthalate. After uniform dissolution, the casting solution was degassed online, triethylene glycol was extruded through an inner hole with a diameter of 0.3 mm, and the casting solution was extruded through an outer hole with a diameter of 0.6 mm. The extrusion thickness of the casting solution was 0.15 mm. After being extruded into a hollow fiber shape, it was induced to phase separate and solidify in a mixed cooling bath of 50% polyethylene glycol 400 and 50% diethylene glycol at -5°C. After extraction and rinsing, a hollow fiber membrane was obtained;

[0039] 2) 4.5 parts of poly (4-methyl-1-pentene) with a weight average molecular weight of 230,000 and a distribution index of 3.4, 3 parts of perfluoropentane and 92.5 parts of trichloroethylene were dissolved at room temperature to form a homogeneous solution, and then dip-coated on the surface of a clean hollow fiber membrane, and then placed in cyclohexane to induce the surface solvent to volatilize to form a 300 nanometer poly (4-methyl-1-pentene) dense functional separation layer;

[0040] 3) The double-layer composite hollow fiber is placed in a muffle furnace and heat treated at 160°C for 5 hours to allow the two layers of polymer to be embedded in each other to form a tight composite layer, thereby obtaining a structurally stable and high-performance poly-4-methyl-1-pentene hollow fiber membrane.

[0041] Embodiment 6:

[0042] 1) At 220°C, 40 parts of poly-4-methyl-1-pentene with a weight average molecular weight of 185,000 and a distribution index of 2.5 were dissolved in 60 parts of a mixed diluent consisting of 75% dioctyl phthalate and 25% dibutyl sebacate. After being uniformly dissolved, the casting solution was degassed online, polyethylene glycol 400 was extruded through an inner hole with a diameter of 0.2 mm, and the casting solution was extruded through an outer hole with a diameter of 0.5 mm. The extrusion thickness of the casting solution was 0.15 mm. After being extruded into a hollow fiber shape, it was induced to phase separate and solidify in a mixed cooling bath of 70% triacetin and 30% glycerol at 10°C. After extraction and rinsing, a hollow fiber membrane was obtained;

[0043] 2) 3 parts of poly-4-methyl-1-pentene with a weight average molecular weight of 185,000 and a distribution index of 2.5, 3 parts of chloroperfluorooctane and 90 parts of a mixed solvent consisting of 50% cyclohexane and 50% trichloroethylene are dissolved at room temperature to form a homogeneous solution, and then dip-coated on the surface of a clean hollow fiber membrane, and then placed in cyclohexane to induce the surface solvent to volatilize to form a 260 nanometer poly-4-methyl-1-pentene dense functional separation layer;

[0044] 3) The double-layer composite hollow fiber is placed in a muffle furnace and heat treated at 150°C for 5 hours to allow the two layers of polymer to be embedded in each other to form a tight composite layer, thereby obtaining a structurally stable and high-performance poly-4-methyl-1-pentene hollow fiber membrane.

[0045] The beneficial effects of the present invention are further demonstrated by corresponding test data below. Tables 1 to 3 are performance test tables of the poly 4-methyl-1-pentene hollow fiber membranes prepared in Examples 1, 2 and 6 of the present invention, respectively.

[0046] Table 1 Performance of poly 4-methyl-1-pentene hollow fiber membrane of Example 1

[0047] Poly (4-methyl-1-pentene) hollow fiber membrane index <![CDATA[O2 Permeation Rate]]> <![CDATA[124mL min -1 cm -2 bar -1 ]]> <![CDATA[CO2 Permeation Rate]]> <![CDATA[89mL min -1 cm -2 bar -1 ]]> BSA adsorption <![CDATA[12.5μg / cm 3 ]]> Bleeding time 85 hours Tensile Strength 0.65N Elongation at break 200%

[0048] Table 2 Performance of poly 4-methyl-1-pentene hollow fiber membrane of Example 2

[0049] Poly (4-methyl-1-pentene) hollow fiber membrane index <![CDATA[O2 permeation rate]]> <![CDATA[62mL min -1 cm -2 bar -1 ]]> <![CDATA[CO2 permeation rate]]> <![CDATA[54 mL min -1 cm -2 bar -1 ]]> BSA adsorption <![CDATA[20 μg / cm 3 ]]> Bleeding time 150 hours Tensile Strength 3N Elongation at break 260%

[0050] Table 3 Performance of poly 4-methyl-1-pentene hollow fiber membrane of Example 6

[0051] Poly (4-methyl-1-pentene) hollow fiber membrane index <![CDATA[O2 permeation rate]]> <![CDATA[86mL min -1 cm -2 bar -1 ]]> <![CDATA[CO2 Permeation Rate]]> <![CDATA[72 mL min -1 cm -2 bar -1 ]]> BSA adsorption <![CDATA[15μg / cm 3 ]]> Bleeding time 120 hours Tensile Strength 1.5 N Elongation at break 230%

[0052] In Table 1: The O2 permeation rate of the fiber membrane of Example 1 is 124 mL min -1 cm -2 bar -1 , CO2 permeation rate is 89mLmin -1 cm -2 bar -1 , the adsorption capacity of bovine serum albumin is 12.5 μg / cm 3 , bleeding time 85 hours, tensile strength 0.65N, elongation at break 200%.

[0053] In Table 2: The O2 permeation rate of the fiber membrane of Example 2 is 62 mL min -1 cm -2 bar -1 , CO2 permeation rate is 54 mLmin -1 cm -2 bar -1 , the adsorption capacity of bovine serum albumin is 20 μg / cm 3 , blood leakage time 150 hours, tensile strength 3N, elongation at break 260%.

[0054] In Table 3: The O2 permeation rate of the fiber membrane of Example 6 is 86 mL min -1 cm -2 bar -1, CO2 permeation rate is 72 mLmin -1 cm -2 bar -1 , the adsorption capacity of bovine serum albumin is 15 μg / cm 3 , bleeding time 120 hours, tensile strength 1.5N, elongation at break 230%.

[0055] It can be seen from Tables 1 to 3 that the comprehensive performance of the hollow fiber membranes prepared in Examples 1, 2 and 6 of the present invention is relatively excellent, among which the oxygen permeation flux of the membrane fiber of Example 1 is the best, reaching 124 mL min -1 cm -2 bar -1 ; The membrane strength of Example 2 reaches 3N; The protein adsorption performance of Example 2 is 20μg / cm 3 , the blood leakage time is increased to 150 hours. The hollow fiber membranes prepared in Examples 3-5 of the present invention are tested for performance, and the excellent comprehensive performance described in the present invention can also be achieved. The poly 4-methyl-1-pentene hollow fiber membrane prepared by the present invention has good gas permeability and anti-fouling and blocking performance, and can be efficiently used in oxygenators.

[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane, characterized in that The following steps are involved: 1) Dissolve 20-40 parts of poly-4-methyl-1-pentene in 60-80 parts of diluent at 220-250°C, degas online to obtain casting solution after uniform dissolution, extrude through a two-hole spinneret, the inner hole flows into the core solution, and the outer hole flows into the casting solution, and after forming, phase separation and solidification occur in a cooling bath, and after extraction and rinsing, a hollow fiber membrane is obtained; 2) dissolving 1-5 parts of poly-4-methyl-1-pentene, 1-5 parts of fluoride and 90-98 parts of alkane solvent at room temperature into a homogeneous solution, wherein the fluoride is at least one of heptafluorobutyric acid, heptafluorobutanol, 1H, 1H, 2H-perfluoro-1-hexene, perfluoropentane, perfluorodecahydronaphthalene and chloroperfluorooctane; dipping the solution on the surface of a clean hollow fiber membrane, and then placing the membrane in a solvent bath to induce volatilization of the surface solvent, thereby reducing the volatilization rate of the solvent in the coating solution and forming an ultra-thin dense functional separation layer of poly-4-methyl-1-pentene; 3) The double-layer composite hollow fiber is placed in a muffle furnace for heat treatment, so that the two layers of polymer are embedded in each other to form a tight composite layer, thereby obtaining a poly-4-methyl-1-pentene hollow fiber membrane.

2. The method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane according to claim 1, characterized in that In step 1), the dissolving temperature is 230-240° C., 25-30 parts of poly-4-methyl-1-pentene, and 65-75 parts of diluent.

3. The method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane according to claim 1, characterized in that In step 1), the weight average molecular weight of the poly-4-methyl-1-pentene is between 180,000 and 230,000, and the molecular weight distribution index is between 2.0 and 3.

4.

4. The method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane according to claim 1, characterized in that In step 1), the diluent is composed of two solvents, one of which is fixed as dioctyl phthalate, with a content of 60-80%, and the other solvent is one or two of diisobutyl phthalate, diisobutyl phthalate, tri(2-ethylhexyl) trimellitate, and dibutyl phthalate, with a content of 20%-40%.

5. The method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane according to claim 1, characterized in that In step 1), the inner hole diameter of the spinneret is 0.2-0.4 mm, the extrusion diameter of the casting solution is 0.5-0.7 mm, and the size of the slit is controlled to be no less than 0.15 mm.

6. The method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane according to claim 1, characterized in that In step 1), the core liquid is one of nitrogen, polyethylene glycol 200, diethylene glycol, triethylene glycol and polyethylene glycol 400; the cooling bath is one of a mixture of 70% triacetin and 30% glycerol, 80% triacetin and 20% polyethylene glycol 200, 50% polyethylene glycol 400 and 50% diethylene glycol; the temperature of the cooling bath is -20-20°C.

7. The method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane according to claim 1, characterized in that In step 2), the ultra-thin thickness of the poly-4-methyl-1-pentene dense functional separation layer is 100 nanometers to 500 nanometers.

8. The method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane according to claim 1, characterized in that In step 3), the heat treatment temperature is 130-180°C and the heat treatment time is 2-6 hours.

9. Application of the method for preparing a long-lasting anti-fouling and high gas permeability poly-4-methyl-1-pentene membrane as described in claim 1 in ECMO membranes.

Citation Information

Patent Citations

  • Modification method for carrying out gaseous polyfluoride grafting on surfaces of membrane type artificial lungs by utilizing low-temperature plasma technology

    CN109157988A

  • Hollow fiber membrane as well as preparation method and application thereof

    CN117771970A