A process for preparing a monolithically formed Ti4O7 ceramic electrode by TiC reduction.

The TiC reduction method was used to prepare a one-piece Ti4O7 ceramic electrode, which solved the problems of complex operation, safety and high cost in the existing technology, and realized the industrial production of efficient and low-cost Ti4O7 ceramic electrodes, with a significant improvement in catalytic efficiency.

CN118495942BActive Publication Date: 2026-11-17DALIAN POLYTECHNIC UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410583078.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2026-11-17
Estimated Expiration
2044-05-11

AI Technical Summary

Technical Problem

Existing technologies for preparing Magneille phase Ti4O7 ceramic electrodes suffer from complex operation, difficulty in ensuring safety, and high cost, making it difficult to achieve industrial mass production.

Method used

The TiC reduction method is used to prepare an integrally formed Ti4O7 ceramic electrode by mixing titanium dioxide, titanium carbide and binder in a certain proportion and then calcining them under an inert atmosphere. The specific steps include mixing, pressing and calcining at 1130-1160℃ for 1-4 hours.

Benefits of technology

This method enables the efficient preparation of high-hardness, high-purity Ti4O7 ceramic electrodes, which is safe, low-cost, suitable for industrial production, and has a higher catalytic efficiency than traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004834668820000051
    Figure BDA0004834668820000051
  • Figure HDA0004834668830000011
    Figure HDA0004834668830000011
  • Figure HDA0004834668830000012
    Figure HDA0004834668830000012
Patent Text Reader

Abstract

This invention provides a process for preparing a one-piece Ti4O7 ceramic electrode by TiC reduction, comprising the following steps: Weighing raw materials titanium dioxide, titanium carbide, and binder according to a mass ratio of titanium dioxide:titanium carbide:binder = (5-10):(1-1.5):1, thoroughly mixing and grinding, pressing into sheets, then sintering under an inert atmosphere, and cooling to obtain the product. This method can produce a one-piece Ti4O7 ceramic electrode with higher hardness than traditional ceramic electrodes prepared using carbon as a reducing agent. Furthermore, the Ti4O7 prepared by this method has high purity and high reactivity. Under constant current power supply conditions used in industry, it achieves a degradation rate of 79.59% for high-concentration, recalcitrant organic pollutant Reactive Brilliant Blue KN-R. The method is simple to operate, highly safe, requires minimal equipment, does not require a vacuum environment, shortens the production cycle, reduces production costs, and allows for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of conductive materials, catalytic chemical materials, and new energy, and specifically to a process for preparing an integrally formed Ti4O7 ceramic electrode by TiC reduction. Background Technology

[0002] With the development of society and technology, a large amount of wastewater is generated, placing a serious burden on the environment, especially polluting the water environment. Therefore, how to better solve the water pollution problem has attracted much attention. Titanium suboxide is an excellent active electrode material with high blackness. Magneli phase Ti4O7 exhibits good conductivity at room temperature, with a single crystal conductivity of 1500 Scm. -1 Bulk density: 3.15 g / cm³ 3 ~9.18 / cm 3 Magneli phase Ti4O7 exhibits high chemical stability, excellent corrosion resistance, and wear resistance, surpassing typical industrial electrode materials. Furthermore, due to its superior electrochemical properties, high oxygen evolution potential, and ease of anodic oxidation, Magneli phase Ti4O7 is widely used in the environmental protection and water treatment industries.

[0003] The preparation of Magneli phase compounds is typically carried out at high temperatures using reducing agents such as Ti, H2, C, and NH3. Existing technologies for preparing Magneli phase compounds mainly employ carbothermal reduction and H2 thermal reduction techniques. In carbothermal reduction, carbon black and organic carbon sources are the primary carbon reducing agents. While these are inexpensive and operate at relatively low temperatures, the carbon sources cannot be fully mixed with titanium dioxide, and the resulting monolithic electrodes exhibit extremely poor hardness. H2 thermal reduction is difficult to control in terms of reduction degree, and its safety is challenging to guarantee. These technologies are not suitable for industrial mass production; therefore, there is a strong need for a method that is easy to operate, ensures production safety, and keeps costs low. Summary of the Invention

[0004] This invention provides a process for preparing an integrally formed Ti4O7 ceramic electrode by TiC reduction, which is simple, has a short production cycle, and low cost.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A process for preparing an integrally formed Ti4O7 ceramic electrode by TiC reduction, comprising the following steps:

[0006] Step 1: Weigh out the raw materials titanium dioxide, titanium carbide and binder according to the mass ratio of titanium dioxide: titanium carbide: binder = (5~10):(1~1.5):1, mix them thoroughly and grind them, compress them into tablets to obtain the precursor matrix tablets;

[0007] Step 2: The precursor substrate sheet obtained in Step 1 is placed in a ceramic boat and then placed in a tube furnace. An inert atmosphere is introduced into the furnace cavity, and after the air in the furnace is purged, it is heated to 1130-1160℃ (preferably 1140-1150℃) at a heating rate of 5-20℃ / min. After calcination for 1-4 hours (preferably 1.5-3 hours), it is cooled to room temperature to obtain a Ti4O7 ceramic electrode.

[0008] Preferably, in step 1, the adhesive comprises polypropylene powder and polyvinyl butyral mixed in a mass ratio of (0.5-1.5):(0.5-1.5) (preferably 1:1).

[0009] Preferably, in step 1, the polypropylene powder and polyvinyl butyral in the adhesive have a powder particle size of 5-10 μm after mixing.

[0010] Preferably, in step 1, the titanium dioxide is anatase titanium dioxide.

[0011] Preferably, in step 1, the titanium dioxide has a particle size of 1-2 μm and a purity of 99.9%.

[0012] Preferably, in step 1, the titanium carbide has a particle size of 2-4 μm and a purity of 99%.

[0013] Preferably, in step 1, the tableting step is: dry pressing, with a pressure of 50-100MPa (preferably 50-80MPa) and a time of 60-180s (preferably 60-100s).

[0014] Preferably, the precursor substrate sheet includes structures such as circular, square, round-square, rectangular, triangular, and tubular.

[0015] Preferably, in step 2, the inert atmosphere is argon; the argon is high-purity argon with a purity of 99.999%.

[0016] Preferably, in step 2, the porcelain boat is located at the center of the furnace cavity to ensure that its height from the furnace cavity is basically the same.

[0017] The beneficial effects of this invention are:

[0018] (1) Magnesite phase Ti4O7 is the phase with the best conductivity and is an excellent conductive material. At the same time, it also has many other excellent properties such as good electrochemical stability, strong corrosion resistance and wear resistance. The present invention uses TiC reduction technology to obtain an integrally formed ceramic electrode of Ti4O7. The product prepared by the method of the present invention has higher reactivity and higher catalytic efficiency than ordinary titanium dioxide electrode material under the same conditions.

[0019] (2) The product prepared by the method of the present invention has a higher hardness than the ceramic electrode prepared by the traditional method using carbon source as reducing agent.

[0020] (3) TiC is used as both a reactant and a reducing agent. The C and CO generated during the reaction process play a reducing role and are eventually discharged as gas. There are no residual carbon impurities, and the product has high phase purity.

[0021] (4) This method uses physical grinding and then calcination in the temperature range of 1130 to 1160℃ to obtain the product. It is simple to operate, safe, does not require a vacuum environment, has low equipment requirements, and has a wide range of reducing atmosphere sources. It can shorten the production cycle, reduce production costs, and can be used for large-scale industrial production. Attached Figure Description

[0022] Figure 1 This is a physical image of the precursor substrate sheet prepared in Example 1 of the present invention.

[0023] Figure 2 This is a physical image of the Ti4O7 ceramic electrode prepared in Example 1 of the present invention.

[0024] Figure 3 The image shows the XRD pattern of the Ti4O7 ceramic electrode prepared in Example 1 of this invention.

[0025] Figure 4 This is a SEM image of the Ti4O7 ceramic electrode prepared in Example 1 of the present invention.

[0026] Figure 5 This is a diagram showing the effect of using a Ti4O7 ceramic electrode as the anode material to degrade active Brilliant Blue KN-R. Detailed Implementation

[0027] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.

[0028] Unless otherwise specified, the raw materials used in the following examples are all commercially available products. The titanium carbide has a particle size of 2-4 μm and a purity of 99%; the titanium dioxide has a particle size of 1-2 μm and a purity of 99.9%; and the argon gas is high-purity argon gas with a purity of 99.999%.

[0029] A method for preparing a one-piece Ti4O7 ceramic electrode by TiC reduction, the method comprising the following steps:

[0030] Step 1: Use an agate mortar to thoroughly mix and grind titanium dioxide powder, titanium carbide powder and binder at a mass ratio of (5-10):(1-1.5):1 until the mixture is uniform. Then, put it into a mold and press it with a pressure of 50-100MPa to obtain the precursor matrix sheet.

[0031] The titanium dioxide powder is anatase type; the binder is composed of 1:1 polypropylene powder (PP) and polyvinyl butyral (PVB), and the powder particle size after mixing the binder is 5-10 μm.

[0032] The titanium dioxide powder, titanium carbide powder, and binder are thoroughly mixed and ground to form a powder particle size of 1–2 μm.

[0033] Step 2: Place the precursor substrate sheet obtained in Step 1 in a ceramic boat, and then place the ceramic boat in a tube furnace, ensuring that it is centered within the furnace cavity. Seal the tube furnace. Introduce high-purity argon gas for 20–30 minutes to purge the air. Heat the furnace to 1130–1160°C at a heating rate of 5–20°C / min, and calcine for 1–4 hours. After holding at this temperature, cool to room temperature to obtain the Ti4O7 ceramic electrode.

[0034] The precursor substrate sheet includes structures such as circular, square, round-square, rectangular, triangular, and tubular.

[0035] Example 1

[0036] A method for preparing a one-piece Ti4O7 ceramic electrode by TiC reduction, the method comprising the following steps:

[0037] Step 1: Using an agate mortar and pestle, thoroughly mix and grind titanium dioxide powder, titanium carbide powder, and binder at a mass ratio of 7:1.2:1 until uniformly mixed. Then, pour the mixture into a mold and press it under a pressure of 60 MPa to obtain a precursor substrate sheet with a diameter of 1.4 cm and a thickness of 2 mm. A picture of the actual precursor substrate sheet is shown below. Figure 1 As shown.

[0038] The titanium dioxide powder is anatase type with a particle size of 2 μm.

[0039] The adhesive is composed of a 1:1 ratio of polypropylene powder (PP) and polyvinyl butyral (PVB), with a powder particle size of 10 μm. The molecular weight of the polypropylene powder is 42.08, and the molecular weight of the polyvinyl butyral is 40,000-70,000.

[0040] Step 2: Place the precursor substrate sheet obtained in Step 1 in a ceramic boat, which is then placed in a tube furnace, ensuring it is centered within the furnace cavity and at roughly the same height. Seal the tube furnace. Purge with high-purity argon gas for 20 minutes to purge air. Heat to 1145°C at a rate of 20°C / min, calcine for 2 hours, and then cool to room temperature to obtain the Ti4O7 ceramic electrode. Figure 2The image shown is a physical photograph of the Ti4O7 ceramic electrode prepared in this embodiment. It can be seen that the sheet remains intact after firing, and its hardness is higher than that of the ceramic electrode prepared in Comparative Example 1 using a traditional carbon source as a reducing agent.

[0041] XRD tests were performed on the prepared Ti4O7 ceramic electrode samples, such as... Figure 3 As shown, a comparison with the PDF50-0787 standard card for Ti4O7 reveals that the sample is pure phase Ti4O7 without any impurities.

[0042] The prepared Ti4O7 ceramic electrode sample was ground into powder and observed under a scanning electron microscope, such as... Figure 4 As shown in the figure, the Ti4O7 ceramic electrode has a high surface porosity, resulting in a larger specific surface area compared to materials with no or few pores of the same volume. This leads to a larger effective contact area with wastewater and more reaction sites for the same volume, thus resulting in higher degradation efficiency.

[0043] In this embodiment, the precursor substrate sheet includes structures such as circular, square, round square, rectangular, triangular, and tubular.

[0044] Comparative Example 1

[0045] A method for preparing titanium dioxide anode material, the method comprising the following steps:

[0046] Step 1: Use an agate mortar and pestle to thoroughly mix and grind the titanium dioxide powder and binder at a mass ratio of 7:1 until uniformly mixed. Then, fill the mixture into a mold and press it under a pressure of 60 MPa to obtain a substrate sheet with a diameter of 1.4 cm and a thickness of 2 mm. The titanium dioxide powder is anatase type with a particle size of 2 μm.

[0047] The adhesive is composed of a 1:1 ratio of polypropylene powder (PP) and polyvinyl butyral (PVB), with a powder particle size of 10 μm. The molecular weight of the polypropylene powder is 42.08, and the molecular weight of the polyvinyl butyral is 40,000-70,000.

[0048] Step 2: Place the substrate sheet obtained in Step 1 in a ceramic boat, which is then placed in a tube furnace, ensuring it is centered within the furnace cavity and at roughly the same height. Seal the tube furnace. Introduce high-purity argon gas for 20 minutes to purge the air. Heat to 1145°C at a rate of 20°C / min, calcine for 2 hours, and then cool to room temperature after holding at that temperature to obtain the titanium dioxide anode material.

[0049] Example 2

[0050] An experiment was conducted using the Ti4O7 ceramic electrode prepared in Example 1 as the anode material to degrade the active Brilliant Blue KN-R:

[0051] The experimental setup, namely the photoelectrocatalytic activity testing device, consists of three parts: a magnetic stirrer, a photoelectrocatalytic reactor, and a DC regulated power supply. The magnetic stirrer is used to ensure that the dye concentration remains relatively uniform at all times. The DC regulated power supply operates at 120V and 0.09A.

[0052] Prepare 200 mL of a 100 mg / L Reactive Brilliant Blue KN-R solution and add 2.84 g of anhydrous sodium sulfate (Na2SO4) as a supporting electrolyte. Pour the prepared Reactive Brilliant Blue KN-R solution into the electrocatalytic reactor as a simulated dye. Use the Ti4O7 ceramic electrode prepared in Example 1 as the anode and a stainless steel sheet as the cathode, inserting them into the reactor in parallel. Turn on the stirrer and, after the solution is completely mixed, use a 5 mL pipette to take 3 mL of the reactor liquid as sample #1. Start the electrocatalytic reaction by turning on the power, which lasts for 120 min. Throughout the electrocatalytic reaction, take 3 mL of the reactor liquid every 20 min using a 5 mL pipette to sequentially sort the samples.

[0053] After the experiment, the absorbance of all samples at 596 nm was measured using a UV759 ultraviolet spectrophotometer (Shanghai Yidian Analytical Instrument Co., Ltd.). The degradation rate of the reactive brilliant blue KN-R was calculated according to Equation 1. The experimental results are shown in [Figure 1]. Figure 5 It can be seen that the integrally formed Ti4O7 ceramic electrode prepared by TiC reduction can achieve a degradation rate of 79.59% for the high-concentration recalcitrant organic pollutant Reactive Brilliant Blue KN-R.

[0054]

[0055] Where: D - degradation rate, %

[0056] Initial absorbance of A0-Reactive Brilliant Blue KN-R solution;

[0057] A t - Absorbance of active Brilliant Blue KN-R at degradation time t.

[0058] Comparative Example 2

[0059] An experiment was conducted using the titanium dioxide electrode prepared in Comparative Example 1 as the anode material to degrade the active Brilliant Blue KN-R:

[0060] The experimental setup, namely the photoelectrocatalytic activity testing device, consists of three parts: a magnetic stirrer, a photoelectrocatalytic reactor, and a DC regulated power supply. The magnetic stirrer is used to ensure that the dye concentration remains relatively uniform at all times. The DC regulated power supply operates at 120V and 0.09A.

[0061] Prepare 200 mL of a 100 mg / L Reactive Brilliant Blue KN-R solution and add 2.84 g of anhydrous sodium sulfate (Na₂SO₄) as the supporting electrolyte. Pour the prepared Reactive Brilliant Blue KN-R solution into the electrocatalytic reactor as a simulated dye. Use the titanium dioxide electrode prepared in Comparative Example 1 as the anode and a stainless steel sheet as the cathode, insert them into the reactor, place them parallel to each other, and then turn on the stirrer. After the solution is completely mixed, use a 5 mL pipette to take 3 mL of the reactor liquid as sample #1. Turn on the power to start the electrocatalytic reaction, which lasts for 120 min. During the entire electrocatalytic reaction, take 3 mL of the reactor liquid every 20 min using a 5 mL pipette to sort the samples sequentially.

[0062] After the experiment, the absorbance of all samples at 596 nm was measured using a UV759 ultraviolet spectrophotometer (Shanghai Yidian Analytical Instrument Co., Ltd.). The degradation rate of the active bright blue KN-R was calculated to be 25% according to Formula 1 in Example 2.

[0063] By comparing Example 2 and Comparative Document 2, under the condition of constant current power supply used in industry, the degradation rate of high concentration of recalcitrant organic pollutant Reactive Brilliant Blue KN-R by titanium dioxide anode material is only 25%, while the integrally formed Ti4O7 ceramic electrode prepared by TiC reduction can reach 79.59%, and the catalytic efficiency is three times that of ordinary titanium dioxide electrode.

[0064] Comparative Example 3

[0065] A method for preparing an integrated ceramic electrode using traditional carbon source nano-carbon black as a reducing agent, the method comprising the following steps:

[0066] Step 1: Use an agate mortar and pestle to thoroughly mix and grind titanium dioxide powder, nano carbon black and binder at a mass ratio of 7:1.2:1 until the mixture is uniform. Then, put it into a mold and press it with a pressure of 60MPa to obtain a precursor matrix sheet with a diameter of 1.4cm and a thickness of 2mm.

[0067] The titanium dioxide powder is anatase type with a particle size of 2 μm.

[0068] The adhesive is composed of a 1:1 ratio of polypropylene powder (PP) and polyvinyl butyral (PVB), with a powder particle size of 10 μm. The molecular weight of the polypropylene powder is 42.08, and the molecular weight of the polyvinyl butyral is 40,000-70,000.

[0069] Step 2: The precursor substrate sheet obtained in Step 1 is placed in a ceramic boat, which is then placed in a tube furnace, ensuring that it is centered within the furnace cavity. The tube furnace is then sealed. High-purity argon gas is introduced and purged for 20 minutes to remove air. The temperature is then increased to 1145°C at a rate of 20°C / min, and calcined for 2 hours. After holding at this temperature, the mixture is cooled to room temperature to obtain Ti4O7 powder.

[0070] When using traditional carbon source nano-carbon black as a reducing agent to prepare integrated ceramic electrodes, the resulting product has a loose structure, extremely poor hardness, and is extremely brittle. It is impossible to obtain an integrated electrode through firing, and it becomes powdery after firing. Therefore, traditional carbon sources are not suitable for use in the preparation of integrated ceramic electrodes.

[0071] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A process for the reduction of TiC to produce integrally formed Ti407 ceramic electrodes, characterized in that, Includes the following steps: Step 1: Weigh the raw materials titanium dioxide, titanium carbide and binder according to the mass ratio of titanium dioxide: titanium carbide: binder = (5~10):(1~1.5):1, mix them thoroughly and grind them, compress them into tablets to obtain the precursor matrix tablets; Step 2: The precursor substrate sheet obtained in Step 1 is placed in a ceramic boat and placed in a tube furnace. An inert atmosphere is introduced into the furnace cavity. After the air in the furnace is purged, the temperature is raised to 1130-1160℃ at a heating rate of 5-20℃ / min. After calcination for 1-4 hours, the temperature is cooled to room temperature to obtain the Ti4O7 ceramic electrode. In step 1, the adhesive comprises polypropylene powder and polyvinyl butyral mixed in a mass ratio of (0.5~1.5):(0.5~1.5); In step 2, the inert atmosphere is argon.

2. The process for the reduction of TiC to produce monolithically formed Ti4O7 ceramic electrodes according to claim 1, characterized in that, In step 1, the particle size of the adhesive is 5-10 μm.

3. The process for preparing an integrally formed Ti4O7 ceramic electrode by TiC reduction according to claim 1, characterized in that, In step 1, the titanium dioxide is anatase titanium dioxide.

4. The process for preparing an integrally formed Ti4O7 ceramic electrode by TiC reduction according to claim 3, characterized in that, In step 1, the titanium dioxide has a particle size of 1~2μm and a purity of 99.9%.

5. The process for preparing an integrally formed Ti4O7 ceramic electrode by TiC reduction according to claim 1, characterized in that, In step 1, the titanium carbide has a particle size of 2~4μm and a purity of 99%.

6. The process for preparing an integrally formed Ti4O7 ceramic electrode by TiC reduction according to claim 1, characterized in that, In step 1, the tableting process is as follows: dry pressing, with a pressure of 50-100 MPa and a time of 60-180 s.

7. The process for preparing an integrally formed Ti4O7 ceramic electrode by TiC reduction according to claim 1, characterized in that, The precursor substrate sheet includes circular, square, round-square, rectangular, triangular, or tubular structures.

8. The process for preparing an integrally formed Ti4O7 ceramic electrode by TiC reduction according to claim 1, characterized in that, In step 2, the argon gas is high-purity argon gas with a purity of 99.999%.

9. In the process of preparing an integrally formed Ti4O7 ceramic electrode by TiC reduction according to claim 1, the ceramic boat in step 2 is located at the center of the furnace cavity.

Citation Information

Patent Citations

  • Porous ceramic products of titanium sub-oxides

    CN110088062A

  • Preparation method of Ti4O7 ceramic electrode

    CN113416070A

  • Ti4O7 powder material and preparation method thereof

    CN117776257A