Antibacterial enamel material, preparation method and use method of antibacterial enamel wet glaze
By combining cuprous oxide and nanotitanium dioxide in the enamel material, long-term sterilization is achieved by using photocatalytic action, the problem of the degradation of antibacterial ability of existing antibacterial enamel materials under light is solved, and the widespread use and stability of the material are improved.
Patent Information
- Application Number
- CN202410962810.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-18
AI Technical Summary
The existing antibacterial enamel materials have a problem of gradually decreasing antibacterial ability during use, especially when encountering sodium hydroxide solution and normal saline, and ultraviolet lamps are needed to ensure sterilization effect, which limits the use conditions of the material.
By adding copper oxide and nanotitanium dioxide to the enamel material, copper oxide uses electrons and holes to generate under normal light, transfer it to nanotitanium dioxide, achieving a bactericidal effect, and mixing it in the enamel glaze-based glaze to reduce the amount of antibacterial agent used And cost, high-energy ball milling and vacuum drying technology are used to improve the adhesion and dispersion of adhesives, ensuring an effective combination of cuprous oxide and nanotitanium dioxide.
It achieves a long-term bactericidal effect under normal light, reduces the limitations of the use of antibacterial materials, avoids the deterioration of antibacterial ability over time, and improves the photocatalytic efficiency and bactericidal performance.
Smart Images

Figure CN118495815B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of enamel materials, and in particular to an antibacterial enamel material, a preparation method of the antibacterial enamel wet glaze and a use method thereof. Background Art
[0002] Enamel materials refer to a type of inorganic non-metallic material made from natural or synthetic compounds through forming and high-temperature sintering. They generally have the advantages of high melting point, high hardness, high wear resistance, and oxidation resistance. Antibacterial enamel materials mainly achieve antibacterial effects by adding antibacterial substances, surface treatment, and adjusting the structure to inhibit the growth and reproduction of bacteria.
[0003] At present, a Chinese invention patent application with publication number CN109592189A and publication date April 9, 2019 proposes a nanosilver negative ion antibacterial and sterilization liner enamel container, which includes 7-12% sodium oxide by weight, 0-5% potassium oxide, 1-6% calcium oxide, 0-12% aluminum oxide, 5-10% boron oxide, 50-75% silicon oxide, 3-10% zirconium oxide, 0.1-2% nanosilver powder and 0.5-5% negative ion powder. The nanosilver carrier is a silica-titania composite carrier, the silver content of the nanosilver is 1-30%, and the nanosilver particle size is 1-100nm.
[0004] The antibacterial principle is to continuously release silver ions, which enter the bacteria and kill them. At the same time, the silver ions catalyze oxygen into active oxygen O, killing bacteria. However, since silver ions are dissolved and released in water, the antibacterial ability will inevitably decrease gradually. Especially after being immersed in sodium hydroxide solution and saline, the antibacterial effect deteriorates rapidly.
[0005] A Chinese invention patent application with publication number CN114351142A and publication date April 15, 2022 proposes a method for preparing an antibacterial enamel liner, wherein the antibacterial material includes nano titanium dioxide.
[0006] The antibacterial principle is that nano-titanium dioxide, as a photocatalyst, can produce hydroxyl radicals and active oxygen under the irradiation of near-ultraviolet light waves, thereby killing bacteria. However, due to the low sensitivity of nano-titanium dioxide to natural light, a certain amount of silver ions must be included in the antibacterial material to compensate for the bactericidal effect under natural light. This still cannot completely solve the problem of the gradual decline in antibacterial ability caused by the release of silver ions; and an ultraviolet lamp must be installed in the enamel liner to ensure the bactericidal effect of the enamel liner, which greatly limits the use conditions of the enamel material.
[0007] It can be seen that the currently available antibacterial enamel materials have great limitations when used. Summary of the invention
[0008] In order to reduce the limitations of the use of antibacterial enamel materials, the present invention provides an antibacterial enamel material, a preparation method of antibacterial enamel wet glaze and a use method thereof.
[0009] In the first aspect, the present invention provides an antibacterial enamel material, which adopts the following technical solution:
[0010] An antibacterial enamel material comprises, by weight percentage, 30.0-45.0% silicon dioxide, 12.0-18.0% titanium dioxide, 10.0-18.0% aluminum oxide, 2.5-4.5% sodium oxide, 0-0.5% potassium oxide, 12.0-20.0% boron oxide, 2.0-5.0% calcium oxide, 2.0-6.0% zinc oxide, 2.0-4.0% cuprous oxide, 1.0-2.5% nano titanium dioxide, 0.5%-1.0% adhesive, the remainder being rare earth oxides and unavoidable impurities, and the content ratio of silicon dioxide to boron oxide is 2.2-2.5:1, and the adhesive is at least one of polyimide powder, polyvinylidene fluoride powder, and polyetheretherketone powder.
[0011] By adopting the above technical solution, cuprous oxide and nano-titanium dioxide are added to the enamel material, so that the cuprous oxide and the nano-titanium dioxide form a combination. Under normal light, electrons and holes will be generated on the cuprous oxide, and the electrons and holes will be transferred to the nano-titanium dioxide, so that the nano-titanium dioxide also has a bactericidal effect under normal light, thus reducing the limitation of the use of the enamel material, and the bactericidal effect does not depend on the precipitation of the substance, so that the enamel material has a long-term bactericidal effect, reducing the limitation of the use of the antibacterial enamel material.
[0012] In a second aspect, the present invention provides a method for preparing an antibacterial enamel wet glaze, which adopts the following technical scheme:
[0013] A method for preparing antibacterial enamel wet glaze comprises the following steps:
[0014] a. Select the following raw materials by mass: 30.0-45.0 parts by weight of silicon dioxide, 12.0-18.0 parts by weight of titanium dioxide, 10.0-18.0 parts by weight of aluminum oxide, 2.5-8.0 parts by weight of sodium oxide, 0-0.5 parts by weight of potassium oxide, 12.0-20.0 parts by weight of boron oxide, 2.0-5.0 parts by weight of calcium oxide, and 2.0-6.0 parts by weight of zinc oxide; according to the above chemical composition, convert the various components into quartz, titanium dioxide, ice crystals, feldspar, borax, and calcined heavy zinc oxide according to common knowledge, weigh and mix, melt at 1100°C-1200°C, cool to obtain enamel frit, then put it into a ball mill for ball milling, and sieve it through 1000 mesh to make enamel glaze base glaze;
[0015] b. The antibacterial agent is placed in the enamel base glaze and mixed to obtain an antibacterial enamel material, wherein the mass fractions of each raw material in the antibacterial agent are: cuprous oxide powder 2.0-4.0, nano titanium dioxide powder 1.0-2.5, and adhesive 0.5%-1.0%;
[0016] c. Mixing the antibacterial enamel material and the suspending agent, wherein the antibacterial enamel material accounts for 90-93% by weight and the remainder is the suspending agent, and then placing it in water to prepare the antibacterial enamel wet glaze, the density of the enamel wet glaze is 1.65-1.85 g / cm³.
[0017] By adopting the above technical scheme, cuprous oxide powder and nano titanium dioxide powder are used as antibacterial agents, and are added after the enamel base glaze is prepared and then mixed. In this way, the cuprous oxide powder and the titanium dioxide powder can be attached to the surface of the enamel base glaze, which can reduce the amount of antibacterial agent used and reduce costs.
[0018] Optionally, in step b, cuprous oxide is prepared by uniformly mixing cupric oxide powder and copper powder in a molar ratio of 1:1.05 to 1.1, and calcining the mixture at a temperature of 800 to 900° C. in an oxygen-free environment for 6 hours.
[0019] By adopting the above technical solution, since an excess of copper powder is added to the copper oxide powder, the copper oxide can fully react, thereby reducing the content of cupric oxide impurities in the obtained cuprous oxide, thereby reducing the photosensitivity weakening effect of copper oxide and improving the utilization rate of light; at the same time, the excess copper can also increase the activity of nano titanium dioxide, thereby improving the bactericidal effect.
[0020] Optionally, in step b, cuprous oxide and an adhesive are first placed in a high-energy ball mill for ball milling for 12 to 24 hours at a ball milling speed of 100 to 300 rpm, and then nano-titanium dioxide is added to the high-energy ball mill for ball milling for 6 to 12 hours.
[0021] By adopting the above technical scheme, static electricity is generated on the adhesive under the ball milling action of the high-energy ball mill and adheres to the cuprous oxide. Then nano-titanium dioxide is added to make the nano-titanium dioxide adhere to the adhesive. In this way, the nano-titanium dioxide adheres to the cuprous oxide, making it easier for the cuprous oxide to transfer electrons and holes to the nano-titanium dioxide, thereby improving the photocatalytic efficiency.
[0022] Optionally, in step b, anhydrous ethanol is slowly added during ball milling, and vacuum drying is performed after ball milling, and the drying time is 8 to 10 hours.
[0023] By adopting the above technical solution, cuprous oxide powder and nano-titanium dioxide can be dispersed more evenly by adding anhydrous ethanol, and then dried by vacuum drying mode, that is, the anhydrous ethanol is removed, and the bubbles in the anhydrous ethanol can be knocked out when the anhydrous ethanol is removed, thereby reducing the probability of electrons on the adhesive being carried away by the bubbles and escaping, and maintaining the bonding performance between cuprous oxide and nano-titanium dioxide.
[0024] Optionally, in step c, triethanolamine is further added to mix the antibacterial enamel material, triethanolamine and the suspending agent, wherein the mass ratio of the antibacterial enamel material to triethanolamine is 90-93%:0.2-0.5%, and the remainder is the suspending agent.
[0025] By adopting the above technical solution, after adding triethanolamine, the particles composed of cuprous oxide and nano-titanium dioxide can be mixed with the enamel base glaze more evenly, reducing the probability of agglomeration of cuprous oxide and titanium dioxide.
[0026] In a third aspect, the present invention provides a method for using an antibacterial enamel wet glaze, which adopts the following technical solution:
[0027] d. Apply the wet enamel glaze evenly on the utensil;
[0028] e. Enameling is carried out at 700-900°C to obtain enameled utensils.
[0029] By adopting the above technical scheme, since the content of sodium oxide and potassium oxide is reduced in the antibacterial enamel material, and the content of boron oxide is set to 12.0-20.0%, the antibacterial enamel material has good thermal stability. At a temperature of 700-900°C, the enamel base glaze can be softened. At this time, cuprous oxide and nano-titanium dioxide will penetrate into the surface of the enamel base glaze, so that the enamelware can have an antibacterial effect.
[0030] Optionally, in step e, the enameling is first performed at 700-800° C., and then enameled at 800-900° C. for 30 minutes to obtain an enameled ware.
[0031] By adopting the above technical scheme, when enameling is carried out at 700-800°C, cuprous oxide and nano-titanium dioxide can fully enter the enamel base glaze, and then the temperature is raised to 800-900°C and enameled for 30 minutes, so that part of the nano-titanium dioxide is transformed from anatase titanium dioxide to rutile titanium dioxide, which can improve the photocatalytic efficiency of anatase titanium dioxide and thus improve the bactericidal performance.
[0032] Optionally, in step e, the enameling is carried out in an environment isolated from oxygen.
[0033] By adopting the above technical solution, the possibility of cuprous oxide converting into cupric oxide can be reduced during enameling, thereby maintaining the cuprous oxide content on the enamel layer and further maintaining the antibacterial ability of the enamel coating.
[0034] In summary, the present invention includes at least one of the following beneficial technical effects:
[0035] 1. Through the setting of cuprous oxide and nano-titanium dioxide, under normal light, electrons and holes will be generated on the cuprous oxide, and the electrons and holes will be transferred to the nano-titanium dioxide, so that the nano-titanium dioxide also has a bactericidal effect under normal light, thus reducing the limitations of the use of enamel materials, and the bactericidal effect does not depend on the precipitation of substances, so that the enamel material has a long-term bactericidal effect.
[0036] 2. When preparing cuprous oxide, the cupric oxide powder and the copper powder are mixed evenly at a molar ratio of 1:1.05 to 1.1, so that the cupric oxide can fully react, reducing the content of cupric oxide impurities in the prepared cuprous oxide, thereby reducing the weakening effect of cupric oxide on photosensitivity and improving the utilization rate of light; at the same time, excess copper can also increase the activity of nano-titanium dioxide, thereby improving the bactericidal effect.
[0037] 3. By placing cuprous oxide and nano-titanium dioxide in a high-energy ball mill for ball milling, nano-titanium dioxide can be well attached to cuprous oxide, which makes it easier for cuprous oxide to transfer electrons and holes to nano-titanium dioxide, thereby improving the photocatalytic efficiency.
[0038] 4. By first calcining at 700-800°C and then calcining at 800-900°C for 30 minutes, cuprous oxide and nano-titanium dioxide can fully enter the enamel base glaze, and then the temperature is raised to 800-900°C and calcined for 30 minutes, so that part of the nano-titanium dioxide is transformed from anatase titanium dioxide to rutile titanium dioxide, which can improve the photocatalytic efficiency of anatase titanium dioxide and thus improve the bactericidal performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 is the XRD pattern of Example 1;
[0040] Figure 2 is the XRD pattern of Comparative Example 4;
[0041] Figure 3 is an image of cuprous oxide after ball milling in Example 1 scanned by an electron microscope;
[0042] Figure 4 is an image of cuprous oxide after ball milling by scanning electron microscope in Comparative Example 5;
[0043] Figure 5 is an image of the surface of the enamelware scanned by an electron microscope in Example 1;
[0044] Figure 6 is an image of the surface of the enamelware scanned by an electron microscope in Comparative Example 6;
[0045] Figure 7 is an image of the surface of the enamelware scanned by an electron microscope in Comparative Example 7;
[0046] Figure 8 is an image of the surface of the enamelware scanned by an electron microscope in Comparative Example 9;
[0047] Fig. 9 This is an EDS spectrum analysis diagram of a local part of the surface of the enamelware in Example 1;
[0048] Fig.10 This is an EDS spectrum analysis diagram of a local surface of the enamelware in Comparative Example 10;
[0049] Fig.11 This is an EDS spectrum analysis diagram of a local surface of the enamelware in Example 11. DETAILED DESCRIPTION
[0050] The present invention is further described in detail below with reference to the embodiments.
[0051] Example 1: This example discloses an antibacterial enamel material, the weight percentage of which includes: 30.0% silicon dioxide, 18.0% titanium dioxide, 18.0% aluminum oxide, 2.5% sodium oxide, 0.5% potassium oxide, 12.0% boron oxide, 5.0% calcium oxide, 6.0% zinc oxide, 4.0% cuprous oxide, 2.5% nano titanium dioxide, 1.0% polyimide powder, and the balance is rare earth oxides and unavoidable impurities.
[0052] The preparation method and use method are as follows:
[0053] a. Select the following raw materials by mass: 30.0 silicon dioxide, 18.0 titanium dioxide, 18.0 aluminum oxide, 2.5 sodium oxide, 0.5 potassium oxide, 12.0 boron oxide, 5.0 calcium oxide, and 6.0 zinc oxide; according to the above chemical composition, convert various components into quartz, titanium dioxide, ice crystal, feldspar, borax, and calcined heavy zinc oxide according to common knowledge, weigh and mix, (due to the different objective reasons such as the origin, manufacturer, batch, etc. of quartz, titanium dioxide, ice crystal, feldspar, borax, and calcined heavy zinc oxide, the proportion of each raw material used will also be different, but as long as the final material content after mixing is consistent with the composition material content ratio of the antibacterial enamel material, the same below), melt at 1150°C, the temperature difference during melting does not exceed ±50°C, cool to obtain enamel frit, then put it into a ball mill for ball milling, and sieve through 1000 mesh to make enamel glaze base glaze.
[0054] b. The copper oxide powder and the copper powder are mixed uniformly in a molar ratio of 1:1.05, and calcined at a temperature of 850°C for 6 hours without oxygen. The temperature difference during calcination does not exceed ±30°C to obtain cuprous oxide powder, and sieve it through 1800 mesh; the mass fractions of the raw materials are selected as follows: 4.0 cuprous oxide powder, 2.5 nano titanium dioxide powder, and 1.0 polyimide powder. The cuprous oxide and polyimide powders are first placed in a high-energy ball mill for 24 hours, and anhydrous ethanol is slowly added during the ball milling at a speed of 300 rpm. Then, nano titanium dioxide is added to the high-energy ball mill for 12 hours, and anhydrous ethanol is slowly added during the ball milling at a speed of 300 rpm. After the ball milling is completed, vacuum drying is performed for 10 hours to prepare an antibacterial agent; the antibacterial agent is placed in an enamel base glaze and mixed to prepare an antibacterial enamel material.
[0055] c. Mix the antibacterial enamel material, triethanolamine and a suspending agent, wherein bentonite is selected as the suspending agent, wherein the antibacterial enamel material accounts for 92% by weight, the triethanolamine accounts for 0.4% by weight, and the remainder is the suspending agent, and then put it into water to make an antibacterial enamel wet glaze, and the density of the enamel wet glaze is 1.75 g / cm³.
[0056] d. Apply the wet enamel evenly on the utensil.
[0057] e. First, enameling is carried out at 750℃, and the temperature difference during enameling does not exceed ±30℃. Enameling is carried out until the temperature difference between the internal temperature and the surface temperature of the utensil is less than 50℃. Then, enameling is carried out at 850℃ for 30 minutes, and the temperature difference during enameling does not exceed ±30℃. Oxygen is isolated during the enameling process to obtain enameled utensil.
[0058] Example 2: This example discloses an antibacterial enamel material, the weight percentage of which includes: 45.0% silicon dioxide, 12.0% titanium dioxide, 10.0% aluminum oxide, 4.5% sodium oxide, 0% potassium oxide, 20.0% boron oxide, 2.0% calcium oxide, 2.0% zinc oxide, 2.0% cuprous oxide, 1.0% nano titanium dioxide, 0.5% polyimide powder, and the remainder is rare earth oxides and unavoidable impurities.
[0059] The preparation method and use method are as follows:
[0060] a. Select the following raw materials by mass: 45.0% silicon dioxide, 12.0% titanium dioxide, 10.0% aluminum oxide, 4.5% sodium oxide, 0% potassium oxide, 20.0% boron oxide, 2.0% calcium oxide and 2.0% zinc oxide; according to the above chemical composition, convert various ingredients into quartz, titanium dioxide, ice crystal, feldspar, borax and calcined heavy zinc oxide according to common knowledge, weigh and mix, melt at 1150°C, with the temperature difference during melting not exceeding ±50°C, cool to obtain enamel frit, then put it into a ball mill for ball milling, and sieve through 1000 mesh to make enamel glaze base glaze.
[0061] b. Mix copper oxide powder and copper powder in a molar ratio of 1:1.1, calcine at a temperature of 850°C for 6 hours in an oxygen-free environment, with a temperature difference of no more than ±30°C during calcination, to obtain cuprous oxide powder; select the mass fractions of raw materials: 2.0 cuprous oxide powder, 1.0 nano titanium dioxide powder, and 0.5 polyimide powder, first place the cuprous oxide and polyimide powders in a high-energy ball mill for 12 hours, slowly add anhydrous ethanol during the ball milling, and the ball milling speed is 100 rpm, then add nano titanium dioxide to the high-energy ball mill for 6 hours, and slowly add anhydrous ethanol during the ball milling, and the ball milling speed is 100 rpm; after the ball milling is completed, vacuum dry for 8 hours to prepare an antibacterial agent; place the antibacterial agent in an enamel base glaze and mix to obtain an antibacterial enamel material.
[0062] c. Mix the antibacterial enamel material, triethanolamine and a suspending agent, wherein bentonite is selected as the suspending agent, wherein the antibacterial enamel material accounts for 92% by weight, the triethanolamine accounts for 0.4% by weight, and the remainder is the suspending agent, and then put it into water to make an antibacterial enamel wet glaze, and the density of the enamel wet glaze is 1.75 g / cm³.
[0063] d. Apply the wet enamel evenly on the utensil.
[0064] e. First, enameling is carried out at 750℃, and the temperature difference during enameling does not exceed ±30℃. Enameling is carried out until the temperature difference between the internal temperature and the surface temperature of the utensil is less than 50℃. Then, enameling is carried out at 850℃ for 30 minutes, and the temperature difference during enameling does not exceed ±30℃. Oxygen is isolated during the enameling process to obtain enameled utensil.
[0065] Example 3: This example discloses an antibacterial enamel material, the weight percentage of which includes: 37.5% silicon dioxide, 15.0% titanium dioxide, 14.0% aluminum oxide, 3.5% sodium oxide, 0.5% potassium oxide, 16.0% boron oxide, 3.5% calcium oxide, 4.0% zinc oxide, 3.0% cuprous oxide, 1.5% nano titanium dioxide, 0.75% polyimide powder, and the remainder is rare earth oxides and unavoidable impurities.
[0066] The preparation method and use method are as follows:
[0067] a. The mass fractions of the raw materials are as follows: 37.5% silicon dioxide, 15.0% titanium dioxide, 14.0% aluminum oxide, 3.5% sodium oxide, 0.5% potassium oxide, 16.0% boron oxide, 3.5% calcium oxide, and 4.0% zinc oxide; according to the above chemical composition, the various components are converted into quartz, titanium dioxide, ice crystals, feldspar, borax, and calcined heavy zinc oxide according to common knowledge, weighed and mixed, melted at 1150°C, with a temperature difference of no more than ±50°C during melting, and cooled to obtain an enamel frit, which is then put into a ball mill for ball milling and sieved through a 1000-mesh sieve to make an enamel glaze base glaze.
[0068] b. The copper oxide powder and the copper powder are mixed uniformly in a molar ratio of 1:1.07, and calcined at a temperature of 850°C for 6 hours in an oxygen-free environment. The temperature difference during calcination does not exceed ±30°C to obtain cuprous oxide powder; the mass fractions of the raw materials are selected as follows: 3.0 cuprous oxide powder, 1.5 nano titanium dioxide powder, and 0.75 polyimide powder. The cuprous oxide and polyimide powders are first ball-milled in a high-energy ball mill for 18 hours, and anhydrous ethanol is slowly added during the ball milling at a speed of 200 rpm. Then, nano titanium dioxide is added to the high-energy ball mill and ball-milled for 18 hours, and anhydrous ethanol is slowly added during the ball milling at a speed of 200 rpm. After the ball milling is completed, vacuum drying is performed for 9 hours to prepare an antibacterial agent; the antibacterial agent is placed in an enamel base glaze and mixed to obtain an antibacterial enamel material.
[0069] c. Mix the antibacterial enamel material, triethanolamine and a suspending agent, wherein bentonite is selected as the suspending agent, wherein the antibacterial enamel material accounts for 92% by weight, the triethanolamine accounts for 0.4% by weight, and the remainder is the suspending agent, and then put it into water to make an antibacterial enamel wet glaze, and the density of the enamel wet glaze is 1.75 g / cm³.
[0070] d. Apply the wet enamel evenly on the utensil.
[0071] e. First, enameling is carried out at 750℃, and the temperature difference during enameling does not exceed ±30℃. Enameling is carried out until the temperature difference between the internal temperature and the surface temperature of the utensil is less than 50℃. Then, enameling is carried out at 850℃ for 30 minutes, and the temperature difference during enameling does not exceed ±30℃. Oxygen is isolated during the enameling process to obtain enameled utensil.
[0072] The test mainly tests the hardness, glossiness, surface smoothness and photocatalytic rate of enamel products. When testing the photocatalytic rate, a 10×10-5 mol / L methyl orange aqueous solution is used as an experimental reference agent, and the methyl orange concentration is tested after exposure to natural light for 3 hours to determine the photocatalytic rate.
[0073] The enamel products prepared in Example 1, Example 2 and Example 3 were tested and experimented.
[0074]
[0075] By comparing Example 1, Example 2, and Example 3, it can be seen that when the content of silicon dioxide is greater, the hardness and glossiness are higher, and when the content of silicon dioxide decreases, the hardness and glossiness become lower. Moreover, when the content of cuprous oxide and nano-titanium dioxide increases, the photocatalytic effect is stronger, and when the content of cuprous oxide and nano-titanium dioxide decreases, the photocatalytic effect decreases, but the decrease is not obvious and is within an acceptable range.
[0076] Comparative Example 1: This comparative example discloses an antibacterial enamel material, the weight percentage of which includes: 30.0% silicon dioxide, 14.0% titanium dioxide, 14.0% aluminum oxide, 2.5% sodium oxide, 0.5% potassium oxide, 20.0% boron oxide, 5.0% calcium oxide, 6.0% zinc oxide, 4.0% cuprous oxide, 2.5% nano titanium dioxide, 1.0% polyimide powder, and the balance is rare earth oxides and unavoidable impurities.
[0077] The preparation method and the use method thereof are exactly the same as those in Example 1 except that the ratio of the enamel base glaze is different from that in Example 1.
[0078] Comparative Example 2: This comparative example discloses an antibacterial enamel material, the weight percentage of which includes: 45.0% silicon dioxide, 15.0% titanium dioxide, 14.0% aluminum oxide, 2.5% sodium oxide, 0.0% potassium oxide, 12.0% boron oxide, 3.0% calcium oxide, 4.0% zinc oxide, 2.0% cuprous oxide, 1.0% nano titanium dioxide, and the balance is rare earth oxides and unavoidable impurities.
[0079] Its preparation method and use method are exactly the same as those in Example 2 except that the ratio of the enamel base glaze is different from that in Example 2.
[0080] Comparative Example 3: This comparative example discloses an antibacterial enamel material, the weight percentage of which includes: 45.0% silicon dioxide, 15.0% titanium dioxide, 14.0% aluminum oxide, 2.5% sodium oxide, 0.0% potassium oxide, 12.0% boron oxide, 3.0% calcium oxide, 4.0% zinc oxide, 2.0% cuprous oxide, 1.0% nano titanium dioxide, 0.5% polyimide powder, and the remainder is rare earth oxides and unavoidable impurities.
[0081] The preparation method and the use method are exactly the same as those of Comparative Example 2, except that the enamelware prepared in Comparative Example 3 is placed in humid air for 72 hours.
[0082] The enamel products prepared in Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested and experimented.
[0083]
[0084] Comparative Example 1 failed during step c because an excessive amount of boron oxide was added, so that the boron oxide could not fully react with silicon dioxide to vitrify, and thus part of the boron oxide reacted with water during the production of wet enamel.
[0085] By comparing Example 3 with Comparative Example 2, it can be seen that after reducing the content of boron oxide, the photocatalytic effect does not change significantly. By comparing Comparative Example 2 with Comparative Example 3, it can be seen that after reducing the content of boron oxide, the photocatalytic effect of enamelware will be significantly reduced as the placement time increases, and the surface glossiness will decrease to a certain extent. The reason is that cuprous oxide is partially oxidized into cupric oxide in a humid environment, which loses its photocatalytic effect, thereby causing the antibacterial effect to decrease. It can be seen that the content ratio of silicon dioxide to boric oxide is preferably 2.2 to 2.5:1. When the content of boric oxide is too high, it is easy to make the enamel wet glaze fail, and when the content of boric oxide is too low, the fluidity of the enamel glaze base glaze becomes worse. During the enameling process, cuprous oxide is not easy to penetrate into the enamel glaze base glaze, which leads to the easy oxidation of part of the cuprous oxide, and the photocatalytic effect of the enamelware will decrease with the extension of time.
[0086] Comparative Example 4: This comparative example discloses an antibacterial enamel material, whose composition is exactly the same as that of Example 1, except that in step b, the molar ratio of copper oxide powder to copper powder is 1:1.
[0087] Comparative Example 5: This comparative example discloses an antibacterial enamel material, which has the same composition as Example 1 except that it does not contain polyimide powder; the difference in its processing steps is that in step b, cuprous oxide and nano-titanium dioxide are simultaneously placed in an ordinary ball mill for ball milling.
[0088] Comparative Example 6: This comparative example discloses an antibacterial enamel material, whose composition is exactly the same as that of Example 1, except that in step c, triethanolamine is not added.
[0089] The enamel products prepared in Comparative Examples 4, 5 and 6 were tested and experimented.
[0090]
[0091] By comparing Comparative Example 4 with Example 1, it can be seen that when the copper oxide powder and the copper powder are added at a molar ratio of 1:1, the photocatalytic effect of the enamelware will be significantly weakened. It can be seen from the XRD image that cuprous oxide contains copper oxide impurities; the presence of copper oxide impurities is because copper oxide fails to completely react with copper, and copper oxide impurities will weaken the photocatalytic effect.
[0092] By comparing Comparative Example 5 with Example 1, it can be seen that when cuprous oxide and nano-titanium dioxide are placed in an ordinary ball mill at the same time, the photocatalytic effect of the enamelware will be significantly weakened, and the photocatalytic effect will almost be lost. Scanning the milled cuprous oxide with an electron microscope revealed that the degree of binding between the octahedral cuprous oxide and the nano-titanium dioxide is low, and only a small amount of nano-titanium dioxide is attached to the cuprous oxide, so that the electrons excited from the cuprous oxide cannot respond to the nano-titanium dioxide, thereby causing the nano-titanium dioxide to basically fail to play a photocatalytic role.
[0093] By comparing Comparative Example 6 with Example 1, it can be seen that when triethanolamine is not added in step c, the photocatalytic effect of the enamelware will be significantly weakened. Scanning the surface of the enamelware with an electron microscope revealed that agglomeration occurred in some areas of the surface of the enamelware, the antibacterial agent was unevenly distributed on the surface of the enamelware, and cuprous oxide and nano-titanium dioxide could not fully exert their photocatalytic effect.
[0094] Comparative Example 7: This comparative example discloses an antibacterial enamel material, whose composition by weight percentage includes: 30.0% silicon dioxide, 15.0% titanium dioxide, 15.0% aluminum oxide, 2.5% sodium oxide, 0.5% potassium oxide, 12.0% boron oxide, 5.0% calcium oxide, 6.0% zinc oxide, 7.0% cuprous oxide, 5.0% nano titanium dioxide, 1.5% polyimide powder, and the remainder is rare earth oxides and unavoidable impurities.
[0095] The preparation method and the use method thereof are completely the same as those in Example 1 except that the ratio of the antibacterial agent is different from that in Example 1.
[0096] Comparative Example 8: This comparative example discloses an antibacterial enamel material, whose composition is exactly the same as that of Comparative Example 1, except that in step b, cuprous oxide powder with a purity of 99.7% is used, and the rest is exactly the same as that of Example 1.
[0097] Comparative Example 9: This comparative example discloses an antibacterial enamel material, whose composition is exactly the same as that of Comparative Example 1, except that in step e, oxygen is not isolated during the enameling process.
[0098] The enamel products prepared in Comparative Examples 7, 8 and 9 were tested and experimented.
[0099]
[0100] By comparing Comparative Example 7 with Example 1, it can be seen that when the content of cuprous oxide and nano-titanium dioxide increases, the photocatalytic effect of the enamelware will not continue to be improved, but will be slightly reduced. Scanning the surface of the enamelware with an electron microscope revealed that the antibacterial agent agglomerates in some areas of the surface of the enamelware. The agglomerated antibacterial agent cannot fully exert its photocatalytic effect, but reduces the photocatalytic effect.
[0101] By comparing Comparative Example 8 with Example 1, it can be seen that when the added cuprous oxide powder is a cuprous oxide powder with a purity of 99.7%, not only does it not continue to improve the photocatalytic effect of the enamelware, but it will slightly reduce the photocatalytic effect. It can be seen that when the cuprous oxide powder contains a certain amount of copper impurities, it will not only not reduce the photocatalytic effect, but will make the nano titanium dioxide have a stronger catalytic effect due to the effect of copper.
[0102] By comparing Comparative Example 9 with Example 1, it can be seen that in step e, oxygen is not isolated during the enameling process, and the photocatalytic effect of the enameled ware will be significantly weakened, but the photocatalytic effect will not be completely lost. After scanning the surface of the enameled ware with an electron microscope, it was found that part of the nano-titanium dioxide particles were attached to the cuprous oxide, so that part of the cuprous oxide was isolated from the air. If oxygen is not isolated during the enameling process, the cuprous oxide is not completely oxidized to cuprous oxide, so that part of the cuprous oxide still has a photocatalytic effect together with the nano-titanium dioxide.
[0103] Comparative Example 10: This comparative example discloses an antibacterial enamel material, whose composition is exactly the same as that of Comparative Example 1, except that in step e, the enameling is always carried out at 750°C, the temperature difference during enameling does not exceed ±30°C, and the temperature difference between the internal temperature and the surface temperature of the utensil during enameling is less than 50°C.
[0104] Comparative Example 11: This comparative example discloses an antibacterial enamel material, whose composition is exactly the same as that of Comparative Example 1, except that in step e, the enameling is always carried out at 850°C, the temperature difference during enameling does not exceed ±30°C, and the temperature difference between the internal temperature and the surface temperature of the utensil during enameling is less than 50°C.
[0105] The enamel products prepared in Comparative Examples 10 and 11 were tested and experimented.
[0106]
[0107] By comparing Comparative Examples 10 and 11 with Example 1, it can be seen that in step e, the calcination is always carried out at 750°C, and the temperature difference during calcination does not exceed ±30°C, which will slightly reduce the photocatalytic effect. Through EDS comparison, it can be seen that the nano titanium dioxide on the surface of the enameled ware remains anatase titanium dioxide; the surface of the enameled ware also has some large anatase and rutile mixed titanium dioxide particles, which are formed by the titanium dioxide in the enamel glaze base glaze.
[0108] In step e, the enamelling is always carried out at 850°C, and the temperature difference during enamelling does not exceed ±30°C, which will slightly reduce the photocatalytic effect. Through EDS comparison, it can be seen that only a small amount of nano titanium dioxide on the surface of the enameled ware is anatase titanium dioxide, and the rest is rutile titanium dioxide; the surface of the enameled ware also has some large anatase and rutile mixed titanium dioxide particles, which are formed by titanium dioxide in the enamel glaze base.
[0109] Through EDS analysis of Example 1, it can be learned that only a small amount of nano titanium dioxide on the surface of the enamelware is rutile titanium dioxide, and the rest is anatase titanium dioxide; the surface of the enamelware also has some large titanium dioxide particles mixed with anatase and rutile types, which are formed by titanium dioxide in the enamel glaze base glaze.
[0110] Through the above analysis, it can be found that when anatase titanium dioxide is partially doped with rutile titanium dioxide, its photocatalytic effect is better than that of pure anatase titanium dioxide and also better than that of titanium dioxide with a higher rutile content.
[0111] The implementation principles of the antibacterial enamel material, the preparation method of the antibacterial enamel wet glaze and the use method of the antibacterial enamel wet glaze in the present application are as follows:
[0112] By reducing the content of sodium oxide and potassium oxide, increasing the content of boron oxide, and controlling the content of silicon dioxide and aluminum oxide, the antibacterial enamel material has better thermal stability. When sintered into enamel base glaze, the enamel base glaze has a good vitrification state and has good fluidity at 700-900°C, which facilitates the penetration of antibacterial materials without leaving obvious flow marks on the surface of the enamelware.
[0113] By adding cuprous oxide and nano titanium dioxide powder as antibacterial agents to the enamel glaze base glaze, the catalytic effect of nano titanium dioxide under natural light can be greatly improved. Enameled utensils no longer rely on ultraviolet lamps to have a good sterilization effect, which reduces the requirements for the external environment and makes the enamel utensils have a wider range of uses. Moreover, cuprous oxide and nano titanium dioxide are leached into the enamel glaze base glaze, and will not dissolve and release ions, so that the enamel ware still has a good antibacterial effect when used for a long time, and the antibacterial effect will not deteriorate with the extension of the use time. At the same time, due to the setting of alumina and titanium dioxide in the enamel glaze base glaze, the glass phase contains more anatase crystal phase and alumina phase, and the anatase crystal and the alumina crystal are in a symbiotic state, so that the hardness and wear resistance of the glaze surface are good, further protecting the antibacterial material, making it difficult for the antibacterial material to be released under wear, and the antibacterial effect is not easy to deteriorate due to wear.
[0114] When preparing the antibacterial agent, the copper oxide powder and the copper powder are evenly mixed at a molar ratio of 1:1.05 to 1.1, and then calcined, so that part of the copper impurities can be doped into the cuprous oxide powder and the copper oxide impurities can be reduced; the presence of metallic copper in the glass phase can improve the photocatalytic effect of nano titanium dioxide, and reducing the content of copper oxide impurities reduces the influence on the photocatalytic effect of nano titanium dioxide.
[0115] When cuprous oxide, adhesive, and nano-titanium dioxide are placed in a high-energy ball mill for ball milling, the adhesive first adheres to the cuprous oxide, and then the nano-titanium dioxide is adsorbed on the adhesive, which ultimately makes the nano-titanium dioxide and cuprous oxide more closely combined, making it easier for cuprous oxide to transfer electrons and holes to the nano-titanium dioxide, thereby improving the photocatalytic efficiency. In addition, the nano-titanium dioxide is coated on the cuprous oxide powder, which increases the difficulty of cuprous oxide being oxidized, further reduces the content of copper oxide, and thus maintains the photocatalytic effect.
[0116] The antibacterial enamel material, triethanolamine and suspending agent are mixed. After the triethanolamine is added, the particles composed of cuprous oxide and nano-titanium dioxide can be mixed more evenly with the enamel base glaze, reducing the probability of agglomeration of cuprous oxide and titanium dioxide; this can greatly improve the utilization rate of nano-titanium dioxide, thereby maintaining the photocatalytic effect. The triethanolamine is decomposed and eliminated during the enamel firing process, and no impurities are introduced.
[0117] During the enameling process, the enameling is first performed at 750°C, and the temperature difference during the enameling process does not exceed ±30°C. The specific enameling time is determined according to the material and size of the appliance. The more difficult it is to heat up the material of the appliance and the larger the size of the appliance, the longer the enameling time of this part. Specifically, when the temperature of the appliance reaches 730°C±30°C, the next step of heating can be performed. After that, the enameling is performed at 850°C for 30 minutes, and the temperature difference during the enameling process does not exceed ±30°C. In this way, part of the anatase nano-titanium dioxide can be converted into rutile nano-titanium dioxide. The photocatalytic effect of the mixture of rutile nano-titanium dioxide and anatase nano-titanium dioxide is better than that of pure titanite nano-titanium dioxide, thereby improving the photocatalytic effect.
[0118] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An antibacterial enamel material, It is characterized in that The composition comprises by weight percentage: 30.0-45.0% silicon dioxide, 12.0-18.0% titanium dioxide, 10.0-18.0% aluminum oxide, 2.5-4.5% sodium oxide, 0-0.5% potassium oxide, 12.0-20.0% boron oxide, 2.0-5.0% calcium oxide, 2.0-6.0% zinc oxide, 3.5-7.5% antibacterial agent, and the balance is rare earth oxide and unavoidable impurities, and the content ratio of silicon dioxide to boron oxide is 2.2-2.5:1; The antibacterial agent includes 2.0-4.0% cuprous oxide, 1.0-2.5% nano titanium dioxide, and 0.5-1.0% adhesive, wherein the adhesive is at least one of polyimide powder, polyvinylidene fluoride powder, and polyetheretherketone powder; The preparation method of the antibacterial agent is as follows: cuprous oxide and an adhesive are placed in a high-energy ball mill for ball milling for 12 to 24 hours at a ball milling speed of 100 to 300 rpm, and then nano titanium dioxide is added to the high-energy ball mill for ball milling for 6 to 12 hours.
2. A method for preparing antibacterial enamel wet glaze, It is characterized by the following step: a. The mass percentage of the raw materials is as follows: 30.0-45.0% silicon dioxide, 12.0-18.0% titanium dioxide, 10.0-18.0% aluminum oxide, 2.5-8.0% sodium oxide, 0-0.5% potassium oxide, 12.0-20.0% boron oxide, 2.0-5.0% calcium oxide, and 2.0-6.0% zinc oxide; according to the above chemical composition, the various components are converted into quartz, titanium dioxide, ice crystals, feldspar, borax, and calcined heavy zinc oxide according to common knowledge, weighed and mixed, melted at 1100°C to 1200°C, and quenched to obtain enamel frit, which is then put into a ball mill for ball milling and sieved through 1000 mesh to make enamel glaze base glaze; b. placing an antibacterial agent in an enamel base glaze and mixing the mixture to obtain an antibacterial enamel material. The preparation method of the antibacterial agent is as follows: placing cuprous oxide and an adhesive in a high-energy ball mill for 12 to 24 hours at a ball milling speed of 100 to 300 rpm, and then adding nano-titanium dioxide to the high-energy ball mill for 6 to 12 hours. The mass fractions of the raw materials in the antibacterial agent are as follows: 2.0 to 4.0% cuprous oxide powder, 1.0 to 2.5% nano-titanium dioxide powder, and 0.5 to 1.0% adhesive; c. Mixing the antibacterial enamel material and the suspending agent, wherein the antibacterial enamel material accounts for 90-93% by weight and the remainder is the suspending agent, and then placing it in water to prepare the antibacterial enamel wet glaze, the density of the enamel wet glaze is 1.65-1.85 g / cm³.
3. The method for preparing an antibacterial enamel wet glaze according to claim 2, Features: In step b, cuprous oxide is prepared by mixing cupric oxide powder and copper powder in a molar ratio of 1: The mixture is uniformly mixed in a ratio of 1.05 to 1.1, and calcined at a temperature of 800 to 900° C. in an oxygen-free environment for 6 hours.
4. A method for preparing an antibacterial enamel wet glaze according to claim 2, Features: In step b, anhydrous ethanol is slowly added during ball milling, and vacuum drying is performed after ball milling, and the drying time is 8 to 10 hours.
5. A method for preparing an antibacterial enamel wet glaze according to any one of claims 2 to 4, Features: In step c, triethanolamine is also added to mix the antibacterial enamel material, triethanolamine and the suspending agent, wherein the mass ratio of the antibacterial enamel material to triethanolamine is 90-93%:0.2-0.5%, and the remainder is the suspending agent.
6. A method for using an antibacterial enamel wet glaze, Features: d. The wet enamel glaze according to any one of claims 2-5 is evenly applied to the utensil; e. Enameling is carried out at 700-900°C to obtain enameled utensils.
7. A method for using the antibacterial enamel wet glaze according to claim 6, Features: In step e, the enameling is first carried out at 700-800° C., and then at 800-900° C. for 30 minutes to obtain an enameled ware.
8. The method for using the antibacterial enamel wet glaze according to claim 6, Features: In step e, the enameling is carried out in an environment isolated from oxygen.