A method for preparing water-resistant polyurethane coating

Through the preparation method of two-component polyurethane coating, the cross-linking reaction and the hydrolysis of silane coupling agent are used to form a dense spatial network structure, which solves the problem of insufficient waterproof performance and hot water resistance of existing polyurethane coatings, and significantly improves the performance of existing polyurethane coatings. The coating is resistant to water and hot water and improves mechanical properties.

CN118516041BActive Publication Date: 2024-10-11FO-SHAN CITY SANSHUI LIANMEI CHEM LTD CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410984191.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-11
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Existing polyurethane waterproof coatings have insufficient waterproof performance and hot water resistance, especially in high-temperature scenarios. Commonly used asphalt can easily cause delamination, affecting the application scope and effect of the coating.

Method used

A two-component polyurethane coating preparation method is adopted, using hydroxy vinyl ether, complex alcohol, silane coupling agent, filler, hydroxyl-terminated polybutadiene, additives, and solvent to form component A, and isocyanate and catalyst to form component A. B. A dense spatial network structure is formed through cross-linking reaction, and the dispersion and hydrophobicity of the filler are improved through a silane coupling agent, thereby improving the water resistance and hot water resistance of the coating.

Benefits of technology

Significantly improves the density and water resistance of the paint coating, enhances the hot water resistance of the coating, reduces water absorption, and improves mechanical strength and anti-yellowing properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention belongs to the technical field of coatings, and discloses a method for preparing a water-resistant polyurethane coating. The preparation method comprises the following steps: (1) mixing hydroxy vinyl ether, complex alcohol, and silane coupling agent, and then adding filler, terminal hydroxyl polybutadiene, auxiliary agent, and solvent to obtain component A; (2) mixing isocyanate and catalyst to obtain component B; (3) component A and component B constitute a polyurethane coating; the complex alcohol comprises glycerol, and at least two of xylitol, sorbitol, and pentaerythritol. The hydroxyl groups in hydroxy vinyl ether, complex alcohol, and terminal hydroxyl polybutadiene are cross-linked and cured with a curing agent to form a three-dimensional spatial network structure, and the gaps in the three-dimensional spatial network structure are filled with fillers, which significantly improves the compactness of the coating, and the hot water resistance of the coating is also improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and particularly relates to a method for preparing a water-resistant polyurethane coating. Background Art

[0002] Common waterproof coatings include polymer cement waterproof coatings and polyurethane waterproof coatings. Although polymer cement waterproof coatings are relatively low in cost, their waterproof performance is relatively average. Existing polyurethane waterproof coatings often require the use of asphalt, which is prone to stratification, resulting in the need to improve the waterproof performance of polyurethane waterproof coatings.

[0003] Moreover, as the application scope of waterproof coatings expands, some waterproofing scenes have a certain degree of high temperature (such as pools storing hot wastewater or bathroom pools), which requires waterproof coatings to have hot water resistance.

[0004] Therefore, there is an urgent need to provide a new polyurethane waterproof coating that has good water resistance, especially hot water resistance, so as to help expand the application of the polyurethane waterproof coating. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for preparing a water-resistant polyurethane coating. The polyurethane coating prepared by the preparation method of the present invention has good water resistance, especially hot water resistance.

[0006] The polyurethane coating of the present invention is a two-component coating, which uses hydroxy vinyl ether, complex alcohol, silane coupling agent, filler, hydroxyl-terminated polybutadiene, auxiliary agent and solvent to form component A, and when used, it is mixed and cured with component B to form a polyurethane coating coating. The hydroxyl groups in hydroxy vinyl ether, complex alcohol (the complex alcohol includes glycerol, which not only provides hydroxyl groups but also helps to be compatible with other alcohols, and the complex alcohol also includes tetrahydroxyl, pentahydroxyl or hexahydroxyl specific alcohols, such as xylitol, sorbitol, pentaerythritol, and these polyols containing more than 3 hydroxyl groups help to form a dense spatial network structure after curing and crosslinking reaction with isocyanate), and the hydroxyl groups in the hydroxyl-terminated polybutadiene are crosslinked and cured with the curing agent to form a three-dimensional spatial network structure, and the gaps in the three-dimensional spatial network structure are filled with fillers, which significantly improves the compactness of the coating, and the silane coupling agent KH570 can not only improve the dispersion uniformity of the filler after hydrolysis, but also provide siloxane groups for improving the hydrophobicity of the coating, thereby improving the water resistance of the coating, and the hot water resistance of the coating is also improved.

[0007] The invention provides a method for preparing a water-resistant polyurethane coating.

[0008] Specifically, a method for preparing a water-resistant polyurethane coating comprises the following steps:

[0009] (1) Mixing hydroxy vinyl ether, complex alcohol and silane coupling agent, and then adding filler, terminal hydroxyl polybutadiene, auxiliary agent and solvent to obtain component A;

[0010] (2) mixing isocyanate and catalyst to obtain component B;

[0011] (3) The component A and the component B constitute the polyurethane coating;

[0012] The complex alcohol includes glycerol and at least two of xylitol, sorbitol and pentaerythritol.

[0013] Preferably, the hydroxy vinyl ether includes 4-hydroxybutyl vinyl ether and / or triethylene glycol divinyl ether.

[0014] Preferably, the filler includes nano silicon dioxide and nano calcium silicate.

[0015] Preferably, the silane coupling agent includes silane coupling agent KH570.

[0016] Preferably, the isocyanate includes at least one of hydrogenated phenylmethane diisocyanate (hydrogenated MDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), and hexamethylene diisocyanate (HDI); hydrogenated phenylmethane diisocyanate, toluene diisocyanate (TDI), and diphenylmethane diisocyanate (MDI) are further preferred. The use of isocyanates containing benzene rings for cross-linking and curing helps to improve the compactness of the coating. Hydrogenated phenylmethane diisocyanate also makes the coating have better yellowing resistance.

[0017] Preferably, the catalyst comprises an organic tin, such as dibutyltin dilaurate, dibutyltin didodecylsulfide.

[0018] Preferably, the auxiliary agent includes at least one of a defoaming agent, sodium lauryl sulfate, and nonylphenol polyethylene glycol.

[0019] Preferably, the defoaming agent is polydimethylsiloxane.

[0020] Preferably, the solvent includes ethanol and water. For example, the solvent is composed of ethanol and water in a mass ratio of 1:(0.5-3).

[0021] Preferably, the mass ratio of the hydroxy vinyl ether, the complex alcohol, the silane coupling agent, the filler and the terminal hydroxyl polybutadiene is 1: (0.5-1.5): (1-5): (0.5-3): (0.5-1.5), and more preferably 1: (0.6-1.2): (1.5-4): (0.8-2.5): (0.7-1.2).

[0022] Preferably, the complex alcohol, calculated by mass, includes 1 part of glycerol, and at least two of 2-5 parts of xylitol, 1-5 parts of sorbitol, and 3-10 parts of pentaerythritol. Further preferably, the complex alcohol, calculated by mass, includes 1 part of glycerol, and at least two of 2.5-3.5 parts of xylitol, 1.5-4.55 parts of sorbitol, and 3.5-8 parts of pentaerythritol.

[0023] Preferably, the mass ratio of the hydroxy vinyl ether to the auxiliary agent and the solvent is 1:(1-5):(8-50), and more preferably 1:(2-5):(10-40).

[0024] Preferably, in the component B, the mass ratio of isocyanate to catalyst is 1:(0.1-0.5), more preferably 1:(0.1-0.3).

[0025] Preferably, the mass ratio of component A to component B is 10:(0.1-2), and more preferably 10:(0.5-1.8).

[0026] Preferably, a method for preparing a water-resistant polyurethane coating comprises the following steps:

[0027] (1) Mixing hydroxy vinyl ether, complex alcohol and silane coupling agent, and then adding filler, terminal hydroxyl polybutadiene, auxiliary agent and solvent to mix to obtain component A, wherein the mass ratio of the hydroxy vinyl ether, complex alcohol, silane coupling agent, filler and terminal hydroxyl polybutadiene is 1: (0.5-1.5): (1-5): (0.5-3): (0.5-1.5);

[0028] (2) mixing isocyanate and catalyst to obtain component B, wherein the mass ratio of isocyanate to catalyst is 1:(0.1-0.5);

[0029] (3) The component A and the component B constitute the polyurethane coating, and the mass ratio of the component A to the component B is 10:(0.1-2);

[0030] The complex alcohol comprises, by weight, 1 part of glycerol, and at least two of 2-5 parts of xylitol, 1-5 parts of sorbitol, and 3-10 parts of pentaerythritol.

[0031] The appropriate dosage relationship of each raw material helps to obtain a polyurethane coating with better water resistance.

[0032] Preferably, polyether triol and hydroxymethyl cellulose are added during the preparation of component A, which helps to further improve the density of the polyurethane coating, thereby improving the water resistance and mechanical strength of the coating.

[0033] Preferably, the mass ratio of the hydroxy vinyl ether to the polyether triol and the hydroxymethyl cellulose is 1:(0.1-2):(0.1-1), and more preferably 1:(0.2-0.6):(0.2-0.4).

[0034] When the water-resistant polyurethane coating prepared by the above preparation method is used, component A and component B are mixed and then cured to obtain a polyurethane coating.

[0035] Preferably, the curing temperature is 40-100° C., and the curing time is 60-150 minutes. More preferably, the curing temperature is 50-90° C., and the curing time is 70-120 minutes.

[0036] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0037] The polyurethane coating of the present invention is a two-component coating, which uses hydroxy vinyl ether, complex alcohol, silane coupling agent, filler, hydroxyl-terminated polybutadiene, auxiliary agent and solvent to form component A, and when used, it is mixed and cured with component B to form a polyurethane coating coating. The hydroxyl groups in hydroxy vinyl ether, complex alcohol (the complex alcohol includes glycerol, which not only provides hydroxyl groups but also helps to be compatible with other alcohols, and the complex alcohol also includes tetrahydroxyl, pentahydroxyl or hexahydroxyl specific alcohols, such as xylitol, sorbitol, pentaerythritol, and these polyols containing more than 3 hydroxyl groups help to form a dense spatial network structure after curing and crosslinking reaction with isocyanate), and the hydroxyl groups in the hydroxyl-terminated polybutadiene are crosslinked and cured with the curing agent to form a three-dimensional spatial network structure, and the gaps in the three-dimensional spatial network structure are filled with fillers, which significantly improves the compactness of the coating, and the silane coupling agent KH570 can not only improve the dispersion uniformity of the filler after hydrolysis, but also provide siloxane groups for improving the hydrophobicity of the coating, thereby improving the water resistance of the coating, and the hot water resistance of the coating is also improved. DETAILED DESCRIPTION

[0038] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0039] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0040] Example 1

[0041] A method for preparing a water-resistant polyurethane coating comprises the following steps:

[0042] (1) 4-hydroxybutyl vinyl ether, complex alcohol, and silane coupling agent KH570 are mixed at a stirring speed of 800 rpm for 30 minutes, and then filler (the filler is composed of nano silicon dioxide and nano calcium silicate in a mass ratio of 1:2), terminal hydroxyl polybutadiene, auxiliary agent (the auxiliary agent is composed of polydimethylsiloxane and sodium lauryl sulfate in a mass ratio of 1:1), and solvent (ethanol and water in a mass ratio of 1:0.8) are added and mixed at a stirring speed of 1000 rpm for 20 minutes to obtain component A, wherein the mass ratio of 4-hydroxybutyl vinyl ether, complex alcohol, silane coupling agent KH570, filler, and terminal hydroxyl polybutadiene is 1:0.8:2:1.5:1;

[0043] The mass ratio of 4-hydroxybutyl vinyl ether to the additive and solvent is 1:2:20;

[0044] The complex alcohol is composed of the following components by weight: 1 part of glycerol, 3 parts of xylitol, 2 parts of sorbitol, and 3 parts of pentaerythritol;

[0045] (2) mixing isocyanate (toluene diisocyanate (TDI)) and catalyst (dibutyltin dilaurate) at a stirring speed of 200 rpm for 10 minutes to obtain component B, wherein the mass ratio of isocyanate to catalyst is 1:0.1;

[0046] (3) Component A and component B constitute a polyurethane coating, and the mass ratio of component A to component B is 10:0.8.

[0047] Example 2

[0048] A method for preparing a water-resistant polyurethane coating comprises the following steps:

[0049] (1) Triethylene glycol divinyl ether, complex alcohol, and silane coupling agent KH570 are mixed at a stirring speed of 700 rpm for 30 minutes, and then filler (the filler is composed of nano silicon dioxide and nano calcium silicate in a mass ratio of 1:1), terminal hydroxyl polybutadiene, auxiliary agent (the auxiliary agent is composed of polydimethylsiloxane and sodium lauryl sulfate in a mass ratio of 1:0.8), and solvent (ethanol and water in a mass ratio of 1:1) are added and mixed at a stirring speed of 800 rpm for 30 minutes to obtain component A, wherein the mass ratio of triethylene glycol divinyl ether, complex alcohol, silane coupling agent KH570, filler, and terminal hydroxyl polybutadiene is 1:1.0:2.2:1.8:1.2; the mass ratio of triethylene glycol divinyl ether to auxiliary agent and solvent is 1:1.8:22;

[0050] The complex alcohol is composed of the following components by weight: 1 part of glycerol, 4 parts of xylitol and 3 parts of sorbitol;

[0051] (2) mixing isocyanate (methylene diphenyl diisocyanate (MDI)) and catalyst (dibutyltin dilaurate) at a stirring speed of 200 rpm for 10 minutes to obtain component B, wherein the mass ratio of isocyanate to catalyst is 1:0.2;

[0052] (3) Component A and component B constitute a polyurethane coating, and the mass ratio of component A to component B is 10:0.9.

[0053] Example 3

[0054] A method for preparing a water-resistant polyurethane coating comprises the following steps:

[0055] (1) 4-hydroxybutyl vinyl ether, complex alcohol, silane coupling agent KH570, polyether triol and hydroxymethyl cellulose are mixed at a stirring speed of 800 rpm for 30 minutes, and then filler (the filler is composed of nano silicon dioxide and nano calcium silicate in a mass ratio of 1:2), terminal hydroxyl polybutadiene, auxiliary agent (the auxiliary agent is composed of polydimethylsiloxane and sodium lauryl sulfate in a mass ratio of 1:1), and solvent (ethanol and water in a mass ratio of 1:0.8) are added and mixed at a stirring speed of 1000 rpm for 20 minutes to obtain component A, wherein the mass ratio of 4-hydroxybutyl vinyl ether, complex alcohol, silane coupling agent, filler and terminal hydroxyl polybutadiene is 1:0.8:2:1.5:1; the mass ratio of 4-hydroxybutyl vinyl ether to auxiliary agent and solvent is 1:2:20;

[0056] The complex alcohol is composed of the following components by weight: 1 part of glycerol, 3 parts of xylitol, 2 parts of sorbitol, and 3 parts of pentaerythritol;

[0057] The mass ratio of 4-hydroxybutyl vinyl ether to polyether triol and hydroxymethyl cellulose is 1:0.3:0.4;

[0058] (2) mixing isocyanate (toluene diisocyanate (TDI)) and catalyst (dibutyltin dilaurate) at a stirring speed of 200 rpm for 10 minutes to obtain component B, wherein the mass ratio of isocyanate to catalyst is 1:0.1;

[0059] (3) Component A and component B constitute a polyurethane coating, and the mass ratio of component A to component B is 10:0.8.

[0060] Example 4

[0061] A method for preparing a water-resistant polyurethane coating comprises the following steps:

[0062] (1) Mix hydroxy vinyl ether (hydroxy vinyl ether is composed of 4-hydroxybutyl vinyl ether and triethylene glycol divinyl ether in a mass ratio of 1:1), complex alcohol, and silane coupling agent KH570, stirring at a speed of 700 rpm for 30 minutes, then add filler (filler is composed of nano silicon dioxide and nano calcium silicate in a mass ratio of 1:1.5), terminal hydroxyl polybutadiene, auxiliary agent (auxiliary agent is composed of polydimethylsiloxane and sodium lauryl sulfate in a mass ratio of 1:0.8), and solvent (ethanol and water in a mass ratio of 1:1.2) and mix at a speed of 700 rpm for 30 minutes to obtain component A, wherein the mass ratio of hydroxy vinyl ether, complex alcohol, silane coupling agent KH570, filler, and terminal hydroxyl polybutadiene is 1:1.0:2.5:1.9:1.5; the mass ratio of hydroxy vinyl ether to auxiliary agent and solvent is 1:1.8:22;

[0063] The complex alcohol is composed of the following components by weight: 1 part of glycerol, 1 part of xylitol and 1 part of pentaerythritol;

[0064] (2) Mixing isocyanate (hydrogenated phenylmethane diisocyanate) and catalyst (dibutyltin dilaurate) at a stirring speed of 200 rpm for 10 minutes to obtain component B, wherein the mass ratio of isocyanate to catalyst is 1:0.15;

[0065] (3) Component A and component B constitute a polyurethane coating, and the mass ratio of component A to component B is 10:1.1.

[0066] Comparative Example 1

[0067] Compared with Example 1, the difference of Comparative Example 1 is that the xylitol and sorbitol in Example 1 are replaced by an equal amount of pentaerythritol, and the rest of the process is the same as that of Example 1.

[0068] Specifically, the content of Comparative Example 1 is as follows:

[0069] A method for preparing a water-resistant polyurethane coating comprises the following steps:

[0070] (1) 4-hydroxybutyl vinyl ether, complex alcohol, and silane coupling agent KH570 are mixed at a stirring speed of 800 rpm for 30 minutes, and then filler (the filler is composed of nano silicon dioxide and nano calcium silicate in a mass ratio of 1:2), terminal hydroxyl polybutadiene, auxiliary agent (the auxiliary agent is composed of polydimethylsiloxane and sodium lauryl sulfate in a mass ratio of 1:1), and solvent (ethanol and water in a mass ratio of 1:0.8) are added and mixed at a stirring speed of 1000 rpm for 20 minutes to obtain component A, wherein the mass ratio of 4-hydroxybutyl vinyl ether, complex alcohol, silane coupling agent KH570, filler, and terminal hydroxyl polybutadiene is 1:0.8:2:1.5:1;

[0071] The mass ratio of 4-hydroxybutyl vinyl ether to the additive and solvent is 1:2:20;

[0072] The complex alcohol is composed of the following components by weight: 1 part of glycerol and 8 parts of pentaerythritol;

[0073] (2) mixing isocyanate (toluene diisocyanate (TDI)) and catalyst (dibutyltin dilaurate) at a stirring speed of 200 rpm for 10 minutes to obtain component B, wherein the mass ratio of isocyanate to catalyst is 1:0.1;

[0074] (3) Component A and component B constitute a polyurethane coating, and the mass ratio of component A to component B is 10:0.8.

[0075] Comparative Example 2

[0076] Compared with Example 1, the difference of Comparative Example 2 is that an equal amount of poly(1,4-butylene adipate diol) is used to replace the complex alcohol in Example 1, and the rest of the process is the same as that of Example 1.

[0077] Specifically, the content of Comparative Example 2 is as follows:

[0078] A method for preparing a water-resistant polyurethane coating comprises the following steps:

[0079] (1) 4-hydroxybutyl vinyl ether, poly(1,4-butylene adipate) diol, and silane coupling agent KH570 were mixed at a stirring speed of 800 rpm for 30 minutes, and then fillers (the fillers were composed of nano-silicon dioxide and nano-calcium silicate in a mass ratio of 1:2), terminal hydroxyl polybutadiene, auxiliary agents (the auxiliary agents were composed of polydimethylsiloxane and sodium lauryl sulfate in a mass ratio of 1:1), and solvents (ethanol and water in a mass ratio of 1:0.8) were added and mixed at a stirring speed of 1000 rpm for 20 minutes to obtain component A, wherein the mass ratio of 4-hydroxybutyl vinyl ether, poly(1,4-butylene adipate) diol, silane coupling agent KH570, fillers, and terminal hydroxyl polybutadiene was 1:0.8:2:1.5:1;

[0080] The mass ratio of 4-hydroxybutyl vinyl ether to the additive and solvent is 1:2:20;

[0081] (2) mixing isocyanate (toluene diisocyanate (TDI)) and catalyst (dibutyltin dilaurate) at a stirring speed of 200 rpm for 10 minutes to obtain component B, wherein the mass ratio of isocyanate to catalyst is 1:0.1;

[0082] (3) Component A and component B constitute a polyurethane coating, and the mass ratio of component A to component B is 10:0.8.

[0083] Comparative Example 3

[0084] Compared with Example 1, the difference of Comparative Example 3 is that the hydroxy-terminated polybutadiene in Example 1 is omitted, and the rest of the process is the same as that of Example 1.

[0085] Specifically, the content of Comparative Example 3 is as follows:

[0086] A method for preparing a water-resistant polyurethane coating comprises the following steps:

[0087] (1) 4-hydroxybutyl vinyl ether, complex alcohol, and silane coupling agent KH570 were mixed at a stirring speed of 800 rpm for 30 minutes, and then fillers (the fillers were composed of nano silicon dioxide and nano calcium silicate in a mass ratio of 1:2), auxiliary agents (the auxiliary agents were composed of polydimethylsiloxane and sodium lauryl sulfate in a mass ratio of 1:1), and solvents (ethanol and water in a mass ratio of 1:0.8) were added and mixed at a stirring speed of 1000 rpm for 20 minutes to obtain component A, wherein the ratio of 4-hydroxybutyl vinyl ether, complex alcohol, silane coupling agent KH570, and filler was 1:0.8:2:1.5;

[0088] The mass ratio of 4-hydroxybutyl vinyl ether to the additive and solvent is 1:2:20;

[0089] The complex alcohol is composed of the following components by weight: 1 part of glycerol, 3 parts of xylitol, 2 parts of sorbitol, and 3 parts of pentaerythritol;

[0090] (2) mixing isocyanate (toluene diisocyanate (TDI)) and catalyst (dibutyltin dilaurate) at a stirring speed of 200 rpm for 10 minutes to obtain component B, wherein the mass ratio of isocyanate to catalyst is 1:0.1;

[0091] (3) Component A and component B constitute a polyurethane coating, and the mass ratio of component A to component B is 10:0.8.

[0092] Product effect testing

[0093] Take the polyurethane resin coating prepared in the above examples 1-4 and comparative examples 1-3, apply (the coating amount is 0.5 mg / cm 2 ) was solidified on a glass substrate to obtain a sample. The sample was then immersed in 60°C distilled water for 48 hours, and the water absorption of the sample was finally tested. Water absorption (%) = (sample mass after immersion for 48 hours - sample initial mass) / sample initial mass * 100%. The lower the water absorption, the better the water resistance. The results are shown in Table 1.

[0094] Table 1

[0095]

[0096] It can be seen from Table 1 that the water absorption rate of the coating corresponding to the embodiment is significantly lower than that of the comparative example. When the type of complex alcohol is changed or the terminal hydroxyl polybutadiene is not used, the high temperature water resistance of the coating formed by the polyurethane resin coating is significantly reduced. The reason may be that when the type of complex alcohol is changed or the terminal hydroxyl polybutadiene is not used, the compactness of the prepared coating will be deteriorated, thereby increasing the water absorption rate of the coating.

[0097] The polyurethane coatings prepared in Example 1, Example 3 and Comparative Example 1 were tested for tensile strength of the coatings formed by the polyurethane coatings according to the standard GB / T19250-2013. The results are shown in Table 2.

[0098] Table 2

[0099]

[0100] It can be seen from Table 2 that the tensile strength of the coating corresponding to the embodiment is greater than that of the comparative example. And it can be seen from the results of Example 1 and Example 3 that when polyether triol and hydroxymethyl cellulose are used, the mechanical properties of the coating can be further improved.

Claims

1. A method for preparing a water-resistant polyurethane coating, characterized in that: The following steps are involved: (1) Mixing hydroxy vinyl ether, complex alcohol and silane coupling agent, and then adding filler, terminal hydroxyl polybutadiene, auxiliary agent and solvent to obtain component A; (2) mixing isocyanate and catalyst to obtain component B; (3) The component A and the component B constitute the polyurethane coating; The complex alcohol includes glycerol and at least two of xylitol, sorbitol and pentaerythritol.

2. The preparation method according to claim 1, characterized in that: The hydroxy vinyl ether includes 4-hydroxybutyl vinyl ether and / or triethylene glycol divinyl ether.

3. The preparation method according to claim 1, characterized in that: The filler includes nano silicon dioxide and nano calcium silicate; and / or the silane coupling agent includes silane coupling agent KH570.

4. The preparation method according to claim 1, characterized in that: The isocyanate includes at least one of hydrogenated phenylmethane diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, and hexamethylene diisocyanate; and / or the catalyst includes organic tin.

5. The preparation method according to claim 1, characterized in that: The auxiliary agent includes at least one of a defoaming agent, sodium lauryl sulfate and nonylphenol polyethylene glycol.

6. The preparation method according to claim 1, characterized in that: The mass ratio of the hydroxy vinyl ether, the complex alcohol, the silane coupling agent, the filler and the terminal hydroxyl polybutadiene is 1: (0.5-1.5): (1-5): (0.5-3): (0.5-1.5).

7. The preparation method according to claim 1, characterized in that: The complex alcohol comprises, by weight, 1 part of glycerol, and at least two of 2-5 parts of xylitol, 1-5 parts of sorbitol, and 3-10 parts of pentaerythritol.

8. The preparation method according to claim 1, characterized in that: The mass ratio of the hydroxy vinyl ether to the auxiliary agent and the solvent is 1:(1-5):(8-50).

9. The preparation method according to claim 1, characterized in that: In the component B, the mass ratio of isocyanate to catalyst is 1:(0.1-0.5); and / or, the mass ratio of component A to component B is 10:(0.1-2).

10. The preparation method according to claim 1, characterized in that: The following steps are involved: (1) Mixing hydroxy vinyl ether, complex alcohol and silane coupling agent, and then adding filler, terminal hydroxyl polybutadiene, auxiliary agent and solvent to mix to obtain component A, wherein the mass ratio of the hydroxy vinyl ether, complex alcohol, silane coupling agent, filler and terminal hydroxyl polybutadiene is 1: (0.5-1.5): (1-5): (0.5-3): (0.5-1.5); (2) mixing isocyanate and catalyst to obtain component B, wherein the mass ratio of isocyanate to catalyst is 1:(0.1-0.5); (3) The component A and the component B constitute the polyurethane coating, and the mass ratio of the component A to the component B is 10:(0.1-2); The complex alcohol comprises, by weight, 1 part of glycerol, and at least two of 2-5 parts of xylitol, 1-5 parts of sorbitol, and 3-10 parts of pentaerythritol.