A kind of amorphous powder resistant to friction and wear and its preparation method
By combining Zr-based amorphous alloy powder with SiC coating layer, the hardness and adhesion problems of amorphous powder in high friction and high wear environments are solved, and the friction and wear resistance and oxidation resistance are improved, which is suitable for in manufacturing, automotive, aerospace and other fields.
Patent Information
- Application Number
- CN202410913964.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Existing amorphous powders have low surface hardness and insufficient adhesion in high friction and high wear environments, and are susceptible to oxidation reactions, resulting in reduced performance and limiting their applications in manufacturing, automobiles, aerospace and other fields.
The Zr-based amorphous alloy powder is combined with the SiC coating layer, and the Zr-based amorphous alloy powder is prepared by high-pressure argon atomization method, and the SiC coating layer is prepared by vapor phase chemical deposition on its surface to form a shell-core structure to improve the hardness. and antioxidant properties.
It significantly improves the friction and wear resistance and service life of amorphous powder, enhances the stability and anti-oxidation performance in high temperature environments, and extends the use temperature and performance maintenance time.
Smart Images

Figure CN118477997B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of amorphous alloy materials, in particular to abrasion-resistant amorphous powder and a preparation method thereof. Background Art
[0002] With the development of industrial technology, the demand for new high-performance materials in the field of materials science is increasing. In many application fields, wear resistance is a crucial aspect of material performance, especially in manufacturing, automobiles, aerospace, energy and electronics. In order to meet the increasing demand for wear resistance, amorphous alloys have become one of the research hotspots. Amorphous is the fourth most common state of matter in nature after gas, liquid and solid. Common amorphous materials include glass, rubber, asphalt and plastic. The structure of amorphous materials has the characteristics of long-range disorder and short-range order. There are no crystal defects such as vacancies and dislocations in amorphous materials, and there are no problems of component segregation and second phases, which lays a structural foundation for the excellent performance of amorphous materials. In the field of metal materials, amorphous alloys not only have the characteristics of amorphous substances, but also have inherent metal properties such as thermal conductivity and electrical conductivity, as well as unique properties such as mechanical properties and electromagnetic properties. Among them, although the friction and wear resistance of amorphous alloys is higher than that of traditional metal materials, they may still face surface wear and damage in high friction and high wear environments. At the same time, the insufficient glass-forming ability of amorphous alloys leads to limited critical size, which hinders their further development and application. The preparation of a friction and wear resistant amorphous powder has become an effective way to solve this problem.
[0003] The amorphous powder prepared in the prior art still has a low surface hardness, which makes it difficult to meet the requirements in a high-friction environment. It is easily worn and damaged under high-load and high-speed conditions, resulting in performance degradation. At the same time, if the amorphous powder is prepared into a coating, there are also problems such as insufficient adhesion and easy falling off. Secondly, the amorphous powder will undergo oxidation reaction in a high temperature or high humidity environment, which accelerates the occurrence of surface wear and reduces its service life and comprehensive performance. Therefore, it is necessary to explore and develop new friction and wear resistant amorphous alloy materials and amorphous powder preparation technologies. Summary of the invention
[0004] The invention provides a friction and wear resistant amorphous powder and a preparation method thereof. The amorphous powder consists of a Zr-based amorphous alloy powder and a SiC coating layer. The Zr-based amorphous alloy consists of Zr, W, Nb, Ti, Cu, Ni, Mn and rare earth metals. Zr is used as a main element. The raw materials are first melted to obtain a master alloy. The Zr-based amorphous alloy powder is then prepared by a high-pressure argon atomization method. Finally, the SiC coating layer is prepared on the surface of the Zr-based amorphous powder by gas phase chemical deposition to obtain a friction and wear resistant amorphous powder. The amorphous powder has excellent friction and wear resistance. In addition, due to the presence of the SiC coating layer, the hardness of the Zr-based amorphous alloy powder is improved while avoiding exposure of the Zr-based amorphous alloy powder to the environment. In a high-temperature environment, the occurrence of oxidation wear is alleviated.
[0005] In order to achieve the above technical goals, the following technical solutions are adopted:
[0006] A friction and wear resistant amorphous powder is composed of a Zr-based amorphous alloy powder and a SiC coating layer;
[0007] The Zr-based amorphous alloy powder includes the following chemical composition in atomic percentage: Zr 23.4%~45.8%, W15.8%~22.1%, Nb 7.1%~10.9%, Ti 8.7%~12.3%, Cu 6.3%~10.6%, Ni 5.9%~8.0%, Mn 10.1%~10.3%, RE 0.05%~2.1%, and the rest are unavoidable impurities;
[0008] RE is a rare earth metal, which is one of Rd, Ce, Pr, and Y, with a purity of 99%. Zr, W, Nb, Ti, Cu, Ni, and Mn are made of zirconium powder, tungsten powder, niobium powder, copper powder, nickel powder, manganese powder with a purity of 99.9%, and titanium powder with a purity of 99.6%, respectively.
[0009] The SiC coating layer is prepared on the surface of the Zr-based amorphous alloy powder by thermally decomposing methyltrichlorosilane and then vapor-phase chemical deposition. The mass fraction ratio of methyltrichlorosilane to the Zr-based amorphous alloy powder is 2:1, and the purity of the methyltrichlorosilane is 99%.
[0010] Furthermore, the preparation of Zr-based amorphous alloy powder includes the following steps:
[0011] P1, according to the chemical composition of the Zr-based amorphous alloy powder, weigh the corresponding mass of zirconium powder, tungsten powder, niobium powder, copper powder, nickel powder, manganese powder, titanium powder and rare earth metal according to atomic percentage, first melt the zirconium powder, tungsten powder and niobium powder in a vacuum arc melting furnace to obtain a Zr-W-Nb alloy melt;
[0012] P2, adding copper powder, nickel powder, manganese powder, titanium powder and rare earth metals to the Zr-W-Nb alloy melt obtained in step P1 in sequence, and melting the mixture in a vacuum arc melting furnace to obtain a liquid alloy;
[0013] P3, using the liquid alloy prepared in step P2 as the master alloy for high-pressure argon atomization, evacuating the atomization chamber, flushing it with argon for 3 times, and then filling it with argon as the atomization medium, keeping the master alloy under an argon pressure of 25-35 bar for 5 minutes, continuously heating it to the atomization temperature, and continuously spraying the master alloy through the injection nozzle, colliding with the argon gas flow to disperse into small droplets, and finally solidifying to obtain the Zr-based amorphous alloy powder.
[0014] Preferably, the vacuum degree of the vacuum arc melting furnace in step P1 is 10 -2 Pa, melting temperature is 3400~3600℃, melting time is 10~20min.
[0015] Preferably, the vacuum degree of the vacuum arc melting furnace in step P2 is 10 -2 Pa, melting temperature is 3000~3300℃, melting time is 5~10min.
[0016] Preferably, in step P3, the atomization temperature is 2500-3000K, the atomization pressure is 3.5MPa, the atomization medium is high-purity argon gas with a purity of 99.99%, and the nozzle diameter is 50-150μm.
[0017] Furthermore, the preparation of the friction and wear resistant amorphous powder comprises the following steps:
[0018] S1, placing Zr-based amorphous alloy powder in a crucible, and heating the reaction chamber to a deposition temperature of vapor phase chemical deposition;
[0019] S2 and H2 are used as carrier gas and dilution gas at the same time, and Ar is used only as dilution gas. When the reaction chamber reaches the deposition temperature, methyltrichlorosilane is transported into the reaction chamber through a mixture of H2 and Ar. Methyltrichlorosilane is pyrolyzed into SiC and HCl, and vapor phase chemical deposition is performed to obtain a Zr-based amorphous alloy powder with a SiC coating layer.
[0020] S3, after cooling to room temperature, collecting the Zr-based amorphous alloy powder with a SiC coating layer prepared in step S2, washing with deionized water and anhydrous ethanol in turn, and drying in an oven at 80° C. for 20 minutes to obtain the friction and wear resistant amorphous powder.
[0021] Preferably, the gas flow rate of Ar as a dilution gas is 90-300 sccm, the gas flow rates of H2 as a dilution gas and a carrier gas are 30-100 sccm and 45-200 sccm respectively, and the material flow rate of methyltrichlorosilane is 70-75 sccm.
[0022] Preferably, the deposition temperature of the vapor phase chemical deposition is 950-1100° C., and the deposition time is 30-120 min.
[0023] The beneficial effects obtained by the present invention are as follows:
[0024] The present invention proposes a kind of amorphous powder resistant to friction and wear and a preparation method thereof, wherein the amorphous powder is composed of two parts: a Zr-based amorphous alloy powder and a SiC coating layer. Firstly, the Zr-based amorphous alloy powder is composed of Zr, W, Nb, Ti, Cu, Ni, Mn and rare earth metals, wherein Zr as the main element accounts for a large proportion in the composition, and the content of W is also relatively high. This is a Zr-based high-W amorphous alloy powder. In its chemical composition, Zr, W and Nb all have high hardness and wear resistance, and W and Nb can still maintain excellent wear resistance in high temperature and high load environments. The synergy of these components helps to improve the hardness and wear resistance of the prepared amorphous alloy powder itself; secondly, the amorphous alloy powder is prepared by high-pressure argon atomization method, and the obtained amorphous alloy powder has uniform particle size, smooth surface and good sphericity. The doping of a small amount of rare earth metal helps to promote the formation of amorphous phase, so that a relatively stable amorphous structure is formed in the amorphous alloy, which is more in line with the requirements of gas atomization powder making; finally, by gas phase chemical deposition A SiC coating layer is deposited on the surface of the prepared Zr-based amorphous alloy powder. On the one hand, the SiC coating can form a core-shell structure with the Zr-based amorphous alloy powder, and the Zr-based amorphous alloy powder is wrapped in the SiC layer. A stable oxide layer is generated on the SiC surface, which has high oxidation resistance and a slow oxidation rate. It can avoid or alleviate the oxygen erosion of the Zr-based amorphous alloy, alleviate the oxidation wear rate of the Zr-based amorphous alloy powder under some working conditions, and is beneficial to improving the service life. On the other hand, the inherent high hardness, high wear resistance and thermal shock resistance of SiC are utilized, which not only improves the friction and wear resistance of the Zr-based amorphous alloy powder, but also increases its use temperature, so that the obtained amorphous powder can maintain good performance under high temperature conditions, and alleviate the damage and wear caused by extreme working conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions therein, the following briefly introduces the drawings required for use in the descriptions of the embodiments and comparative examples. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0026] Figure 1 A comparison diagram of particle size distribution of the amorphous powder prepared in Example 3 and the Zr-based amorphous alloy powder prepared in Comparative Example 1;
[0027] Figure 2 The final mass gain diagram of each embodiment and comparative example sample after high temperature oxidation under different conditions;
[0028] Figure 3 The effect of SiC coating on the final mass gain of the sample after high-temperature oxidation;
[0029] Figure 4 The friction and wear resistance test results of the samples of various embodiments and comparative examples at room temperature are shown. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The described embodiments are part of the embodiments of the present invention, but not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1: A friction and wear resistant amorphous powder is composed of a Zr-based amorphous alloy powder and a SiC coating layer, wherein the SiC coating layer is prepared on the surface of the Zr-based amorphous alloy by vapor phase chemical deposition;
[0032] The preparation of Zr-based amorphous alloy powder comprises the following steps:
[0033] P1, Zr-based amorphous alloy powder includes the following chemical composition in atomic percentage: Zr 23.4%, W 22.1%, Nb 10.9%, Ti 12.3%, Cu 10.6%, Ni 8.0%, Mn 10.3%, Ce 2.1%, and the rest are unavoidable impurities. According to the atomic percentage, zirconium powder, tungsten powder, niobium powder, copper powder, nickel powder, manganese powder with a purity of 99.9%, titanium powder with a purity of 99.6% and cerium powder with a purity of 99% are weighed, and the zirconium powder, tungsten powder and niobium powder are first melted in a vacuum arc melting furnace, and the vacuum degree of the vacuum arc melting furnace is 10 -2Pa, melting temperature is 3400℃, melting time is 15min, and Zr-W-Nb alloy melt is obtained;
[0034] P2, copper powder, nickel powder, manganese powder, titanium powder and rare earth metal are added to the Zr-W-Nb alloy melt obtained in step P1 in sequence, and the mixture is melted in a vacuum arc melting furnace, wherein the vacuum degree of the vacuum arc melting furnace is 10 -2 Pa, melting temperature is 3000℃, melting time is 8min, and liquid alloy is obtained;
[0035] P3, using the liquid alloy prepared in step P2 as the master alloy for high-pressure argon atomization, evacuating the atomization chamber to vacuum, flushing with argon for 3 times, and then filling with argon as the atomization medium, keeping the master alloy under an argon pressure of 30 bar for 5 minutes, and continuously heating to the atomization temperature, the atomization temperature is 2750K, the atomization pressure is 3.5 MPa, the argon is high-purity argon with a purity of 99.99%, and the master alloy is continuously sprayed through a spray nozzle with a nozzle diameter of 100 μm, colliding with the argon gas flow to disperse into small droplets, and finally solidifying to obtain the Zr-based amorphous alloy powder.
[0036] The method for preparing the friction and wear resistant amorphous powder comprises the following steps:
[0037] S1, placing Zr-based amorphous alloy powder in a crucible, and heating the reaction chamber to a deposition temperature of vapor phase chemical deposition, which is 1050° C.;
[0038] S2, H2 is used as both a carrier gas and a dilution gas, and Ar is used only as a dilution gas. When the reaction chamber reaches a deposition temperature, methyltrichlorosilane is delivered to the reaction chamber through a mixture of H2 and Ar. The gas flow rate of Ar as a dilution gas is 195 sccm, and the gas flow rates of H2 as a dilution gas and a carrier gas are 65 sccm and 130 sccm, respectively. The material flow rate of methyltrichlorosilane is 70 sccm. The mass fraction ratio of methyltrichlorosilane to Zr-based amorphous alloy powder is 2:1. Methyltrichlorosilane is pyrolyzed into SiC and HCl, and vapor phase chemical deposition is performed. The deposition time is 90 min to obtain a Zr-based amorphous alloy powder with a SiC coating layer.
[0039] S3, after cooling to room temperature, collecting the Zr-based amorphous alloy powder with a SiC coating layer prepared in step S2, washing with deionized water and anhydrous ethanol in turn, and drying in an oven at 80° C. for 20 minutes to obtain the friction and wear resistant amorphous powder.
[0040] Example 2: A friction and wear resistant amorphous powder is composed of a Zr-based amorphous alloy powder and a SiC coating layer, wherein the SiC coating layer is prepared on the surface of the Zr-based amorphous alloy by vapor phase chemical deposition;
[0041] The preparation of Zr-based amorphous alloy powder comprises the following steps:
[0042] P1, Zr-based amorphous alloy powder includes the following chemical composition in atomic percentage: Zr 30.5%, W 21.5%, Nb 10.2%, Ti 10.5%, Cu 8.4%, Ni 6.9%, Mn 10.2%, Ce 1.6%, and the rest are unavoidable impurities. According to the atomic percentage, zirconium powder, tungsten powder, niobium powder, copper powder, nickel powder, manganese powder with a purity of 99.9%, titanium powder with a purity of 99.6% and cerium powder with a purity of 99% are weighed, and the zirconium powder, tungsten powder and niobium powder are first melted in a vacuum arc melting furnace, and the vacuum degree of the vacuum arc melting furnace is 10 -2 Pa, melting temperature is 3450℃, melting time is 15min, and Zr-W-Nb alloy melt is obtained;
[0043] P2, copper powder, nickel powder, manganese powder, titanium powder and rare earth metal are added to the Zr-W-Nb alloy melt obtained in step P1 in sequence, and the mixture is melted in a vacuum arc melting furnace, wherein the vacuum degree of the vacuum arc melting furnace is 10 -2 Pa, melting temperature is 3100℃, melting time is 8min, and liquid alloy is obtained;
[0044] P3, using the liquid alloy prepared in step P2 as the master alloy for high-pressure argon atomization, evacuating the atomization chamber to vacuum, flushing with argon for 3 times, and then filling with argon as the atomization medium, keeping the master alloy under an argon pressure of 30 bar for 5 minutes, and continuously heating to the atomization temperature, the atomization temperature is 2750K, the atomization pressure is 3.5 MPa, the argon is high-purity argon with a purity of 99.99%, and the master alloy is continuously sprayed through a spray nozzle with a nozzle diameter of 100 μm, colliding with the argon gas flow to disperse into small droplets, and finally solidifying to obtain the Zr-based amorphous alloy powder.
[0045] The preparation method of the friction and wear resistant amorphous powder is consistent with that in Example 1.
[0046] Example 3: A friction and wear resistant amorphous powder is composed of a Zr-based amorphous alloy powder and a SiC coating layer, wherein the SiC coating layer is prepared on the surface of the Zr-based amorphous alloy by vapor phase chemical deposition;
[0047] The preparation of Zr-based amorphous alloy powder comprises the following steps:
[0048] P1, Zr-based amorphous alloy powder includes the following chemical composition in atomic percentage: Zr 34.6%, W 18.9%, Nb 8.9%, Ti 10.5%, Cu 8.4%, Ni 6.9%, Mn 10.2%, Ce 1.1%, and the rest are unavoidable impurities. According to the atomic percentage, zirconium powder, tungsten powder, niobium powder, copper powder, nickel powder, manganese powder with a purity of 99.9%, titanium powder with a purity of 99.6% and cerium powder with a purity of 99% are weighed, and the zirconium powder, tungsten powder and niobium powder are first melted in a vacuum arc melting furnace, and the vacuum degree of the vacuum arc melting furnace is 10 -2 Pa, melting temperature is 3500℃, melting time is 15min, and Zr-W-Nb alloy melt is obtained;
[0049] P2, copper powder, nickel powder, manganese powder, titanium powder and rare earth metal are added to the Zr-W-Nb alloy melt obtained in step P1 in sequence, and the mixture is melted in a vacuum arc melting furnace, wherein the vacuum degree of the vacuum arc melting furnace is 10 -2 Pa, melting temperature is 3150℃, melting time is 8min, and liquid alloy is obtained;
[0050] P3, using the liquid alloy prepared in step P2 as the master alloy for high-pressure argon atomization, evacuating the atomization chamber to vacuum, flushing with argon for 3 times, and then filling with argon as the atomization medium, keeping the master alloy under an argon pressure of 30 bar for 5 minutes, and continuously heating to the atomization temperature, the atomization temperature is 2750K, the atomization pressure is 3.5 MPa, the argon is high-purity argon with a purity of 99.99%, and the master alloy is continuously sprayed through a spray nozzle with a nozzle diameter of 100 μm, colliding with the argon gas flow to disperse into small droplets, and finally solidifying to obtain the Zr-based amorphous alloy powder.
[0051] The preparation method of the friction and wear resistant amorphous powder is consistent with that in Example 1.
[0052] Example 4: A friction and wear resistant amorphous powder is composed of a Zr-based amorphous alloy powder and a SiC coating layer, wherein the SiC coating layer is prepared on the surface of the Zr-based amorphous alloy by vapor phase chemical deposition;
[0053] The preparation of Zr-based amorphous alloy powder comprises the following steps:
[0054] P1, Zr-based amorphous alloy powder includes the following chemical composition in atomic percentage: Zr 38.8%, W 16.9%, Nb 7.5%, Ti 10.5%, Cu 8.4%, Ni 6.9%, Mn 10.2%, Ce 0.65%, and the rest are unavoidable impurities. According to the atomic percentage, zirconium powder, tungsten powder, niobium powder, copper powder, nickel powder, manganese powder with a purity of 99.9%, titanium powder with a purity of 99.6% and cerium powder with a purity of 99% are weighed, and the zirconium powder, tungsten powder and niobium powder are first melted in a vacuum arc melting furnace, and the vacuum degree of the vacuum arc melting furnace is 10 -2 Pa, melting temperature is 3550℃, melting time is 15min, and Zr-W-Nb alloy melt is obtained;
[0055] P2, copper powder, nickel powder, manganese powder, titanium powder and rare earth metal are added to the Zr-W-Nb alloy melt obtained in step P1 in sequence, and the mixture is melted in a vacuum arc melting furnace, wherein the vacuum degree of the vacuum arc melting furnace is 10 -2 Pa, melting temperature is 3200℃, melting time is 8min, and liquid alloy is obtained;
[0056] P3, using the liquid alloy prepared in step P2 as the master alloy for high-pressure argon atomization, evacuating the atomization chamber to vacuum, flushing with argon for 3 times, and then filling with argon as the atomization medium, keeping the master alloy under an argon pressure of 30 bar for 5 minutes, and continuously heating to the atomization temperature, the atomization temperature is 2750K, the atomization pressure is 3.5 MPa, the argon is high-purity argon with a purity of 99.99%, and the master alloy is continuously sprayed through a spray nozzle with a nozzle diameter of 100 μm, colliding with the argon gas flow to disperse into small droplets, and finally solidifying to obtain the Zr-based amorphous alloy powder.
[0057] The preparation method of the friction and wear resistant amorphous powder is consistent with that in Example 1.
[0058] Example 5: A friction and wear resistant amorphous powder is composed of a Zr-based amorphous alloy powder and a SiC coating layer, wherein the SiC coating layer is prepared on the surface of the Zr-based amorphous alloy by vapor phase chemical deposition;
[0059] The preparation of Zr-based amorphous alloy powder comprises the following steps:
[0060] P1, Zr-based amorphous alloy powder includes the following chemical composition in atomic percentage: Zr 45.8%, W 15.8%, Nb 7.1%, Ti 8.7%, Cu 6.3%, Ni 5.9%, Mn 10.1%, Ce 0.05%, and the rest are unavoidable impurities. According to the atomic percentage, zirconium powder, tungsten powder, niobium powder, copper powder, nickel powder, manganese powder with a purity of 99.9%, titanium powder with a purity of 99.6% and cerium powder with a purity of 99% are weighed, and the zirconium powder, tungsten powder and niobium powder are first melted in a vacuum arc melting furnace, and the vacuum degree of the vacuum arc melting furnace is 10 -2 Pa, melting temperature is 3600℃, melting time is 15min, and Zr-W-Nb alloy melt is obtained;
[0061] P2, copper powder, nickel powder, manganese powder, titanium powder and rare earth metal are added to the Zr-W-Nb alloy melt obtained in step P1 in sequence, and the mixture is melted in a vacuum arc melting furnace, wherein the vacuum degree of the vacuum arc melting furnace is 10 -2 Pa, melting temperature is 3300 °C, melting time is 8 min, and liquid alloy is obtained;
[0062] P3, using the liquid alloy prepared in step P2 as the master alloy for high-pressure argon atomization, evacuating the atomization chamber to vacuum, flushing with argon for 3 times, and then filling with argon as the atomization medium, keeping the master alloy under an argon pressure of 30 bar for 5 minutes, and continuously heating to the atomization temperature, the atomization temperature is 2750K, the atomization pressure is 3.5 MPa, the argon is high-purity argon with a purity of 99.99%, and the master alloy is continuously sprayed through a spray nozzle with a nozzle diameter of 100 μm, colliding with the argon gas flow to disperse into small droplets, and finally solidifying to obtain the Zr-based amorphous alloy powder.
[0063] Example 6: The preparation of Zr-based amorphous alloy powder is consistent with Example 3.
[0064] The method for preparing the friction and wear resistant amorphous powder comprises the following steps:
[0065] S1, placing Zr-based amorphous alloy powder in a crucible, and heating the reaction chamber to a deposition temperature of vapor phase chemical deposition, which is 950° C.;
[0066] S2, H2 is used as both a carrier gas and a dilution gas, and Ar is used only as a dilution gas. When the reaction chamber reaches a deposition temperature, methyltrichlorosilane is delivered to the reaction chamber through a mixture of H2 and Ar. The gas flow rate of Ar as a dilution gas is 195 sccm, and the gas flow rates of H2 as a dilution gas and a carrier gas are 65 sccm and 130 sccm, respectively. The material flow rate of methyltrichlorosilane is 70 sccm. The mass fraction ratio of methyltrichlorosilane to Zr-based amorphous alloy powder is 2:1. Methyltrichlorosilane is pyrolyzed into SiC and HCl, and vapor phase chemical deposition is performed. The deposition time is 120 min to obtain a Zr-based amorphous alloy powder with a SiC coating layer.
[0067] S3, after cooling to room temperature, collecting the Zr-based amorphous alloy powder with a SiC coating layer prepared in step S2, washing with deionized water and anhydrous ethanol in turn, and drying in an oven at 80° C. for 20 minutes to obtain the friction and wear resistant amorphous powder.
[0068] Example 7: The preparation of Zr-based amorphous alloy powder is consistent with Example 3.
[0069] The method for preparing the friction and wear resistant amorphous powder comprises the following steps:
[0070] S1, placing Zr-based amorphous alloy powder in a crucible, and heating the reaction chamber to a deposition temperature of vapor phase chemical deposition, which is 1100° C.;
[0071] S2, H2 is used as both a carrier gas and a dilution gas, and Ar is used only as a dilution gas. When the reaction chamber reaches a deposition temperature, methyltrichlorosilane is delivered to the reaction chamber through a mixture of H2 and Ar. The gas flow rate of Ar as a dilution gas is 195 sccm, and the gas flow rates of H2 as a dilution gas and a carrier gas are 65 sccm and 130 sccm, respectively. The material flow rate of methyltrichlorosilane is 70 sccm. The mass fraction ratio of methyltrichlorosilane to Zr-based amorphous alloy powder is 2:1. Methyltrichlorosilane is pyrolyzed into SiC and HCl, and vapor phase chemical deposition is performed. The deposition time is 90 min to obtain a Zr-based amorphous alloy powder with a SiC coating layer.
[0072] S3, after cooling to room temperature, collecting the Zr-based amorphous alloy powder with a SiC coating layer prepared in step S2, washing with deionized water and anhydrous ethanol in turn, and drying in an oven at 80° C. for 20 minutes to obtain the friction and wear resistant amorphous powder.
[0073] Comparative Example 1:
[0074] Based on Example 3, the difference is that the SiC coating layer is not prepared, and the remaining steps are consistent with Example 3.
[0075] Comparative Example 2:
[0076] Based on Example 3, the difference is that the W element is not added during the preparation of the Zr-based amorphous alloy powder, and the remaining steps are consistent with Example 3.
[0077] Experimental example:
[0078] 1. Particle size analysis:
[0079] The particle size distribution of Zr-based amorphous alloy powder and amorphous powder was tested by a laser particle size analyzer, the medium was deionized water, and the dispersion mode was wet method.
[0080] The particle size distribution of the amorphous powder prepared in Example 3 and the Zr-based amorphous alloy powder prepared in Comparative Example 1 is as follows: Figure 1 shown.
[0081] 2. Friction and wear resistance test:
[0082] The amorphous powder was sprayed onto the surface of the substrate using HVOF technology to obtain an amorphous coating. The surface of the amorphous coating was polished to a mirror surface with 800-2500 mesh sandpaper, and then cleaned in anhydrous ethanol with an ultrasonic machine until it was free of dirt. The sample was cut into 15mm×15mm×5mm, and the friction and wear resistance of the amorphous alloy coating was tested using an SFT-2M pin-disc friction and wear tester and an MFT-4000 reciprocating friction and wear tester. The pin-disc friction test was carried out at room temperature, with a grinding ball of Φ4mm Si3N4 ball, a load of 16N and 32N, a total friction distance of 200m, and a friction time of 30min. The reciprocating friction was carried out at room temperature, with a grinding ball of Φ4mm Al2O3 ball, a load of 30N, a reciprocating friction length of 5mm, a friction speed of 200mm / min, and a friction time of 30min. The samples before and after the friction test were weighed, and the specific wear rate was calculated according to the following formula:
[0083] K = V / (N·D) = (S·L) / (N·D);
[0084] K——wear rate, mm 3 ·N -1 ·m -1 ;
[0085] V——wear volume, mm 3 , calculated from S·L, S is the side area of the profile (mm 2 ), L is the wear scar length (mm);
[0086] N——Loading force, N;
[0087] D——friction distance, m.
[0088] The test results of the friction and wear resistance of the samples of the embodiments and comparative examples at room temperature are shown in Table 1 and Figure 4 shown.
[0089] 3. High temperature oxidation test:
[0090] High-temperature oxidation is carried out in a thermogravimetric analyzer filled with dry air. First, 20 mg of the prepared friction and wear resistant amorphous powder sample in each embodiment and comparative example is placed in an alumina crucible. The sample is then heated from room temperature to 673K, 723K, 773K, 823K, and 873K, respectively, at a heating rate of 100K / min, followed by isothermal insulation for 20min, 40min, 60min, and 80min, and then cooled to room temperature at a rate of 100K / min.
[0091] The final mass gains of the samples of the embodiments and comparative examples after high temperature oxidation at different conditions are as follows: Figure 2 The effect of SiC coating on the final mass gain of the sample after high temperature oxidation is shown in Figure 3 shown.
[0092] 4. Friction and wear resistance under high temperature environment:
[0093] The samples subjected to the high temperature oxidation test were subjected to a wear rate test according to the test method for friction and wear resistance test.
[0094] The test results of the friction and wear resistance of the samples of the embodiments and comparative examples under high temperature environment are shown in Table 1 and Figure 4 shown.
[0095] Table 1 Friction and wear resistance test of samples of various embodiments and comparative examples at room temperature and high temperature
[0096]
[0097] pass Figure 1 From the particle size distribution of the Zr-based amorphous powder and the prepared friction and wear resistant amorphous powder shown in FIG, it can be seen that the particle size of the sample is relatively uniform. The preparation of the SiC coating layer improves the overall particle size of the amorphous powder. It also shows from the side that the thickness of the SiC coating layer prepared on the surface of the Zr-based amorphous alloy by this method is relatively uniform. The friction and wear resistance test of each experimental example and comparative example sample was carried out at room temperature, and the specific wear rate obtained is shown in Tables 1 and Figure 4As shown, it can be seen that the specific wear rate of the sample increases with the increase of the proportion of Zr, W, and Nb elements. This is because Zr, W, and Nb all have strong hardness and good wear resistance. It can also be compared and found that with the increase of the deposition time and deposition temperature of the SiC coating layer, combined with the particle size distribution, it can be seen that the thickness of the SiC coating layer increases, which further improves the wear resistance of the amorphous powder. On the other hand, through the friction and wear resistance test of the samples oxidized at high temperature, it can be found that the SiC coating effectively improves the friction and wear resistance of the amorphous powder in a high temperature environment. This is due to the good stability of SiC at high temperature and the ability to maintain good friction and wear resistance, which has a strengthening effect on the friction and wear resistance of the Zr-based amorphous alloy powder; finally, the high-temperature oxidation behavior of each team ratio and embodiment was studied. Compared with the final mass gain at different temperatures to reflect the oxidation resistance of the amorphous powder, it can be seen that the preparation of the SiC coating significantly reduces the final mass gain, indicating that the preparation of the SiC coating is beneficial to improving the oxidation resistance at high temperatures. SiC can form a stable and dense oxide film at high temperatures, which effectively prevents oxygen from further corroding the SiC coating and the Zr-based amorphous alloy powder wrapped therein. Although the Zr, W, Ce and other components in the Zr-based amorphous alloy powder can also generate a stable oxide layer at high temperatures to prevent further oxidation and thus have good oxidation resistance, the oxidation process of SiC is slower, which makes the protective effect of the oxide layer better and the oxidation resistance can be well maintained, reducing the occurrence of oxidative wear and improving the use temperature and service life of the prepared friction and wear resistant amorphous powder.
[0098] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0099] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A friction and wear resistant amorphous powder, characterized in that: The friction and wear resistant amorphous powder is composed of Zr-based amorphous alloy powder and a SiC coating layer; The Zr-based amorphous alloy powder comprises the following chemical composition in atomic percentage: Zr 23.4%-45.8%, W 15.8%-22.1%, Nb 7.1%-10.9%, Ti 8.7%-12.3%, Cu 6.3%-10.6%, Ni 5.9%-8.0%, Mn 10.1%-10.3%, RE 0.05%-2.1%, and the rest are unavoidable impurities; In the chemical composition, RE is a rare earth metal, which is one of Rd, Ce, Pr, and Y, with a purity of 99%, and Zr, W, Nb, Ti, Cu, Ni, and Mn are respectively made of zirconium powder, tungsten powder, niobium powder, copper powder, nickel powder, manganese powder with a purity of 99.9%, and titanium powder with a purity of 99.6% as raw materials; The SiC coating layer is prepared on the surface of the Zr-based amorphous alloy powder by pyrolysis of methyltrichlorosilane and vapor phase chemical deposition, the mass fraction ratio of methyltrichlorosilane to Zr-based amorphous alloy powder is 2:1, and the purity of the methyltrichlorosilane is 99%; The preparation of the Zr-based amorphous alloy powder comprises the following steps: P1, according to the chemical composition of the Zr-based amorphous alloy powder, weigh the corresponding mass of zirconium powder, tungsten powder, niobium powder, copper powder, nickel powder, manganese powder, titanium powder and rare earth metal according to atomic percentage, first melt the zirconium powder, tungsten powder and niobium powder in a vacuum arc melting furnace to obtain a Zr-W-Nb alloy melt; P2, adding copper powder, nickel powder, manganese powder, titanium powder and rare earth metals to the Zr-W-Nb alloy melt obtained in step P1 in sequence, melting the mixture in a vacuum arc melting furnace to obtain a liquid alloy; P3, using the liquid alloy prepared in step P2 as a master alloy for high-pressure argon atomization, evacuating the atomization chamber, flushing it with argon for 3 times, and then filling it with argon as an atomization medium, keeping the master alloy under an argon pressure of 25-35 bar for 5 minutes, and continuously heating it to the atomization temperature, the master alloy is continuously sprayed out through the injection nozzle, collides with the argon gas flow to disperse into small droplets, and finally solidifies to obtain the Zr-based amorphous alloy powder; The method for preparing the friction and wear resistant amorphous powder comprises the following steps: S1, placing Zr-based amorphous alloy powder in a crucible and heating the reaction chamber to a deposition temperature; S2 and H2 are used as carrier gas and dilution gas at the same time, and Ar is used only as dilution gas. When the reaction chamber reaches the deposition temperature, methyltrichlorosilane is transported into the reaction chamber through a mixture of H2 and Ar. Methyltrichlorosilane is pyrolyzed into SiC and HCl, and vapor phase chemical deposition is performed to obtain a Zr-based amorphous alloy powder with a SiC coating layer. S3, after cooling to room temperature, collecting the Zr-based amorphous alloy powder with a SiC coating layer prepared in step S2, washing with deionized water and anhydrous ethanol in turn, and drying in an oven at 80° C. for 20 minutes to obtain the friction and wear resistant amorphous powder.
2. The amorphous powder resistant to friction and wear according to claim 1, characterized in that: The vacuum degree of the vacuum arc melting furnace in step P1 is 10 -2 Pa, melting temperature is 3400~3600℃, melting time is 10~20min.
3. The amorphous powder resistant to friction and wear according to claim 2, characterized in that: The vacuum degree of the vacuum arc melting furnace in step P2 is 10 -2 Pa, melting temperature is 3000~3300℃, melting time is 5~10min.
4. The amorphous powder resistant to friction and wear according to claim 3, characterized in that: The atomization temperature in step P3 is 2500-3000K, the atomization pressure is 3.5MPa, the atomization medium is high-purity argon gas with a purity of 99.99%, and the nozzle diameter is 50-150μm.
5. The amorphous powder resistant to friction and wear according to claim 4, characterized in that: The gas flow rate of Ar as a dilution gas is 90-300 sccm, the gas flow rates of H2 as a dilution gas and a carrier gas are 30-100 sccm and 45-200 sccm respectively, and the material flow rate of methyltrichlorosilane is 70-75 sccm.
6. The amorphous powder resistant to friction and wear according to claim 5, characterized in that: The deposition temperature of the vapor phase chemical deposition is 950-1100° C., and the deposition time is 30-120 min.
Citation Information
Patent Citations
Preparation method of SiC foam in-filling Cf / C-glassy carbon ultra high temperature vacuum heat insulation round tube
CN108752030A
Preparation method of surface coating of zirconium alloy cladding and surface coating
CN109576656A
Method for preparing amorphous composite coating through laser cladding
CN111139474A
Preparation method of anti-corrosion zirconium-based amorphous alloy composite material coating
CN113026013A
Method for reinforcing surface of zirconium-based amorphous alloy through laser irradiation of silicon carbide particles
CN113278903A