Zinc-based dual-ligand coordination polymer crystal material and preparation method and application thereof
By designing zinc-based double-ligand coordination polymer crystal materials Zn-1 and Zn-2, and utilizing their one-dimensional chain structure and the three-dimensional supramolecular structure formed by hydrogen bonds, the complexity and complexity of existing iron detection methods are solved. Low sensitivity problem, realizing portable, low-cost, high-sensitivity Fe3+ detection, suitable for quality inspection and environmental monitoring.
Patent Information
- Application Number
- CN202410976919.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The existing iron (Fe3+) detection methods are complex, time-consuming, low-sensitivity and high-cost. They lack portable, low-cost, high-sensitivity detection sensors and are difficult to be widely used in actual production and life.
A zinc-based double-ligand coordination polymer crystal material Zn-1 and Zn-2 is designed. Zn ions are combined with flexible dicarboxylic acid and 1,10-phenanthroline ligands to form a one-dimensional chain structure. Hydrogen bonds form a three-dimensional supramolecular structure, which can be used as a fluorescent recognition sensor to quickly detect Fe3+.
It achieves high-sensitivity detection of Fe3+, has good thermal stability and fluorescence recognition capabilities, is suitable for quality inspection and environmental monitoring, and reduces detection costs and operational complexity.
Smart Images

Figure CN118496517B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of crystalline materials, and particularly relates to a zinc-based double-ligand coordination polymer crystal material and a preparation method and application thereof. Background Art
[0002] Fe 3+ Is a typical nutrient, it is one of the most essential elements in the process of hemoglobin formation, DNA synthesis, oxygen storage, etc. But when the concentration exceeds a certain threshold, it becomes harmful, leading to serious physiological disorders such as insomnia, decreased immunity, gastrointestinal dysfunction and cirrhosis. According to the WHO guidelines on drinking water quality, the maximum allowable limit of iron is 0.3 mg / L. However, with the rapid development of industry, iron has become an important source of inorganic pollutants. For example: in industry, a large amount of Fe 3+ The wastewater is directly discharged into rivers; in agricultural production, excessive use of iron-containing fertilizers and pesticides can also lead to Fe 3+ Increased concentrations affect plant growth and even enter the human body through the food chain. 3+ The importance and impact of Fe in biological and environmental systems, therefore, for human health, the environmental 3+ The detection of concentration is very important. Traditional detection methods include inductively coupled plasma, spectroscopy, voltammetry, mass spectrometry, etc. However, traditional detection methods are usually complicated and time-consuming, with low sensitivity, low selectivity and high actual application costs. The development of highly sensitive and rapid specific detection methods has important research significance.
[0003] With the rapid development of science and technology, people pay more and more attention to ecological environment protection and have higher and higher requirements for quality of life. 3+ Detection sensors are attracting more and more attention. In recent years, there are many different materials of Fe 3+ Sensors were invented. But can the new Fe 3+ There are still very few sensors, and the sensitivity of the sensors needs to be further improved. More repeatable and easy-to-operate Fe 3+ Detection sensors need further development. Among them, fluorescence recognition is a commonly used Fe 3+ The identification method has the advantages of low cost and fast analysis speed. The luminescent materials with fluorescent identification function have great application prospects in sensing, and it is expected to prepare detectors that can replace large instruments for portable identification.
[0004] Coordination polymers, also known as complexes, are a new type of organic-inorganic hybrid materials. They are coordination entities with repeated 1, 2 or 3-dimensional extensions formed by self-assembly of inorganic or metal cations / metal clusters and organic ligands through coordination bonds. Compared with traditional hybrid materials, coordination polymers have the advantages of being designable and controllable. Applying the principles of crystal engineering, coordination polymers can select rare earth metal ions with special luminescence when designing their structures, and can also introduce ligands / functional groups with specific properties into the structure. By regulating the structural components, pore size and shape, etc., the purpose of regulating functional applications can be achieved. Therefore, coordination polymers have great potential application value in the field of fluorescence recognition. However, the design and synthesis of coordination polymers seem simple, but so far there is still no mature theory to effectively guide the self-assembly process, and Fe 3+ There are even fewer probes. Compared with rigid ligands, flexible ligands are more prone to flipping and more difficult to predict structures in the ligands of synthetic complexes, so there are fewer studies on flexible ligands. However, due to the variable configuration of flexible ligands, it is easier to synthesize complex materials with novel structures. The present invention is guided by the synthesis of novel zinc complex fluorescent probes, and selects flexible dicarboxylic acid - 2,2'-(1,2-phenylenebis(methylene))bis(sulfuryl) dinicotinic acid as the main ligand. Through the mixed ligand method, a precise design and synthesis of a probe that can be used to quickly identify Fe 3+ The Zn-1 and Zn-2 prepared by the present invention can quickly detect Fe 3+ , can be used as a new type of fluorescence recognition sensor. This material can be used in quality inspection, environmental protection and other fields, and is of great significance for improving food quality and safety and maintaining environmental health. Summary of the invention
[0005] One of the purposes of the present invention is to provide a zinc-based bi-ligand coordination polymer crystal material, wherein the zinc-based bi-ligand coordination polymer crystal material is formed by Zn ions and two ligands through coordination bonds, wherein one ligand is an organic ligand 2,2'-(1,2-phenylenebis(methylene))bis(sulfadiyl) dinicotinic acid H2L, and the chemical structure is as follows:
[0006] ;
[0007] Another ligand is 1,10-phenanthroline (CAS: 66-71-7) phen, the chemical structure of which is shown below:
[0008] .
[0009] The zinc-based dual-ligand coordination polymer crystal material has a one-dimensional chain structure, and the one-dimensional chain structure forms a three-dimensional supramolecular structure through H-bonding.
[0010] Furthermore, the molecular formula of the zinc-based dual-ligand coordination polymer crystal material is [Zn2(L)2(phen)2(H2O)] n (named Zn-1), the Zn-1 belongs to the triclinic system P -1 space group, the unit cell parameters are: a =11.2842(5) Å, b =12.4733(5) Å, c =20.9595(10) Å, α =93.8570(10), β =103.215(2), γ =90.488(2).
[0011] Furthermore, the molecular formula of the zinc-based dual-ligand coordination polymer crystal material is [ZnL(phen)] n (named as Zn-2), the Zn-2 belongs to the triclinic system P -1 space group, the unit cell parameters are: a =9.7389(4) Å, b =11.7190(4) Å, c =12.6870(4) Å, α =80.1720(10), β =89.3640(10), γ =87.2590(10).
[0012] Furthermore, the asymmetric structural unit of Zn-1 contains two different Zn(II), Zn1 and Zn2, wherein the coordination number of Zn1 and Zn2 is 5; Zn1 and Zn2 are coordinated with two N atoms and three O atoms, wherein the N atoms come from the ligand phen, and the three O atoms coordinated by Zn1 come from the two ligands L 2- ; Two of the O atoms coordinated to Zn2 come from ligand L 2- , another O atom comes from the coordinated water molecule;
[0013] In Zn-1, the ligand L 2- All adopt the trans conformation, similar to the Z-configuration; in Zn-1, the ligand L 2- There are two coordination modes. The first is that both carboxyl groups are monodentate coordinated, and the second is that one carboxyl group is monodentate coordinated and the other carboxyl group is chelate coordinated.
[0014] There is no ligand directly connected between Zn1 and Zn2; Zn1 and Zn2 are both connected to two ligands L at the same time. 2- , each L 2- Then connect two Zn(II); based on Zn1 and Zn2 respectively with ligand L 2-Two 1D chain structures are formed; in Zn-1, there is a strong intermolecular H-bonding effect between the two 1D chains formed by Zn1 and Zn2, O9—H9D···O2 and O9—H9C···O4, so the two one-dimensional chain structures are very stable, and the 1D chains can form a three-dimensional supramolecular structure through H bonding.
[0015] Furthermore, the asymmetric structural unit of Zn-2 contains a Zn(II), Zn1. The coordination number is 5, coordinated with two N atoms and three O atoms, the N atom comes from the ligand phen, and the three O atoms all come from the two ligands L 2- ; In Zn-2, ligand L 2- There is only one coordination mode, one carboxyl group is monodentate coordinated and the other carboxyl group is chelate coordinated; each Zn(II) is connected to two ligands L 2- , each L 2- Then two Zn(II) are connected to form a 1D chain structure.
[0016] In Zn-2, there are weak hydrogen bonds between molecules in the one-dimensional chain structure. A The distance between them is greater than 2.5 Å, and through weak H-bonding, a three-dimensional supramolecular structure is formed between the 1D chain structures.
[0017] The present invention also provides a method for preparing the zinc-based dual-ligand coordination polymer crystal material Zn-1, comprising the following steps:
[0018] Weigh ZnCl2·2H2O, main ligand H2L and auxiliary ligand phen into a 20.0 ml pressure-resistant thick glass sample bottle, and measure DMF / water (1:1) mixed solution into the above glass sample bottle. Finally, cover the bottle cap and seal the sample bottle, place it in a forced air drying oven, and heat it at 90.0℃ for 3 days. After the system slowly cools to room temperature, take out the sample bottle to obtain a colorless rod-shaped complex [Zn2(L)2(phen)2(H2O)] n We refer to this complex as Zn-1.
[0019] Furthermore, the mass ratio of the main ligand H2L to the auxiliary ligand phen is 2:1, the added amount of the DMF / water mixed liquid is limited to 1 mg of the auxiliary ligand phen corresponding to 1 ml of the mixed solution, and the mass ratio of the ZnCl2·2H2O to the main ligand H2L is 13.6:20.
[0020] The present invention also provides a method for preparing the zinc-based dual-ligand coordination polymer crystal material Zn-2, comprising the following steps:
[0021] Weigh ZnSO4·7H2O, main ligand H2L and auxiliary ligand phen into a 20.0 ml pressure-resistant thick glass sample bottle, and measure DMF / water (1:1) mixed solution into the above glass sample bottle. Finally, cover the bottle cap and seal the sample bottle, place it in a forced air drying oven, and heat it at 90.0℃ for 3 days. After the system slowly cools to room temperature, take out the sample bottle to obtain a colorless rod-shaped complex [ZnL(phen)] n We refer to this complex as Zn-2.
[0022] Furthermore, the mass ratio of the main ligand H2L to the auxiliary ligand phen is 2:1, the added amount of the DMF / water mixed liquid is limited to 1 mg of the auxiliary ligand phen corresponding to 1 ml of the mixed solution, and the mass ratio of the ZnCl2·2H2O to the main ligand H2L is 28.7:20.
[0023] The present invention also provides the application of the zinc-based dual-ligand coordination polymer crystal material in metal ion recognition, especially for Fe 3+ Identify applications.
[0024] Beneficial technical effects of the present invention:
[0025] (1) Generally speaking, coordination polymers with good thermal stability are more suitable for identification materials and are easier to apply to high temperature and complex environments. The thermal degradation process of coordination polymers is often accompanied by the breaking of coordination bonds and the combustion of ligands. Therefore, the thermal stability of coordination polymers is generally related to the strength of coordination bonds and the number of node ligand links. 2+ The coordination numbers of Zn-1 and Zn-2 complexes of the present invention are 4, 5 and 6. 2+ The coordination number of Zn-1 is 5, and Zn2 in Zn-1 has a coordinated water molecule. Therefore, in the complex Zn-1, even if Zn2 loses a coordinated water molecule and the coordination number becomes 4, the structure can still remain intact. Although the complex structures of Zn-1 and Zn-2 are 1D chain structures, there are intermolecular forces such as hydrogen bonds between adjacent chains, which increases the stability of the complex structure. Thermogravimetric analysis shows that the weight loss is about 1.5% before 150°C, and this weight loss platform is the weight loss of the coordinated water molecule. After that, until 300°C, o C Zn-1 shows obvious weight loss, indicating structural collapse. Therefore, the structure of Zn-1 can remain stable below 300℃. Zn-2 has no obvious weight loss before 320℃, but its structure collapses and its weight loss is obvious after 320℃, which shows that Zn-2 can be stable to 320℃. Good thermal stability is conducive to the application and promotion of Zn-1 and Zn-2.
[0026] (2) When the excitation wavelength is 250 nm, within the scanning range of 270-600 nm, the solid-state fluorescence emission spectrum shows that the strongest emission peak of the ligand H2L is at 400 nm, phen has the strongest emission peak at 374 nm, Zn-1 has the strongest emission peak at 385 nm, and Zn-2 has the strongest emission peak at 381 nm. When Zn-1 and Zn-2 were added to 0.001 mmol / mL NaNO3, KNO3, AgNO3, Co(NO3)2, Ni(NO3)2, Cu(NO3)2, Zn(NO3)2, Cd(NO3)2, Pb(NO3)2, Fe(NO3)3, Al(NO3)3 and rare earth metal salts Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3 and Lu(NO3)3 solutions prepared with ethanol as solvent, the fluorescence intensity changed significantly compared with when no metal salt was added. For Zn-1, the addition of most metal ions enhanced the fluorescence of the strongest emission peak at 385 nm, but when Fe 3+ , Cu 2+ , Pr 3+ and Eu 3+ When the fluorescence intensity is reduced to different degrees. 2+ , Pr 3+ and Eu 3+ In comparison, Fe 3+ The effect of weakening the fluorescence intensity of Zn-1 is very obvious. Compared with the case without adding Fe(NO3)3, the fluorescence intensity of Zn-1 in 0.001 mmol / mL Fe(NO3)3 solution is reduced to 0.094% of the original value, which is a decrease of more than 99.9%. 3+ In the solution, Zn-1 undergoes fluorescence quenching. 3+ It has good recognition ability. For Zn-2, the addition of most metal ions can enhance the fluorescence of the strongest emission peak near 374 nm, such as rare earth metal ions. However, when Fe 3+ 、Al 3+ and Cu 2+ When the fluorescence intensity is reduced to different degrees, it indicates that Zn-2 3+ 、Al 3+ and Cu 2+ All have certain recognition functions. 3+ and Cu 2+ In comparison, Zn-2 has a significant effect on Fe 3+The fluorescence intensity of Zn-2 in 0.001 mmol / mL Fe(NO3)3 solution can be reduced to 4.39% of the original value. 3+ In the solution, both Zn-1 and Zn-2 can produce fluorescence quenching. 3+ Both have recognition ability, and Zn-1 has strong affinity for Fe 3+ The recognition effect is better. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of the coordination environment of Zn(II) in Zn-1 (symmetry code: ix, -1+y, z.).
[0028] Figure 2 The 1D double-chain structure in Zn-1 shows hydrogen bonding between the white chain formed by Zn1 and the black chain formed by Zn2. Light dashed line: O9—H9D···O2; dark dashed line: O9—H9C···O4.
[0029] Figure 3 Schematic diagram of the coordination environment of Zn(II) in Zn-2 (symmetry code: ix, y, 1+z.).
[0030] Figure 4 It is the 1D chain structure existing in Zn-2.
[0031] Figure 5 This is the thermogravimetric analysis diagram of Zn-1.
[0032] Figure 6 This is the thermogravimetric analysis diagram of Zn-2.
[0033] Figure 7 This is the XRD pattern of Zn-1.
[0034] Figure 8 This is the XRD pattern of Zn-2.
[0035] Fig. 9 This is the infrared spectrum of Zn-1.
[0036] Fig.10 This is the infrared spectrum of Zn-2.
[0037] Fig.11 The fluorescence emission spectra of Zn-1 and Zn-2 of the present invention and their ligands H2L and phen when the excitation wavelength is 250 nm.
[0038] Fig.12 The Zn-1 of the present invention is 10 -3Fluorescence emission spectra in mmol / mL NaNO3, KNO3, AgNO3, Co(NO3)2, Ni(NO3)2, Cu(NO3)2, Zn(NO3)2, Cd(NO3)2, Pb(NO3)2, Fe(NO3)3, and Al(NO3)3 solutions.
[0039] Fig.13 The Zn-1 of the present invention is 10 -3 Bar graph of emission peak intensity near 380nm in mmol / mL NaNO3, KNO3, AgNO3, Co(NO3)2, Ni(NO3)2, Cu(NO3)2, Zn(NO3)2, Cd(NO3)2, Pb(NO3)2, Fe(NO3)3, and Al(NO3)3 solutions.
[0040] Fig.14 The Zn-1 of the present invention is 10 -3 Fluorescence emission spectra in mmol / mL rare earth salts Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3, and Lu(NO3)3 solutions.
[0041] Fig.15 The Zn-1 of the present invention is 10 -3 Bar chart of emission peak intensity near 380nm in mmol / mL rare earth salt solutions of Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3, and Lu(NO3)3.
[0042] Fig.16 The Zn-2 of the present invention is 10 -3 Fluorescence emission spectra in mmol / mL NaNO3, KNO3, AgNO3, Co(NO3)2, Ni(NO3)2, Cu(NO3)2, Zn(NO3)2, Cd(NO3)2, Pb(NO3)2, Fe(NO3)3, and Al(NO3)3 solutions.
[0043] Fig.17 The Zn-2 of the present invention is 10 -3Bar graph of emission peak intensity near 365 nm in mmol / mL NaNO3, KNO3, AgNO3, Co(NO3)2, Ni(NO3)2, Cu(NO3)2, Zn(NO3)2, Cd(NO3)2, Pb(NO3)2, Fe(NO3)3, and Al(NO3)3 solutions.
[0044] Fig.18 The Zn-2 of the present invention is 10 -3 Fluorescence emission spectra (270nm-700nm) in mmol / mL rare earth salt solutions of Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3, and Lu(NO3)3.
[0045] Fig.19 The Zn-2 of the present invention is 10 -3 Fluorescence emission spectra (270nm-450nm) in mmol / mL rare earth salt solutions of Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3, and Lu(NO3)3.
[0046] Fig. 20 The Zn-2 of the present invention is 10 -3 Bar chart of emission peak intensity near 365 nm in mmol / mL rare earth salt solutions of Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3, and Lu(NO3)3. DETAILED DESCRIPTION
[0047] The present invention will be further described below in conjunction with examples, but the present invention is not limited to the following examples.
[0048] Example 1
[0049] ZnCl2·2H2O (13.6 mg), main ligand H2L (20.0 mg) and auxiliary ligand phen (10.0 mg) were placed in a 20.0 ml pressure-resistant thick glass sample bottle, and 10.0 ml of DMF / water (volume ratio 1: 1) solution was measured and placed in the above glass sample bottle. Finally, the sample bottle was sealed with a sample bottle cap, placed in a forced air drying oven, and heated at 90.0°C for 3 days to obtain colorless block crystals of Zn-1.
[0050] Example 2
[0051] ZnSO4·7H2O (28.7 mg), main ligand H2L (20.0 mg) and auxiliary ligand phen (10.0 mg) were placed in a 20.0 ml pressure-resistant thick glass sample bottle, and 10.0 ml of DMF / water (volume ratio 1: 1) solution was measured and placed in the above glass sample bottle. Finally, the sample bottle was sealed with a sample bottle cap, placed in a forced air drying oven, and heated at 90.0°C for 3 days to obtain colorless block crystals of Zn-2.
[0052] (1) Crystal structure determination:
[0053] The Zn-1 crystals obtained in Example 1 and the Zn-2 crystals obtained in Example 2 with better growth conditions and fewer cracks were selected and glued to the drawn glass wire. The diffraction data of Zn-1 obtained in Example 1 and Zn-2 obtained in Example 2 were collected under Mo-Kα radiation (λ = 0.71073 Å) using a Bruker APEX-II CCD single crystal diffractometer at room temperature. Zn-2 was refined using Shellxl-2018 in the OLEX2 program. The structure was solved using the XS structure solver, and the SHELXTL software package was used for least squares optimization. In the improvement process, the anisotropic displacement parameters of non-hydrogen atoms were given. The positions of hydrogen atoms on the ligands were determined by the theoretical hydrogenation method. The crystallographic data are shown in Table 1.
[0054] Table 1 Crystallographic data of Zn-1 and Zn-2 materials
[0055]
[0056] The structure of the complex Zn-1 is shown in Figure 1 and Figure 2 As shown, Figure 1The schematic diagram of the coordination environment of Zn(II), i.e., the asymmetric structural unit, shows that the asymmetric structural unit of Zn-1 contains two different Zn(II), Zn1 and Zn2, and the coordination numbers of Zn1 and Zn2 are both 5; Zn1 and Zn2 are coordinated with two N atoms and three O atoms, the N atoms come from the ligand phen, and the O atoms coordinated by Zn1 have two O atoms from the ligand L 2- , and another O atom comes from the coordinated water molecule; the three O atoms coordinated by Zn2 all come from the ligand L 2- .
[0057] In Zn-1, the ligand L 2- All adopt the trans conformation, similar to the Z-configuration; in Zn-1, the ligand L 2- There are two coordination modes. The first is that both carboxyl groups are monodentate coordinated, and the second is that one carboxyl group is monodentate coordinated and the other carboxyl group is chelate coordinated.
[0058] Figure 2 Indicated by L 2- The one-dimensional chain structure composed of Zn(II) and the H-bond interaction between the two chains shows that there is no direct connection between Zn1 and Zn2; Zn1 and Zn2 are both connected to two ligands L 2- , each L 2- Then connect two Zn(II); based on Zn1 and Zn2 respectively with ligand L 2- Two 1D chain structures are formed; in Zn-1, there is a strong intermolecular H-bonding effect between the two 1D chains formed based on Zn1 and Zn2, O9—H9D···O2 and O9—H9C···O4, so the two one-dimensional chain structures are very stable, and the 1D chains form a three-dimensional supramolecular structure through H bonding.
[0059] The structure of the complex Zn-2 is shown in Figure 3 and Figure 4 As shown, Figure 3 The coordination environment of Zn(II) is shown, showing that the asymmetric structural unit of Zn-2 contains two different Zn(II), Zn1 and Zn2, and the coordination numbers of Zn1 and Zn2 are both 5; Zn1 and Zn2 are coordinated with two N atoms and three O atoms, the N atoms come from the ligand phen, and the three O atoms come from the ligand L 2- ; In Zn-2, ligand L 2- There is only one coordination mode, one carboxyl group is monodentate coordinated and the other carboxyl group is chelate coordinated.
[0060] Figure 4 Indicated by L 2- The one-dimensional chain structure composed of Zn(II) and Zn1 shows that both Zn2 and Zn1 are connected to two ligands L at the same time.2- , each L 2- Then two Zn(II) are connected, and there is no ligand directly connected between Zn1 and Zn2. 2- Two 1D chain structures are formed, and the 1D chains form a three-dimensional supramolecular structure through H bonding.
[0061] In Zn-2, there are weak hydrogen bonds between molecules in the one-dimensional chain structure. A The distance between them is greater than 2.5 Å, and through weak H-bonding, a three-dimensional supramolecular structure is formed between the 1D chain structures.
[0062] Figure 5-6 The thermogravimetric analysis diagrams of Zn-1 and Zn-2 respectively show that Zn-1 and Zn-2 have good thermal stability and can maintain the stability of the framework structure below 300°C.
[0063] Figure 7-8 The X-ray powder diffraction spectra of Zn-1 and Zn-2 respectively show that the prepared Zn-1 and Zn-2 have good phase purity.
[0064] Figure 9-10 Fourier transform infrared spectra of Zn-1 and Zn-2, respectively, show that: Shimadzu FTIR-8400S spectrometer was used to analyze the −1 The FT-IR spectra of Zn-1 and Zn-2 were collected in the range of , and the corresponding characteristic absorption peaks were characterized. The results confirmed the coordination between the metal and the ligand.
[0065] Fig.11 It is the fluorescence emission spectrum of Zn-1, Zn-2 and its ligand of the present invention. The solid-state luminescence spectrum of Zn-1, Zn-2 and its ligand was studied at room temperature. As can be seen from the figure, when the excitation wavelength is 250 nm, the strongest emission peak of H2L ligand is at 405 nm, the strongest emission peak of phen ligand is at 375 nm, the strongest emission peak of Zn-1 is at 385 nm, and the strongest emission peak of Zn-2 is at 379 nm. The emission spectra of Zn-1 and Zn-2 are similar to the peak types of H2L ligand and phen ligand, and the position of the strongest emission peak is between the positions of the strongest emission peaks of the two ligands, so the luminescence of the complex Zn-1 and Zn-2 mainly comes from the ligand luminescence, which is mainly caused by the electronic transition between the ligand and the ligand.
[0066] Fig.12 The fluorescence emission spectra of Zn-1 in different non-rare earth metal ion solutions are shown in Figure 2. -3mmol / mL NaNO3, KNO3, AgNO3, Co(NO3)2, Ni(NO3)2, Cu(NO3)2, Zn(NO3)2, Cd(NO3)2, Pb(NO3)2, Fe(NO3)3, Al(NO3)3 solutions, the results showed that the emission spectra had similar shapes, with the strongest emission peak near 380nm, but different fluorescence intensities. 3+ In solution, it leads to fluorescence quenching, so Fe 3+ It has fluorescent recognition function.
[0067] Fig.13 The strongest emission peak intensity bar chart of Zn-1 in different non-rare earth metal ion solutions. -3 mmol / mL NaNO3, KNO3, AgNO3, Co(NO3)2, Ni(NO3)2, Cu(NO3)2, Zn(NO3)2, Cd(NO3)2, Pb(NO3)2, Fe(NO3)3, Al(NO3)3 solutions, the strongest emission peak fluorescence intensity is different. 2+ Highest medium strength, Fe 3+ Medium intensity is the lowest.
[0068] Fig.14 The fluorescence emission spectra of Zn-1 in different rare earth metal ion solutions are shown in Figure 2. -3 In mmol / mL rare earth salt solutions of Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3, and Lu(NO3)3, the fluorescence emission spectra have similar shapes, with the strongest emission peak near 380 nm, but the fluorescence intensities are different. Compared with the blank sample, Pr 3+ and Gd 3+ The intensity of the middle peak has weakened, while the middle peaks of other rare earth ions have increased.
[0069] Fig.15 The strongest emission peak intensity bar chart of Zn-1 in different rare earth metal ion solutions. -3The fluorescence intensity is different in mmol / mL rare earth salt solutions of Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3, and Lu(NO3)3. 3+ The highest medium strength, Pr 3+ Medium intensity is the lowest.
[0070] Fig.16 The fluorescence emission spectra of Zn-2 in different non-rare earth metal ion solutions are shown in Figure 2. -3 mmol / mL NaNO3, KNO3, AgNO3, Co(NO3)2, Ni(NO3)2, Cu(NO3)2, Zn(NO3)2, Cd(NO3)2, Pb(NO3)2, Fe(NO3)3, Al(NO3)3 solutions, the emission spectra are similar in shape, with the strongest emission peak near 365 nm, but the fluorescence intensities are different. 3+ In solution, it leads to fluorescence quenching, so Fe 3+ It has fluorescent recognition function.
[0071] Fig.17 The strongest peak emission intensity bar chart of Zn-2 in different non-rare earth metal ion solutions. -3 mmol / mL NaNO3, KNO3, AgNO3, Co(NO3)2, Ni(NO3)2, Cu(NO3)2, Zn(NO3)2, Cd(NO3)2, Pb(NO3)2, Fe(NO3)3, Al(NO3)3 solutions, the strongest emission peak fluorescence intensity is different. When Fe 3+ The fluorescence is quenched in solution, so the Fe 3+ It has fluorescent recognition function.
[0072] Fig.18 The fluorescence emission spectra of Zn-2 in different rare earth metal ion solutions within the test range of 270nm-700nm. -3In mmol / mL rare earth salt solutions of Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3, and Lu(NO3)3, the shapes of the fluorescence emission spectra are similar, but the fluorescence intensities are different. 3+ In addition to the emission peak near 365 nm, there are stronger emission peaks at 488 nm, 543 nm, 583 nm, and 620 nm. These peaks are Tb 3+ The characteristic peak of this complex is 3+ It has a certain identification function.
[0073] Fig.19 The fluorescence emission spectra of Zn-2 in different rare earth metal ion solutions in the range of 270 nm-450 nm are shown in Figure 2. -3 In mmol / mL rare earth salt solutions of Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3, and Lu(NO3)3, the shapes of the emission spectra are similar, but the fluorescence intensities are enhanced compared with those of the blank samples.
[0074] Fig. 20 The bar graph shows the emission peak intensity of Zn-2 at 365 nm in different rare earth metal ion solutions. -3 mmol / mL rare earth salt Y(NO3)3, La(NO3)3, Ce(NO3)3, Pr(NO3)3, Nd(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Er(NO3)3, Tm(NO3)3, Yb(NO3)3, Lu(NO3)3 solutions have different emission peak intensities, which are all enhanced compared with the blank sample. 3+ Medium intensity is the highest.
Claims
1. A zinc-based dual-ligand coordination polymer crystal material, characterized in that: The zinc-based dual-ligand coordination polymer crystal material is formed by Zn ions and two ligands through coordination bonds, one ligand is an organic ligand 2,2'-(1,2-phenylenebis(methylene))bis(thiodiyl) dinicotinic acid, H2L, and the chemical structure is as follows: ; Another ligand is 1,10-phenanthroline, phen, whose chemical structure is shown below: ; The zinc-based dual-ligand coordination polymer crystal material has a one-dimensional chain structure, and the one-dimensional chain structure forms a three-dimensional supramolecular structure through H-bonding; The molecular formula of the zinc-based dual-ligand coordination polymer crystal material is [Zn2(L)2(phen)2(H2O)] n , named Zn-1, the asymmetric structural unit of Zn-1 contains two different Zn (II), Zn1 and Zn2, the coordination numbers of Zn1 and Zn2 are both 5; Zn1 and Zn2 are coordinated with two N atoms and three O atoms, the N atoms come from the ligand phen, and the three O atoms coordinated by Zn1 are all from the ligand L 2- ; The O atoms coordinated by Zn2 have two ligands L 2- , another O atom comes from the coordinated water molecule; Or the molecular formula of the zinc-based dual-ligand coordination polymer crystal material is [ZnL(phen)] n , named Zn-2, the asymmetric structural unit of Zn-2 contains a Zn(II), Zn1; the coordination number is 5, coordinated with two N atoms and three O atoms, the N atom comes from the ligand phen, and the three O atoms all come from the two ligands L 2- .
2. The zinc-based dual-ligand coordination polymer crystal material according to claim 1, characterized in that: The Zn-1 belongs to the triclinic system P -1 space group, the unit cell parameters are: a = 11.2842(5) Å, b = 12.4733(5) Å, c = 20.9595(10)Å, α = 93.8570(10), β = 103.215(2), γ = 90.488(2).
3. The zinc-based dual-ligand coordination polymer crystal material according to claim 1, characterized in that: The Zn-2 belongs to the triclinic system P -1 space group, the unit cell parameters are: a =9.7389(4) Å, b =11.7190(4) Å, c =12.6870(4)Å, α = 80.1720(10), β = 89.3640(10), γ = 87.2590(10).
4. The zinc-based dual-ligand coordination polymer crystal material according to claim 2, characterized in that: In Zn-1, the ligand L 2- All adopt the trans conformation, similar to the Z-configuration; in Zn-1, the ligand L 2- There are two coordination modes. The first is that both carboxyl groups are monodentate coordinated, and the second is that one carboxyl group is monodentate coordinated and the other carboxyl group is chelate coordinated. There is no ligand directly connected between Zn1 and Zn2; Zn1 and Zn2 are both connected to two ligands L 2- , each L 2- Then connect two Zn(II); based on Zn1 and Zn2 respectively with ligand L 2- Two 1D chain structures are formed; in Zn-1, there is a strong intermolecular H-bonding effect between the two 1D chains formed based on Zn1 and Zn2, O9—H9D···O2 and O9—H9C···O4, so the two one-dimensional chain structures are very stable, and the 1D chains form a three-dimensional supramolecular structure through H bonding.
5. The zinc-based dual-ligand coordination polymer crystal material according to claim 3, characterized in that: In Zn-2, the ligand L 2- There is only one coordination mode, one carboxyl group is monodentate coordinated and the other carboxyl group is chelate coordinated; each Zn(II) is connected to two ligands L 2- , each L 2- Then two Zn(II) are connected to form a 1D chain structure; In Zn-2, there are weak hydrogen bonds between molecules in the one-dimensional chain structure. A The distance between them is greater than 2.5Å, and through weak H-bonding, adjacent 1D chain structures can form a three-dimensional supramolecular structure.
6. A method for preparing the zinc-based dual-ligand coordination polymer crystal material as claimed in claim 2 or 4, characterized in that: The steps include: Weigh ZnCl2·2H2O, main ligand H2L and auxiliary ligand phen into a 20.0 ml pressure-resistant thick glass sample bottle, and measure DMF / water 1:1 mixed solution and place it in the above glass sample bottle; finally, cover the bottle cap and seal the sample bottle, place it in a forced air drying oven, and heat it at 90.0℃ for 3 days; after the system slowly cools to room temperature, take out the sample bottle to obtain a colorless rod-shaped complex [Zn2(L)2(phen)2(H2O)] n , the complex is referred to as Zn-1.
7. The method for preparing the zinc-based dual-ligand coordination polymer crystal material according to claim 6, characterized in that: The mass ratio of the main ligand H2L to the auxiliary ligand phen is 2:1, the added amount of the DMF / water mixed liquid is limited to 1 mg of the auxiliary ligand phen corresponding to 1 ml of the mixed solution, and the mass ratio of the ZnCl2·2H2O to the main ligand H2L is 13.6:
20.
8. A method for preparing the zinc-based dual-ligand coordination polymer crystal material as claimed in claim 3 or 5, characterized in that: The steps include: Weigh ZnSO4·7H2O, main ligand H2L and auxiliary ligand phen into a 20.0 ml pressure-resistant thick glass sample bottle, and measure DMF / water 1:1 mixed solution and place it in the above glass sample bottle; finally, cover the bottle cap and seal the sample bottle, place it in a forced air drying oven, and heat it at 90.0℃ for 3 days; after the system slowly cools to room temperature, take out the sample bottle to obtain a colorless rod-shaped complex [ZnL(phen)] n , the complex is referred to as Zn-2.
9. The method for preparing the zinc-based dual-ligand coordination polymer crystal material according to claim 8, characterized in that: The mass ratio of the main ligand H2L to the auxiliary ligand phen is 2:1, the added amount of the DMF / water mixed liquid is limited to 1 mg of the auxiliary ligand phen corresponding to 1 ml of the mixed solution, and the mass ratio of the ZnCl2·2H2O to the main ligand H2L is 28.7:
20.
10. Use of the zinc-based biligand coordination polymer crystal material according to any one of claims 1 to 5 in metal ion recognition.