A migration-resistant rubber antioxidant and a preparation method and application thereof
By using EMA modification to prepare the migration-resistant rubber antioxidant E2P, the processing difficulties of existing aniline antioxidants were solved, achieving a highly efficient and environmentally friendly rubber anti-aging effect and improving the migration resistance and aging performance of rubber.
Patent Information
- Application Number
- CN202410569500.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-05-09
AI Technical Summary
Existing aniline antioxidants suffer from problems such as inconvenient processing of oily liquids, cumbersome production, high cost, long reaction time, and reproductive toxicity, making it difficult to meet the multifunctional and environmentally friendly needs of the rubber industry.
3,4-Epoxycyclohexylmethyl methacrylate (EMA) was used as a modifier and reacted with p-aminodiphenylamine in hexafluoroisopropanol solvent to generate migration-resistant rubber antioxidant E2P. The product was synthesized in a one-pot process to obtain a dark brown solid product, simplifying the processing.
It improves the processing convenience of rubber, reduces toxicity, enhances the migration resistance and aging resistance of antioxidants, meets the requirements of green chemistry, and reduces production costs.
Smart Images

Figure CN118496110B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of multifunctional rubber additives, specifically relating to a migration-resistant rubber antioxidant, its preparation method, and its application. Background Technology
[0002] Rubber, as an important strategic resource, plays an irreplaceable role in various industries. The aging process of rubber is irreversible, causing significant damage to the internal structure, appearance, performance, and overall value of rubber materials after aging. Unsaturated rubbers (such as natural rubber (NR) and butadiene rubber (BR)) have double bonds in their molecular backbone, making them prone to reaction with oxidants in the air, such as oxygen and ozone. This reaction destabilizes the double bonds within the rubber molecules, potentially leading to self-crosslinking and increased crosslinking density. Macroscopically, this manifests as hardening and brittleness, altering the mechanical properties of the rubber material, such as tensile strength, elongation at break, and hardness. The most direct solution is to add suitable antioxidants to the rubber formulation. Antioxidants are indispensable additives in the rubber industry because they effectively prevent the aging and degradation of rubber products, thereby improving their reliability and service life. Generally, aniline antioxidants, due to their highly reactive antioxidant groups, possess the strongest antioxidant properties among all antioxidant types. However, the presence of the aniline group generally results in a darker color, making them suitable only for products insensitive to color contamination, such as tire manufacturing and automotive gaskets. Traditional aniline antioxidants, such as antioxidant 4020, often possess only a single antioxidant group, failing to adequately meet the current development requirements of multifunctional, environmentally friendly, and low-cost rubber additives. Therefore, there is an urgent need to develop a new type of migration-resistant antioxidant to meet the needs of the current rubber industry. p-Aminodiphenylamine (PPDA or RT-Peptide) is an important precursor to commercial aniline antioxidants such as antioxidants 4010 and 4020, and has also become one of the main raw material monomers for antioxidant modification. Its primary amine group has high reactivity and can react with many active groups. Glycidyl acrylate (ether) compounds are currently a popular PPDA modification reactant. On one hand, glycidyl acrylate (ether) compounds contain epoxy groups, which can undergo an epoxy ring-opening reaction with the primary amine groups in PPDA, allowing glycidyl acrylate (ether) to be grafted onto the PPDA molecule. On the other hand, glycidyl acrylate (ether) compounds contain carbon-carbon double bonds at the other end. Studies have shown that they can co-crosslink with the unsaturated rubber backbone, allowing the entire molecule to be mounted on the rubber molecular chain, increasing the difficulty of antioxidant molecule migration and alleviating the "blooming" phenomenon of traditional antioxidants on the rubber surface.Among common glycidyl acrylates (ethers), 4-hydroxybutyl acrylate glycidyl ether (HAGE) has a long carbon chain, which can improve the compatibility between antioxidants and rubber. However, this substance is expensive, and as rubber antioxidants are a widely used chemical raw material, the high price of HAGE limits its application in antioxidant modification. Allyl glycidyl ether (AGE) is inexpensive, but it is highly toxic, especially to the human reproductive system. Therefore, using AGE as a modifier for aniline antioxidants does not conform to the principles of "green chemistry". Glycidyl methacrylate (GMA) is a popular aniline modification reactant. It has the advantages of simple molecular structure, high reactivity, and lower toxicity than AGE. Currently, there has been relatively detailed research in the field of GMA-modified aniline antioxidants.
[0003] Patent application CN 110343207 A discloses a rubber antioxidant using styrene-GMA copolymer as a carrier and its preparation method. The rubber antioxidant is prepared by reacting styrene-GMA copolymer with an amine antioxidant. The specific preparation method includes dissolving the styrene-GMA copolymer in a solvent at room temperature, adding an amine antioxidant and a catalyst, heating, stirring, and reacting to obtain a crude product. This crude product is then flocculated and washed with a flocculant, separated into phases, filtered to obtain a solid product, and finally dried. The rubber antioxidant prepared by this method exhibits better stability and lower migration compared to traditional antioxidants. However, this method of mounting antioxidant groups onto the macromolecular chain has a fatal weakness: the grafting rate of the reactive sites (GMA) is difficult to increase. If the GMA grafting rate is too high, the system viscosity increases, making intermolecular cross-linking more likely. If the grafting rate is too low, insufficient antioxidant groups cannot be attached, thus reducing the overall antioxidant effect. Therefore, the application of this method is greatly limited.
[0004] Patent application CN 115260585 A discloses a method for using GMA-modified p-aminodiphenylamine as a rubber antioxidant. In this patent, researchers directly mix GMA and PPDA. GMA is an oily liquid at room temperature, which can dissolve PPDA to form an antioxidant composition. This antioxidant composition is then directly blended and plasticized with raw rubber. After uniform mixing, the compound is vulcanized. The high temperature and pressure during rubber vulcanization promote the epoxy ring-opening reaction between GMA and PPDA to generate GMA-PPDA. This composition exhibits both antioxidant and migration-resistant properties when applied to rubber. However, because this composition is an oily liquid at room temperature, leakage is likely during processing, resulting in antioxidant loss and making it difficult to achieve the expected antioxidant performance. Furthermore, the vulcanization time generally does not exceed 30 minutes. Within such a short time, it is difficult to ensure that PPDA and GMA react completely to generate the target product.
[0005] Patent application CN 115260585 discloses a GMA-modified p-aminodiphenylamine rubber antioxidant and its preparation method. The rubber antioxidant is prepared by reacting p-aminodiphenylamine with the epoxy groups of GMA. Specifically, the preparation method involves heating and stirring p-aminodiphenylamine and GMA to react, obtaining a fluid product, followed by granulation to obtain the final antioxidant product. Compared with traditional antioxidants, the rubber antioxidant prepared by this method has good stability and low migration rate. However, this method has a long reaction time and requires high temperature. Furthermore, at room temperature, the epoxy ring-opening product of GMA and p-aminodiphenylamine is a viscous liquid, requiring subsequent granulation for convenient processing, which undoubtedly increases the complexity of the process and production costs.
[0006] In summary, GMA-modified diphenylamine antioxidants have the following problems: (1) the product is an oily liquid, which is not conducive to the subsequent processing of rubber composites; (2) granulation of the oily product increases the complexity of production and raises production costs; (3) the reaction time is long and energy consumption is high; (4) although the toxicity is lower than that of AGE, GMA still has reproductive toxicity. Therefore, it is urgent to develop a new high-performance rubber antioxidant to overcome the problems existing in the current technology. Summary of the Invention
[0007] The primary objective of this invention is to provide a method for preparing a migration-resistant rubber antioxidant. This invention uses 3,4-epoxycyclohexylmethyl methacrylate (EMA) as a substitute for glycidyl methacrylate (GMA) and as a donor for the methacrylic acid group in the aniline antioxidant. Compared to GMA, EMA has a larger molecular weight and lower physiological toxicity to humans.
[0008] Another object of the present invention is to provide a migration-resistant rubber antioxidant prepared by the above method. The final product of the present invention, E2P, is a dark brown solid, which is beneficial for subsequent rubber processing.
[0009] Another object of the present invention is to provide the application of the above-mentioned migration-resistant rubber antioxidant. The present invention synthesizes an acrylate-containing migration-resistant antioxidant, and through experimental research and data analysis, applies it to unsaturated rubber, thereby demonstrating the feasibility of using E2P antioxidants as high-performance rubber antioxidants.
[0010] Another object of the present invention is to provide a high-performance rubber containing the above-mentioned anti-migration antioxidant.
[0011] The objective of this invention is achieved through the following technical solution:
[0012] A method for preparing a migration-resistant rubber antioxidant includes the following steps:
[0013] (1) Dissolve and react p-aminodiphenylamine and 3,4-epoxycyclohexylmethyl methacrylate in an organic solvent to obtain a reaction solution;
[0014] (2) The washing reaction solution was subjected to vacuum distillation and drying to obtain a migration-resistant rubber antioxidant.
[0015] In step (1):
[0016] The p-aminodiphenylamine is preferably p-aminodiphenylamine with a purity of 99 wt%.
[0017] The 3,4-epoxycyclohexylmethyl methacrylate is preferably 3,4-epoxycyclohexylmethyl methacrylate with a purity of 99 wt%.
[0018] The organic solvent is preferably hexafluoroisopropanol.
[0019] The hexafluoroisopropanol is preferably hexafluoroisopropanol with a purity of 99 wt%.
[0020] The molar ratio of p-aminodiphenylamine to 3,4-epoxycyclohexylmethyl methacrylate is preferably 1:2 to 4; more preferably 1:2.2.
[0021] The organic solvent is used as a reaction medium and does not participate in the reaction; its volume (mL) is preferably 0.5 to 2 times the total mass (g) of p-aminodiphenylamine and 3,4-epoxycyclohexylmethyl methacrylate; more preferably, it is 1 to 1.5 times the total mass (g) of p-aminodiphenylamine and 3,4-epoxycyclohexylmethyl methacrylate.
[0022] The preferred reaction conditions are under a nitrogen protective atmosphere, at 60–80°C and 800–1000 rpm for 1–6 h; more preferably, under a nitrogen protective atmosphere, at 70°C and 800 rpm for 3 h.
[0023] The washing reagent in step (2) is preferably a mixture of n-heptane and chloroform; more preferably a mixture of n-heptane and chloroform in a volume ratio of 3:0.5 to 1.5; and most preferably a mixture of n-heptane and chloroform in a volume ratio of 3:1.
[0024] In step (2):
[0025] The washing is preferably carried out under stirring.
[0026] The stirring speed is preferably 400-600 rpm.
[0027] The preferred conditions for vacuum distillation are distillation at 60–80°C for 0.5–2 hours; more preferably, distillation at 70°C for 1.5 hours.
[0028] The drying process is preferably vacuum drying.
[0029] The drying conditions are preferably 60-80°C for 0.5-2 hours; more preferably 70°C for 1.5 hours.
[0030] A migration-resistant rubber antioxidant is obtained by the above preparation method.
[0031] The above-mentioned anti-migration rubber antioxidants are used as anti-migration agents for rubber vulcanization.
[0032] The rubber is preferably unsaturated rubber; more preferably, it is at least one of natural rubber and butadiene rubber.
[0033] A high-performance rubber comprising unsaturated rubber and the aforementioned migration-resistant rubber antioxidant.
[0034] The migration-resistant rubber antioxidant and the unsaturated rubber are preferably mixed in a mass ratio of 1 to 6:100; more preferably in a mass ratio of 3:100.
[0035] A rubber tread compound comprising the following components by weight: 100 parts rubber, 30-50 parts carbon black, 3-4 parts zinc oxide, 2-3 parts stearic acid, 1-15 parts sulfur, and 1-6 parts of the above-mentioned migration-resistant rubber antioxidant; preferably comprising the following components by weight: 100 parts rubber, 50 parts carbon black, 3.5 parts zinc oxide, 2.4 parts stearic acid, 1.2 parts sulfur, and 3 parts of the above-mentioned migration-resistant rubber antioxidant.
[0036] The rubber is preferably unsaturated rubber; more preferably, it is at least one of natural rubber and butadiene rubber.
[0037] The carbon black is preferably at least one of N234 carbon black and N330 carbon black.
[0038] Principles and overview of the invention:
[0039] This invention synthesizes a rubber antioxidant with high anti-aging effect and high migration resistance. Anti-aging groups are linked using epoxy groups as linking points, thereby synthesizing a rubber antioxidant with high anti-aging effect and high migration resistance, namely, p-aminodiphenylamine (PPDA) two-grafted 3,4-epoxycyclohexylmethyl methacrylate (EMA) antioxidant EMA2-PPDA (E2P). This antioxidant is then applied to unsaturated rubbers, including but not limited to natural rubber and butadiene rubber, and its mechanical properties, aging properties, and migration resistance are tested to characterize its high migration resistance and anti-aging effect.
[0040] This invention uses p-aminodiphenylamine as a precursor and 3,4-epoxycyclohexylmethyl methacrylate as an acrylate donor. The target product is generated through a ring-opening reaction between the nucleophilic primary amine group and the epoxy group. This step requires nitrogen protection and stirring. Then, using hexafluoroisopropanol as a catalyst, the migration-resistant rubber antioxidant p-aminodiphenylamine-grafted 3,4-epoxycyclohexylmethyl methacrylate was successfully synthesized. The antioxidant product obtained by this method is pure and requires no subsequent granulation or curing treatment; it can be used directly. The acrylate in the antioxidant molecule can participate in vulcanization crosslinking with the unsaturated backbone of the unsaturated rubber and enter the crosslinking network.
[0041] The high-performance, multifunctional rubber antioxidant p-aminodiphenylamine di-grafted 3,4-epoxycyclohexylmethyl methacrylate provided by this invention is used as an antioxidant for unsaturated rubber, wherein the unsaturated rubber can be selected from natural rubber and cis-butadiene rubber. The antioxidant was added to a rubber formulation, and its application value was tested. Its aging resistance and migration resistance are significantly better than those of commercially available antioxidant 4020 (also known as DMBPPD), and its production process does not use hazardous chemical raw materials such as toxic gases or highly toxic substances.
[0042] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0043] (1) The preparation method provided by the present invention uses hexafluoroisopropanol as a solvent and catalyst, which greatly accelerates the reaction rate. After the reaction is completed, it can be recycled and reused. Moreover, hexafluoroisopropanol has low toxicity and a low boiling point (59°C at normal pressure), making it very easy to separate from the reaction system.
[0044] (2) The present invention adopts a one-pot reaction, which is simple to operate, has a mild reaction environment and conditions, and has a high yield of the final product.
[0045] (3) Compared with traditional GMA-aniline modified antioxidants, EMA modified antioxidants are solid products, which facilitates subsequent rubber processing and blending processes.
[0046] (4) Compared with traditional GMA-aniline modified antioxidants, EMA modified antioxidants have larger molecular weights and better migration resistance.
[0047] (5) Compared with GMA, EMA is less toxic and conforms to the concept of "green chemistry".
[0048] (6) The antioxidant E2P prepared in this invention has better aging resistance and migration resistance as a rubber additive than GMA-modified antioxidant and traditional antioxidant 4020. Attached Figure Description
[0049] Figure 1 The images show the FT-IR spectra of the precursor and product involved in Example 1.
[0050] Figure 2 The above are the 1H NMR spectra of the precursor and product involved in Example 1. Detailed Implementation
[0051] The following embodiments further illustrate specific implementations of the present invention, but the implementation and protection of the present invention are not limited thereto. It should be noted that any processes not specifically described below are those that can be implemented or understood by those skilled in the art by referring to existing technology. Reagents or instruments whose manufacturers are not specified are considered to be conventional products that can be purchased commercially.
[0052] Example 1
[0053] A three-necked flask was placed in an oil bath. After assembling the thermometer and reflux condenser, 0.022 mol (4.31 g) of 3,4-epoxycyclohexylmethyl methacrylate (EMA, molecular weight 196.24) and 0.01 mol (1.84 g) of p-aminodiphenylamine (PPDA, molecular weight 184.237) were weighed out. The weighed p-aminodiphenylamine and 3,4-epoxycyclohexylmethyl methacrylate were added to the flask, and a magnetic stirrer was placed inside. The system appeared as a dark brown oily substance. Nitrogen gas was introduced, and under a nitrogen protective atmosphere, the temperature was raised to 70°C. Magnetic stirring was started (800 rpm), and then 6 mL of hexafluoroisopropanol was added dropwise to dissolve the reactants. After thorough mixing, the reaction was allowed to proceed for 3 hours, yielding a dark brown, viscous liquid. Excess EMA monomer was removed by washing with a mixed organic solution (heptane and chloroform in a 3:1 volume ratio). The specific procedure was as follows: 100 mL of the mixed organic solution was added to a beaker, and a magnetic stirrer was placed inside. The mixture was stirred at 500 rpm. A dark brown, viscous liquid was slowly added dropwise to flocculate the mixture. The liquid precipitated to the bottom, and the excess EMA monomer flocculated out, appearing pale yellow (this phenomenon occurs when EMA monomer is added directly to the mixed organic solution, as confirmed by preliminary experiments). The supernatant was removed, and the above procedure was repeated until no more flocculation occurred, at which point the dark brown, viscous liquid was collected. The washed dark brown, viscous liquid was then distilled under reduced pressure at 70°C for 1.5 h to remove excess chloroform, n-heptane, and the catalyst (hexafluoroisopropanol). The product was then vacuum dried at 70°C for 1.5 h in a vacuum drying oven to obtain a dark brown solid, E2P, with a yield of approximately 95%.
[0054] Yield = Actual product quantity / Theoretical product quantity × 100%.
[0055] The theoretical amount of E2P product is calculated based on the reaction coefficient of the chemical reaction. Theoretically, 0.01 mol of p-aminodiphenylamine will react with 0.02 mol of 3,4-epoxycyclohexylmethyl methacrylate to produce 0.01 mol of E2P.
[0056] The FT-IR and 1H NMR spectra of the precursor 3,4-epoxycyclohexylmethyl methacrylate (EMA), p-aminodiphenylamine (PPDA), and the product E2P are shown below. Figure 1 and Figure 2 As shown. From Figure 2 The results show that the peaks displayed by the 1H NMR spectrum correspond to the amount of hydrogen in different chemical environments in the compound, which further proves the successful synthesis of E2P.
[0057] Example 2
[0058] 1.2g of sulfur masterbatch (80% sulfur content), 3g of antioxidant E2P (prepared through Example 1), 3.5g of zinc oxide, 2.4g of stearic acid, and 50g of carbon black N234 were added to 100g of natural rubber (NR-SVR3, Guangzhou Desheng New Materials Co., Ltd.) using an open mill to obtain a compound rubber, denoted as NR-E2P, which was then vulcanized at 150℃. A portion of the obtained vulcanized rubber sheets was aged in an oven at 100℃ for 5 days, and the performance aging rate was tested (defined as: performance parameters before aging / performance parameters after aging × 100%, the same below).
[0059] Comparative Example 1
[0060] A three-necked flask was placed in an oil bath. After attaching the thermometer and reflux condenser, 0.022 mol of glycidyl methacrylate (GMA) (molecular weight 142.15, 3.13 g) and 0.01 mol of p-aminodiphenylamine (PPDA) (1.84 g) were weighed. The weighed p-aminodiphenylamine and glycidyl methacrylate were added to the flask, and a magnetic stirrer was placed inside. Nitrogen gas was introduced, and the temperature was raised to 70°C under a nitrogen protective atmosphere. The magnetic stirrer was turned on (800 rpm), and then 6 mL of hexafluoroisopropanol was added dropwise to dissolve the reactants. After mixing thoroughly, the reaction was allowed to proceed for 3 hours, yielding a purplish-red viscous oily liquid. Excess GMA monomer was removed by washing with a mixed organic solution (heptane and chloroform in a 3:1 volume ratio). The specific procedure was as follows: 100 mL of the mixed organic solution was added to a beaker, and a magnetic stirrer was placed inside. Stirring was started (500 rpm). A purplish-red oily substance was slowly added dropwise for flocculation. The purplish-red oily liquid precipitated to the bottom, and the excess GMA monomer flocculated out, appearing milky white (this phenomenon occurs if GMA monomer is added directly to the mixture, as confirmed by preliminary experiments). The upper layer of liquid was removed, and the above operation was repeated until no more flocculation occurred, at which point the purplish-red oily liquid was collected. The washed purplish-red oily liquid was then distilled under reduced pressure at 70°C for 1.5 h to remove excess chloroform, n-heptane, and catalyst. The product was then vacuum dried in a vacuum drying oven at 70°C for 1.5 h to obtain the oily liquid antioxidant GP, with a yield of approximately 90%.
[0061] Yield = Actual product quantity / Theoretical product quantity × 100%.
[0062] Comparative Example 2
[0063] 1.2g of sulfur masterbatch (sulfur content 80%), 3g of antioxidant 4020 (purchased from Fujian Fuxiang Chemical Co., Ltd.), 3.5g of zinc oxide, 2.4g of stearic acid, and 50g of carbon black N234 were added to 100g of natural rubber (NR-SVR3, Guangzhou Desheng New Materials Co., Ltd.) using an open mill to obtain a compound rubber, designated NR-4020. The compound was vulcanized at 150℃, and a portion of the vulcanized rubber sheets were aged in an oven at 100℃ for 5 days to test the performance aging rate.
[0064] Comparative Example 3
[0065] The compound, denoted as NR-GP, was prepared by adding 1.2g of sulfur masterbatch (80% sulfur content), 3g of antioxidant GP (prepared from Comparative Example 1), 3.5g of zinc oxide, 2.4g of stearic acid, and 50g of carbon black N234 to 100g of natural rubber (NR-SVR3, Guangzhou Desheng New Materials Co., Ltd.) using an open mill. The compound was then vulcanized at 150℃. A portion of the vulcanized rubber sheets was aged in an oven at 100℃ for 5 days to test the aging rate.
[0066] The thermo-oxidative aging performance parameters of the vulcanizates prepared in Examples 2 and 2-3 after 5 days are shown in Table 1. Tensile strength and elongation at break were tested according to standard GB / T528-2009; tear strength was tested according to standard GB / T 529-2008.
[0067] Table 1. Aging performance (100℃ × 5d) of vulcanizates prepared in the examples and comparative examples. Aging rate
[0068] Test Project Example 2 Comparative Example 2 Comparative Example 3 Tensile strength retention rate (%) 79 55 65 Elongation at break retention rate (%) 57 40 45 Tear strength retention rate (%) 71 45 55
[0069] Compared with Comparative Examples 2 and 3, the rubber products of Example 2 showed a significant improvement in performance retention after hot air aging, indicating that the antioxidant E2P prepared in this invention has superior antioxidant properties.
[0070] 1.00 g of the vulcanized rubber sheets prepared in the examples and comparative examples were soaked in 20 mL of anhydrous ethanol for 7 days. The soaking solution was then subjected to ultraviolet spectrophotometry to determine the extraction concentration of the antioxidant under this formulation. The extraction rate of the antioxidant (defined as the ratio of the mass of extracted antioxidant to the mass of antioxidant added to 1.00 g of vulcanized rubber) was calculated, as shown in Table 2.
[0071] The migration resistance of the vulcanizates prepared in the examples and comparative examples is shown in Table 2.
[0072] Table 2 Migration Resistance Test of Vulcanized Rubber
[0073] Test Project Example 2 Comparative Example 2 Comparative Example 3 Extraction rate (%) 2.1 90 8.4
[0074] Compared with Comparative Examples 2 and 3, the antioxidant in Example 2 had a lower extraction rate, indicating better migration resistance.
[0075] The above examples are preferred embodiments of the present invention, but the implementation of the present invention is not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A method for preparing a migration-resistant rubber antioxidant, characterized in that, Includes the following steps: (1) Dissolve and react p-aminodiphenylamine and 3,4-epoxycyclohexylmethyl methacrylate in an organic solvent to obtain a reaction solution; (2) The washing reaction solution was subjected to vacuum distillation and drying to obtain a migration-resistant rubber antioxidant; The organic solvent is hexafluoroisopropanol; The structure of the migration-resistant rubber antioxidant is shown below: 。 2. The method for preparing the migration-resistant rubber antioxidant according to claim 1, characterized in that: The washing reagent is a mixture of n-heptane and chloroform.
3. The method for preparing the migration-resistant rubber antioxidant according to claim 1 or 2, characterized in that: The molar ratio of p-aminodiphenylamine to 3,4-epoxycyclohexylmethyl methacrylate is 1:2 to 4; The amount of the organic solvent used is calculated as 0.5 to 2 times the total mass of p-aminodiphenylamine and 3,4-epoxycyclohexylmethyl methacrylate by volume; wherein, volume is in mL and mass is in g.
4. The method for preparing the migration-resistant rubber antioxidant according to claim 1, characterized in that: The reaction conditions are as follows: under a nitrogen protective atmosphere, at 60–80°C and 800–1000 rpm for 1–6 hours; The washing is carried out under stirring; The conditions for vacuum distillation are distillation at 60–80°C for 0.5–2 hours; The drying process described is vacuum drying.
5. A migration-resistant rubber antioxidant, characterized in that: It is obtained by the preparation method according to any one of claims 1 to 4.
6. The application of the migration-resistant rubber antioxidant according to claim 5 in the preparation of vulcanizing antioxidants for rubber.
7. A high-performance rubber, characterized in that: It contains unsaturated rubber and the migration-resistant rubber antioxidant as described in claim 5.
8. The high-performance rubber according to claim 7, characterized in that: The migration-resistant rubber antioxidant is mixed with the unsaturated rubber at a mass ratio of 1 to 6:
100.
9. A rubber tread compound, characterized in that... It comprises the following components in parts by weight: 100 parts rubber, 30-50 parts carbon black, 3-4 parts zinc oxide, 2-3 parts stearic acid, 1-15 parts sulfur, and 1-6 parts of the migration-resistant rubber antioxidant as described in claim 5.
10. The rubber tread compound according to claim 9, characterized in that: The rubber mentioned is at least one of natural rubber and butadiene rubber; The carbon black is at least one of N234 carbon black and N330 carbon black.
Citation Information
Patent Citations
Rubber anti-aging agent with styrene-glycidyl methacrylate (GMA) copolymer as carrier and preparation method of rubber anti-aging agent
CN110343207A
Anti-aging agent composition as well as preparation method and application thereof
CN115260585A
Novel anti-aging agent as well as preparation method and application thereof